Three-dimensional chip stacking preparation method and three-dimensional chip stacking structure

By preparing metal bump conductive structures with protrusions and semi-cured organic films on the chip surface, the vacuum reflow process is used to solve the problem of solder diffusion and filling difficulties in three-dimensional chip stack packaging, improving packaging efficiency and reliability.

CN117393446BActive Publication Date: 2024-10-29GUANGDONG INST OF SEMICON IND TECH
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202311517268.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-11-14
Publication Date
2024-10-29
Estimated Expiration
2043-11-14

AI Technical Summary

Technical Problem

In the existing three-dimensional chip stack packaging technology, the reflow soldering bonding method has problems such as short circuit caused by solder diffusion, difficulty in underfilling, warping and deformation, etc., resulting in low packaging efficiency and poor reliability.

Method used

A metal bump conductive structure with spikes and a semi-cured organic film are prepared on the surface of the chip. Chip stacking and bonding are achieved at a lower temperature through a vacuum reflow process. The organic film is used for insulation and bonding to reduce the height of the conductive structure. Consistency requirements.

Benefits of technology

It achieves fast and accurate multi-layer chip stacking, simplifies the filling of insulating structures, improves the reliability of inter-chip interconnections and the stability of packaging structures, and reduces process difficulty and cost.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117393446B_ABST
    Figure CN117393446B_ABST
Patent Text Reader

Abstract

The present invention discloses a three-dimensional chip stacking structure and a preparation method, the method comprising forming a conductive structure; preparing an organic film in a semi-cured state on the first surface and / or the second surface of the chip, and opening a window on the organic film to expose the first conductive structure and / or the second conductive structure; at a relatively low temperature, sequentially fixing the first conductive structure of the upper chip on the second conductive structure of the lower chip to complete the stacking of multi-layer chips; applying pressure on the top of the stacked multi-layer chips, and infiltrating the sidewalls of the spurs and metal bumps of the first conductive structure and the second conductive structure of the stacked multi-layer chips through a vacuum reflow process to achieve complete bonding of the first conductive structure and the second conductive structure, and bonding the upper and lower chips through the organic film; and heating the organic film to completely cure. The scheme of the present invention can effectively reduce the process difficulty when the upper and lower chips are interconnected and the cost of the three-dimensional stacking package, and the yield and reliability of the obtained three-dimensional chip stacking structure are better.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of integrated circuit packaging, and in particular to a three-dimensional chip stacking preparation method and a three-dimensional chip stacking structure. Background Art

[0002] The development of technologies such as artificial intelligence, intelligent driving, and high-performance computing has put forward higher requirements for storage technology, and it is necessary to develop storage technology with higher bandwidth and larger capacity. In order to meet the demand for storage technology with higher bandwidth and larger capacity, advanced packaging technology has received more and more widespread attention. At present, the more mainstream advanced packaging mainly includes fan-out wafer-level packaging (FO), wafer-level chip scale packaging (WLCSP), 2.5D / 3D packaging, and system-level packaging (SiP), etc. Among them, three-dimensional chip stacking packaging is an IC packaging method in which a complete computer chip (such as dynamic random access memory) is placed on top of another chip (such as a central processing unit), which relies on the metallized interconnection structure between the silicon layers to achieve electrical connectivity between the corresponding chips. Since multiple bare chips or substrates can be directly stacked by bonding to achieve a metal interconnection structure in a three-dimensional direction, the three-dimensional chip stacking packaging can greatly reduce the interconnection distance between chips, thereby increasing the speed and bandwidth of data transmission, reducing latency and power consumption, and increasing storage capacity. Therefore, the three-dimensional chip stacking packaging has become an effective solution for the development of high-performance memory.

[0003] For three-dimensional chip stacking packaging technology, interlayer bonding is one of the core technologies of three-dimensional stacking technology. At present, the industry usually adopts methods such as thermal compression bonding and reflow soldering chip bonding to achieve interlayer bonding of three-dimensional stacking. Among them, thermal compression bonding requires higher pressure and higher temperature, and is usually in the form of die to wafer (also known as chip-level stacking), so the process is difficult, and thermal compression bonding requires interlayer bonding layer by layer, so the packaging efficiency is low. In addition, this technology uses NCF or NCP, but NCF and NCP are easy to remain between the upper and lower layers of solder after use, which is easy to cause short circuits and seriously affect the reliability of solder interconnection between chips. Three-dimensional chip stacking using reflow soldering is usually in the form of wafer to wafer (also known as wafer-level stacking). This technology first stacks a large number of chips through solder, then heats the solder to reflow to achieve effective bonding of the upper and lower layers, and finally uses bottom filling and plastic sealing processes to achieve filling of solder gaps and plastic sealing protection of the chip surrounding area. Due to the wafer-level stacking and massive reflow bonding of chips, this technology has high packaging efficiency, but it has at least the following key defects that need to be solved:

[0004] 1) This technology first bonds the solder and then fills the gaps between the solder with insulating materials. This causes the solder to diffuse and connect to each other during the heat reflow process, causing a short circuit, which will have an adverse effect on the pin size and spacing;

[0005] 2) This technology performs bottom filling of the solder gap at the end of the packaging process. The multi-layer stacking structure and the very limited space between layers make bottom filling very difficult;

[0006] 3) During the reflow process, the chip and substrate will warp and deform, and the chip bonding yield will decrease. Summary of the invention

[0007] An embodiment of the present invention provides a three-dimensional chip stacking preparation method to solve at least one technical problem existing in the current three-dimensional chip stacking packaging technology when using a reflow bonding method to perform interlayer bonding.

[0008] In a first aspect, an embodiment of the present invention provides a method for preparing a three-dimensional chip stack, comprising:

[0009] Forming a conductive structure on the first surface and the second surface of the chip on which the metallized filled TSV and the rewiring layer are prepared, wherein the conductive structure includes a first conductive structure located on the first surface of the chip and a second conductive structure located on the second surface of the chip, and the second conductive structure is a metal bump with a spur;

[0010] Preparing a semi-cured organic film on the first surface and / or the second surface of the chip, and opening a window on the semi-cured organic film to expose the first conductive structure and / or the second conductive structure;

[0011] At a relatively low temperature, the stacking of multiple layers of chips is completed by sequentially fixing the first conductive structure of the upper layer chip on the protrusions of the second conductive structure of the lower layer chip;

[0012] Applying pressure on the top of the stacked multi-layer chips, through a vacuum reflow process, wet the protrusions and sidewalls of the metal bumps of the first conductive structure of the upper chip and the second conductive structure of the lower chip of the stacked multi-layer chips, so as to achieve complete bonding of the first conductive structure and the second conductive structure, and bond the upper and lower chips through the semi-cured organic film;

[0013] The organic film is heated and completely cured to form a three-dimensional chip stacking structure.

[0014] In a second aspect, the three-dimensional chip stacking preparation method described in the first aspect of the present invention is applied to chip-level stacking or wafer-level stacking.

[0015] In a third aspect, an embodiment of the present invention provides a three-dimensional chip stacking structure, comprising:

[0016] substrate;

[0017] At least two chip layers are located on the substrate, each chip layer includes at least one chip;

[0018] At least two bonding structures located between adjacent chip layers, wherein the bonding structure is formed by bonding a first conductive structure on a first surface of a chip located in an upper chip layer and a second conductive structure on a second surface of a chip located in a lower chip layer, and the second conductive structure is a metal bump with a spur;

[0019] An organic film located between adjacent chip layers and used to bond the adjacent chip layers, the organic film isolating adjacent bonding structures from each other, wherein the organic film is formed by heating the semi-cured organic film to fully cure it;

[0020] The TSVs penetrate the chips in the chip layer, and the first surface and the second surface of each chip are connected through the TSVs penetrating the chip.

[0021] In a fourth aspect, an embodiment of the present invention provides a three-dimensional chip stacking structure manufactured by the method described in the first aspect of the embodiment of the present invention.

[0022] The beneficial effect of the embodiment of the present invention is that: the solution provided by the embodiment of the present invention has conductive structures prepared on both the first surface and the second surface of the chip, and the second conductive structure on the second surface is a metal bump with spurs. The first conductive structure can be fixed on the metal bump only by a pick-and-place process, so that a large number of upper chips and lower chips can be accurately and quickly batch-temporarily bonded at a relatively low temperature, thereby enabling a large number of stacked multi-layer chips temporarily bonded in batches to be subjected to a massive reflow process to achieve rapid stacking and packaging of chips, thereby greatly reducing packaging costs. In addition, the solution of the embodiment of the present invention completes the stacking of the insulating structure while the chips are stacked, which makes it extremely simple to fill the gap between the upper and lower chips. At the same time, since the organic film prepared by the embodiment of the present invention is cured only after the reflow process, it has been in a semi-cured state before that and has a certain fluidity. Therefore, the embodiment of the present invention has a lower requirement for the high consistency of the conductive structure, i.e., the first conductive structure and the metal bump with spurs, and a larger process window. In addition, the insulating structure of the embodiment of the present invention uses an organic film to isolate the conductive structure to prevent the conductive structure from short-circuiting, and the organic film is very easy to be cleaned and will not cause residual problems. Therefore, the solution of the embodiment of the present invention can also greatly improve the reliability of the prepared three-dimensional stacked packaging structure. Finally, the upper and lower wafers / chips in the embodiment of the present invention are bonded by an organic film, that is, the organic film not only prevents the short circuit of the conductive structure, but also plays the role of a bonding layer between the upper and lower layers. This bonding method avoids the high temperature requirements required for interlayer bonding, and thus avoids the thermal stress and other damages caused by high-temperature processing processes such as hot pressing to the packaging structure, which can effectively improve the reliability of the prepared three-dimensional stacked packaging structure, and effectively reduce the process difficulty of interconnecting the upper and lower chips in the prior art (that is, bonding can be achieved only through reflow process and curing), thereby further reducing the process cost of the three-dimensional stacked packaging. Since the three-dimensional stacked packaging structure prepared by the embodiment of the present invention has a high reliability, and the process difficulty and process cost are lower, it can be widely used in the manufacture of high-performance memory, high-capacity memory, high-bandwidth memory, etc. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the accompanying drawings required for use in the description of the embodiments will be briefly introduced below. Obviously, the accompanying drawings described below are some embodiments of the present invention. For ordinary technicians in this field, other accompanying drawings can be obtained based on these accompanying drawings without paying any creative work.

[0024] Figure 1 A flow chart schematically shows a method for preparing a three-dimensional chip stack according to an embodiment of the present invention;

[0025] Figure 2A flow chart schematically shows a method for preparing a first conductive structure according to an embodiment of the present invention;

[0026] Figure 3 A vertical cross-sectional view schematically shows a chip structure formed in the process of preparing a first conductive structure according to an embodiment of the present invention;

[0027] Figure 4 A vertical cross-sectional view schematically shows a chip structure formed in the process of preparing a first conductive structure according to an embodiment of the present invention;

[0028] Figure 5 A vertical cross-sectional view schematically shows a chip structure formed in the process of preparing a first conductive structure according to an embodiment of the present invention;

[0029] Figure 6 A vertical cross-sectional view schematically shows a chip structure formed in the process of preparing the second conductive structure according to an embodiment of the present invention;

[0030] Figure 7 A vertical cross-sectional view schematically shows a chip structure formed in the process of preparing the second conductive structure according to an embodiment of the present invention;

[0031] Figure 8 A vertical cross-sectional view schematically shows a structure obtained during the preparation process of Example 1 according to one embodiment of the present invention;

[0032] Fig. 9 A vertical cross-sectional view schematically shows a structure obtained during the preparation process of Example 1 according to one embodiment of the present invention;

[0033] Fig.10 A vertical cross-sectional view schematically shows a structure obtained during the preparation process of Example 1 according to one embodiment of the present invention;

[0034] Fig.11 A vertical cross-sectional view schematically shows a structure obtained during the preparation process of Example 1 according to one embodiment of the present invention;

[0035] Fig.12 A vertical cross-sectional view schematically shows a structure obtained during the preparation process of Example 1 according to one embodiment of the present invention;

[0036] Fig.13 A vertical cross-sectional view schematically shows a structure obtained during the preparation process of Example 1 according to one embodiment of the present invention;

[0037] Fig.14A vertical cross-sectional view schematically shows a structure obtained during the preparation process of Example 1 according to one embodiment of the present invention;

[0038] Fig.15 A vertical cross-sectional view schematically shows a structure obtained during the preparation process of Example 1 according to one embodiment of the present invention;

[0039] Fig.16 A vertical cross-sectional view schematically shows a structure obtained during the preparation process of Example 1 according to one embodiment of the present invention;

[0040] Fig.17 A vertical cross-sectional view schematically shows a structure obtained during the preparation process of Example 1 according to one embodiment of the present invention;

[0041] Fig.18 A vertical cross-sectional view schematically shows a structure obtained during the preparation process of Example 2 according to an embodiment of the present invention;

[0042] Fig.19 A vertical cross-sectional view schematically shows a structure obtained during the preparation process of Example 2 according to an embodiment of the present invention;

[0043] Fig. 20 A vertical cross-sectional view schematically shows a structure obtained during the preparation process of Example 3 according to an embodiment of the present invention;

[0044] Fig.21 A vertical cross-sectional view schematically shows a structure obtained during the preparation process of Example 3 according to an embodiment of the present invention;

[0045] Fig. 22 A vertical cross-sectional view of a three-dimensional chip stacking structure in some embodiments is schematically shown. DETAILED DESCRIPTION

[0046] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0047] It should be noted that, in the absence of conflict, the embodiments and features in the embodiments of the present application may be combined with each other.

[0048] It should also be noted that the terms used in this application are generally commonly used by those skilled in the art. If there is any inconsistency with the commonly used terms, the terms in this application shall prevail. For those of ordinary skill in the art, the specific meanings of the terms in this application in the present invention can be understood according to the specific circumstances.

[0049] Finally, it should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply that there is any such actual relationship or order between these entities or operations. It should be understood that the terms used in this way can be interchanged under appropriate circumstances, which is only the way of distinguishing the objects of the same attributes when describing them in the embodiments of the present application. Moreover, the terms "include" and "comprise" not only include those elements, but also include other elements that are not clearly listed, or also include elements inherent to such processes, methods, articles or equipment. In the absence of more restrictions, the elements limited by the statement "include..." do not exclude the existence of other identical elements in the process, method, article or equipment including the elements.

[0050] In this article, the term "chip" refers to any type of semiconductor chip (chip) or integrated circuit chip or semiconductor die (die) or integrated circuit die that implements specific functions and has been cut from a wafer, and also refers to any type of semiconductor chip or integrated circuit chip that implements specific functions and is still on the wafer.

[0051] In this article, the term "chip-level stacking" refers to the die to wafer stacking form, which refers to the stacking packaging process of bonding chips or dies that meet specific functions cut from the wafer together through three-dimensional chip stacking packaging technology to form a three-dimensional chip stacking structure.

[0052] In this article, the term "wafer level stacking" refers to the stacking form of wafer to wafer, which means that when the chip is still on the wafer, one type of whole wafer is bonded to another type of whole wafer through three-dimensional chip stacking packaging technology to form a stacking packaging process with a three-dimensional chip stacking structure.

[0053] The three-dimensional chip stacking packaging technology stacks multiple bare chips or substrates by bonding to achieve a metal interconnection structure of the chip in the three-dimensional direction, greatly reducing the interconnection distance between chips, effectively reducing latency and power consumption, increasing the bandwidth of data transmission, and improving storage capacity, providing an effective solution for the development of high-performance memory. However, the existing three-dimensional chip stacking packaging process often has problems such as difficulty in alignment when interconnecting the upper and lower chips, easy generation of thermal stress problems at high temperatures, complex process flow, and low yield. These problems seriously limit the application of three-dimensional chip stacking packaging in the preparation of high-capacity, high-bandwidth memory. The embodiment of the present invention provides a three-dimensional chip stacking preparation method based on the reflow soldering process, which can enable all chip layers to be stacked and packaged together to be temporarily bonded quickly and accurately at a relatively low temperature, and after temporary bonding, all layers of chips can be completely bonded together through a mass reflow process, which greatly reduces the process difficulty of interconnecting upper and lower chips and the packaging cost of three-dimensional chip stacking in the prior art. The solution provided by the embodiment of the present invention is to prepare an insulating structure before the mass reflow, that is, the stacking of the insulating structure is completed while the chips are stacked, so the high consistency requirements of the conductive structure are lower and the difficulty of preparing the insulating structure is greatly reduced. Therefore, the yield and reliability of the prepared three-dimensional chip packaging structure are effectively improved, and it can be applied to the preparation of high-performance memory. Among them, it should be noted that the lower temperature in the embodiment of the present invention means a temperature lower than the melting point of the material of the first conductive structure. In practical applications, the specific temperature corresponding to the lower temperature can be determined according to the material of the first conductive structure. Taking the first conductive structure as solder as an example, the lower temperature can refer to a temperature lower than the melting point of the solder. When other materials are used to prepare the first conductive structure, the lower temperature can refer to a temperature lower than the melting point of the material of the corresponding material. Of course, in some cases, the lower temperature may also refer to room temperature.

[0054] The embodiments of the present invention will be described in detail below with reference to the accompanying drawings.

[0055] Figure 1 The process of a three-dimensional chip stacking preparation method according to an embodiment of the present invention is schematically shown. Figure 1 As shown, it can be implemented as including:

[0056] Operation S1, forming a conductive structure on a first surface and a second surface of a chip on which TSV and a rewiring layer are prepared, wherein the conductive structure includes a first conductive structure located on the first surface of the chip and a second conductive structure located on the second surface of the chip, and the second conductive structure is a metal bump with a spur;

[0057] Operation S2, preparing a semi-cured organic film on the first surface and / or the second surface of the chip, and opening a window on the semi-cured organic film to expose the first conductive structure and / or the second conductive structure;

[0058] Operation S3, at a relatively low temperature, by sequentially fixing the first conductive structure of the upper chip on the protrusions of the second conductive structure of the lower chip, thereby completing the stacking of the multiple layers of chips;

[0059] Operation S4, applying pressure on the top of the stacked multi-layer chips, and wetting the protrusions and sidewalls of the metal bumps of the first conductive structure of the upper chip and the second conductive structure of the lower chip of the stacked multi-layer chips through a vacuum reflow process, so as to achieve complete bonding of the first conductive structure and the second conductive structure, and bond the upper and lower chips through the semi-cured organic film;

[0060] In operation S5 , the organic film is heated and completely cured to form a three-dimensional chip stacking structure.

[0061] In operation S1, the first surface specifically refers to the surface of the chip where the pin layer is formed, and the prepared first conductive structure is specifically formed on the pin layer. The second surface specifically refers to the other surface of the chip opposite to the surface where the pin layer is formed, on which a rewiring layer is generally prepared, and the second conductive structure is specifically formed on the rewiring layer of the second surface. Of course, in some embodiments, a rewiring layer can also be prepared on the first surface where the pin layer is located according to demand. Before operation S1, the pin layer and the rewiring layer can be prepared by corresponding process flows, which include but are not limited to preparing TSV inside the chip and performing metallization filling, preparing a rewiring layer that is conductive with the TSV on the second surface of the chip, and preparing a pin layer that is conductive with the TSV on the first surface of the chip, etc. These process flows can be prepared according to demand with reference to existing processes, so they will not be repeated here.

[0062] The following is combined with Figures 2 to 5 , the preparation process of the first conductive structure is described in detail. Figure 2 The preparation process of the first conductive structure is schematically shown, as shown in FIG. Figure 2 As shown, it can be implemented as including:

[0063] Operation S11, a layer of photoresist is prepared on the first surface of the chip, and through exposure and development processes, the preparation position of the first conductive structure is exposed. Taking the first conductive structure as a solder ball as an example, the vertical cross-sectional view of the chip structure thus formed is as follows: Figure 3 As shown, solder ball preparation positions 102 separated by photoresist 101 are formed on the first surface 10A of the chip 10 , wherein the solder ball preparation positions and their numbers can be specifically designed according to requirements.

[0064] Operation S12, through the electroplating process, a first conductive structure is prepared at a preparation position on the first surface of the chip. Taking the first conductive structure as a solder ball as an example, the vertical cross-sectional view of the chip structure thus formed is as follows: Figure 4 As shown, solder balls 103 are formed at solder ball preparation positions 102 .

[0065] Operation S13, through the film stripping process, the photoresist on the first surface of the chip is stripped. Taking the first conductive structure as a solder ball as an example, the vertical cross-sectional view of the chip structure thus formed is as follows: Figure 5 As shown, the photoresists 101 on the first surface are all removed, and only solder balls 103 are formed at corresponding preparation positions. These solder balls 103 are the first conductive structures formed on the first surface.

[0066] In some possible implementations, the material of the first conductive structure may be soft gold, indium, gallium, tin, tin-silver, tin-gold, other metals or alloys thereof. Using a soft metal or alloy to prepare the first conductive structure can make it easier to insert and fix the first conductive structure on the protrusion of the second conductive structure, thereby making it easier to achieve temporary bonding between chips.

[0067] In some other possible implementations, the material of the first conductive structure can also be nano- to micron-scale solder. In other possible implementations, the material of the first conductive structure can also be nano- to micron-scale linear or granular conductive porous dielectric materials of metals such as copper, silver, gold, and tin. Using a metal or alloy of this material to prepare the first conductive structure can make it easier for the first conductive structure to be inserted and fixed on the protrusions of the second conductive structure, thereby making it easier to achieve temporary bonding between chips. More preferably, nanoscale particles or mixed particles of nano and micron scales also have the characteristic of low melting point (nanoparticles have low melting point). Using a material with this characteristic to prepare the first conductive structure can also make it easier for the first conductive structure to achieve complete bonding with the second conductive structure during reflow soldering, further reducing the difficulty of the interlayer bonding process. The preparation process of the second conductive structure is similar to the process of preparing the first conductive structure. It is also necessary to first prepare a layer of photoresist on the first surface of the chip, and expose the preparation position of the second conductive structure through exposure and development processes. The difference is that after the preparation position of the second conductive structure is exposed, a metal bump and a spur located above the metal bump are prepared at the corresponding position on the second surface of the chip through electroplating, chemical plating and other processes, and the vertical cross-sectional view of the chip structure thus formed is as follows: Figure 6As shown in FIG. 1 , the formed second conductive structure includes a metal bump 104 and a spur 105 located on the metal bump 104, and the second conductive structure is separated by the photoresist 101 on the second surface 10B. Afterwards, similar to the preparation process of the first conductive structure, a film stripping process is also required to remove the photoresist on the second surface 10B of the chip, and the vertical cross-sectional view of the chip structure thus formed is as shown in FIG. Figure 7 shown.

[0068] It should be noted that when forming the conductive structure, either the first conductive structure or the second conductive structure can be prepared first. When preparing the second conductive structure, the spurs on the metal bump can be prepared at the same time as the metal bump, or the spurs on the metal bump can be prepared after the metal bump is prepared. The embodiment of the present invention does not limit the order. It should also be noted that for the same chip, after the processing of operation S1, the chip structure obtained has conductive structures formed on both the first surface and the second surface. For example, Fig.11 As shown, a first conductive structure, i.e., a solder ball 103, is formed on the first surface 10A of the obtained chip structure, and a second conductive structure, i.e., a metal bump 104 with a spur 105, is formed on the second surface. Among them, the spurs and the metal bumps in the second conductive structure can be made of different materials or the same material, and the embodiment of the present invention is not limited to this. In some possible embodiments, the material of the metal bump of the second conductive structure is a metal such as copper, nickel, gold, silver, or an alloy thereof, and the material of the spurs of the second conductive structure is selected from metals such as nickel, copper, gold, or silver. In other embodiments, the material of the second conductive structure can also be selected from other metals or alloys, as long as its hardness is higher than that of the first conductive structure, so that the first conductive structure can be more easily inserted and fixed on the spurs of the second conductive structure, thereby making it easier to achieve temporary bonding between chips. It should be noted that when the metal bumps and spurs of the second conductive structure are made of the same material, it is preferred to consider preparing the metal bumps and spurs at one time. For example, taking the case where both the metal bumps and the protrusions are made of copper, the metal bumps and the protrusions can be prepared at one time by electroplating. In this case, the prepared metal bump refers to a relatively neat metal layer at the bottom, and the protrusion is a metal structure protruding from the surface of the relatively neat metal layer.

[0069] As a possible implementation manner, the height of the metal bump is between 0.5 micrometers and 50 micrometers, and the height of the protrusion is between 0.05 micrometers and 10 micrometers.

[0070] In a preferred embodiment, a metal protective film may be prepared on the surface and sidewalls of the metal bumps, and the metal used in the metal protective film may be silver, gold, nickel or palladium. Preferably, the metal used in the metal protective film is a metal different from the material of the metal bumps. By preparing a metal protective film on the surface and sidewalls of the metal bumps, the metal bumps can be protected during the three-dimensional stacking packaging process, effectively preventing the metal bumps from oxidation, thereby improving the reliability of the prepared three-dimensional stacking structure.

[0071] As a possible implementation, the spurs on the metal bump in the second conductive structure are formed by deposition by chemical or physical methods. In a preferred implementation, the surface of the spurs can also be plated with an inert metal passivation layer such as palladium or gold to protect the spurs and prevent them from oxidation. In actual operation, the metal protective film of the metal bump and the inert metal passivation layer of the spurs can be prepared together or separately, and they can be prepared using exactly the same materials or different materials. For example, taking the metal bump as a copper metal bump, the material of the spur as copper, and the materials of the metal protective film and the inert metal passivation layer as palladium and gold, nano copper wires can be prepared on the copper metal bumps by electroplating, and then a layer of palladium and gold is electroplated on the copper wire and the copper metal surface and sidewalls for passivation treatment, thereby preparing a second conductive structure with a metal protective film and an inert metal passivation layer.

[0072] As a preferred embodiment, the spikes can be formed into clusters of metal wires, rods, cones or other shapes, and the diameter of the smallest unit constituting the cluster is in the nanometer to micrometer range. Preparing the spikes into such a structure allows the spikes to be better inserted into the first conductive structure during temporary bonding, thereby playing a stable fixing role and improving the bonding effect of temporary bonding. It should be noted that the clusters are aggregates of smaller particles, and the diameter of the smallest unit constituting the clusters is in the nanometer to micrometer range, which means that the diameters of these smaller particles are in the nanometer to micrometer range.

[0073] like Figure 5 and 7As shown, the first conductive structure and the second conductive structure are both arranged at intervals, that is, there are gaps between adjacent first conductive structures and second conductive structures. As a preferred embodiment, in order to achieve insulation isolation between the first conductive structures to prevent short circuits of the conductive structures, and also to achieve close bonding between adjacent chip layers, in an embodiment of the present invention, an organic film filled in the gaps between the first conductive structure and / or the second conductive structure is prepared on the first surface and / or the second surface of the chip, so as to achieve isolation between the conductive structures through the filled organic film, prevent the occurrence of short circuits, and achieve close bonding and stable bonding between the upper and lower chips. The use of organic film as the insulating structure can not only achieve isolation between conductive structures, but also because the embodiment of the present invention prepares an organic film in a semi-cured state, the bonding between the upper and lower chips can be achieved through the organic film. Compared with inorganic insulating materials such as silicon dioxide, the insulating structure of the embodiment of the present invention can achieve bonding between the upper and lower chips during the vacuum reflow process, and the bonding between the insulating structures can be completed only by heating and curing after the vacuum reflow process. The bonding difficulty is much lower than that of inorganic insulating materials. This also enables the embodiment of the present invention to prepare and stack the insulating structure before the reflow process. Compared with the traditional reflow soldering process, the preparation difficulty and bonding difficulty of the insulating structure are greatly reduced. Moreover, since the insulating structure is prepared before the reflow process and the insulating structure is an organic film in a semi-cured state, the method of the embodiment of the present invention has low requirements for the high consistency of the conductive structure, especially the first conductive structure, which further reduces the process difficulty and packaging cost of the stacked package, while also avoiding warping and improving the reliability of the prepared three-dimensional stacked structure. In operation S2, an organic film can be prepared only in the gap between the first conductive structure of the chip, or only in the gap between the second conductive structure of the chip, or simultaneously in the gap between the first conductive structure and the second conductive structure. The organic film can be specifically a negative photoresist. For example, the negative photoresist can be prepared by a dry film method or a coating method using a single material or a composite material such as polyimide, photoresist, epoxy resin, etc. Since the negative photoresist is very easy to be washed off, there will be no residual problem. Therefore, the solution of the embodiment of the present invention effectively avoids the problems of disconnection and reliability caused by the easy residue of insulating materials between the upper and lower layers of solder, and further improves the reliability of the prepared three-dimensional stacked structure. The specific method of preparing the organic film can be to prepare a layer of negative photoresist in B-stage on the surface of the chip where the first conductive structure and / or the second conductive structure are formed, and then open a window on the negative photoresist in B-stage through exposure, development and other processes, so that the conductive structure on the corresponding surface, that is, the first conductive structure and / or the second conductive structure, is exposed, so that the organic film can fill the gap between the first conductive structure and / or the second conductive structure.Specifically, the thickness of the prepared organic film can be determined according to the height of the gap between the upper and lower chips, and can be exemplarily between 2-50 μm. Preferably, the organic film prepared in the embodiment of the present invention is in a semi-cured state. Among them, the semi-cured state preferably refers to the organic film prepared by operation S2 being in the B-stage and having a certain fluidity. The organic film in a semi-cured state makes the organic film of the embodiment of the present invention not only act as an insulating structure for isolating the conductive structure, but also play a role in achieving the bonding of the upper and lower chip layers. At the same time, since the organic film of the embodiment of the present invention before the reflow process is fluid, it can also reduce the bonding requirements between the first conductive structure on the upper chip, such as solder, and the metal bumps on the lower chip, such as the consistency of the height of the solder and the metal bumps.

[0074] It should be noted that, in a specific implementation, operation S2 is not limited to being performed after operation S1, and it may be performed after the corresponding conductive structure is prepared. For example, in the case of filling the gap of the first conductive structure with an organic film, after the first conductive structure is prepared (such as after operation S13), a layer of negative photoresist is directly prepared on the first surface, and then a window is opened on the organic film in a semi-cured state through exposure, development and other processes to expose the first conductive structure to form an organic film filling the gap of the first conductive structure; in the case of filling the gap of the first conductive structure and the second conductive structure with an organic film at the same time, after the corresponding conductive structure is prepared, an organic film filling the gap of the corresponding conductive structure may be prepared, and then another conductive structure preparation process is performed.

[0075] Since the second conductive structure of the embodiment of the present invention is a metal bump with protrusions, therefore, in operation S3, the embodiment of the present invention can fix the first conductive structure of the stacked upper chips on the protrusions of the second conductive structure of the lower chip through a pick and place process, thereby achieving temporary bonding between chips under low temperature conditions, facilitating and quickly completing the stacking of multi-layer chips. The process is simple and can effectively reduce the process difficulty and cost of interconnection between chips. Furthermore, since high-temperature hot pressing is not required, damage to the stacked structure by thermal stress can be avoided, thereby improving the reliability and yield of the prepared three-dimensional chip stacking structure.

[0076] In specific applications, the operation of fixing the first conductive structure of the upper chip on the protrusion of the second conductive structure of the lower chip can be repeated according to the number of chips to be stacked to complete the stacking of multiple layers of chips. Among them, in a preferred embodiment, before fixing the first conductive structure of the upper chip on the protrusion of the second conductive structure of the lower chip, the upper chip to be placed on the lower chip can be pre-treated by heating formic acid or the like to prevent the first conductive structure of the upper chip and the second conductive structure of the lower chip from being oxidized during fixation, thereby ensuring the yield of chip interconnection and the reliability of the prepared three-dimensional chip stacking structure. It should be noted that the pick and place process (also known as the pick-place process) is a mature prior art technology that can be implemented by reference and will not be described in detail here. It should also be noted that in operation S3, under relatively low temperature conditions, temporary bonding and stacking of all chip layers can be completed only by a pick-and-place process, and since a semi-cured organic film has been prepared in advance in operation S2, not only the temporary bonding and stacking of all chip layers is completed by operation S3, but also the stacking of insulating structures between all chip layers is completed, so that through the reflow process of operation S4, the bonding of the conductive structures and insulating structures between all layers of chips can be completed in batches, greatly improving the packaging efficiency and reducing the packaging cost. In operation S4, by subjecting the multi-layer stacked chips formed by temporary bonding in operation S3 to a vacuum reflow process, the conductive structures of the stacked multi-layer chips can be completely bonded, and at the same time, the upper and lower chips can be bonded by the organic film. Among them, in a preferred embodiment of the present invention, applying pressure on the top of the stacked multi-layer chips can effectively ensure the strength of the bonding between the upper and lower chips, thereby ensuring the long-term reliability of the prepared three-dimensional chip stacking structure.

[0077] Among them, the vacuum reflow process (also known as vacuum reflow soldering process) is a mature existing technology. In operation S4, the vacuum reflow process can be performed with reference to the existing technology to achieve complete bonding of the first conductive structure of the upper chip and the metal bumps of the lower chip. By adopting the vacuum reflow process, oxidation of the first conductive structure of the upper chip and the second conductive structure of the lower chip can be further avoided, thereby improving the yield of the package and the reliability of the prepared three-dimensional chip stacking structure.

[0078] In the embodiment of the present invention, before the first conductive structure of the upper chip and the metal bump of the lower chip are completely bonded by vacuum reflow, the organic film is in the B-stage and has a certain fluidity (i.e., semi-cured state). Therefore, by applying pressure and vacuum reflow at the top of operation S4, the organic film can fully fill the gap between the upper chip and the lower chip, and the upper chip and the lower chip are more tightly bonded. After that, by further heating and curing the organic film by operation S5, the complete bonding of the insulating structure can be completed, and the difficulty of the bonding process of the insulating structure can be greatly reduced. Moreover, since the organic film is easily removed by using negative photoresist, the yield of the interconnection between the chips and the reliability of the packaging structure can also be greatly improved. In particular, after vacuuming and reflowing, the first conductive structure and the second conductive structure can be completely infiltrated to achieve complete bonding, and in particular, the first conductive structure can diffuse and fill the gaps formed between the organic films to further improve and ensure the yield and stability of the chip interconnection.

[0079] It should be noted that, in the case where the organic film is prepared only in the gaps between the first conductive structures of the chip, the organic film is bonded to the second surface of the lower chip after the vacuum reflow process of operation S4 to achieve bonding between adjacent layers of chips; in the case where the organic film is prepared only in the gaps between the second conductive structures of the chip, the organic film is bonded to the first surface of the upper chip after vacuum reflow to achieve bonding between adjacent layers of chips; in the case where the organic film is prepared in the gaps between the first conductive structures of the chip and the gaps between the second conductive structures of the chip at the same time, the organic film in the gap between the solder of the upper chip and the organic film in the gap between the metal bumps of the lower chip are bonded to each other after vacuum reflow, thereby achieving bonding between adjacent layers of chips. Based on this, when preparing the organic film, there are more process route options (such as preparing the organic film only in the gaps of the first conductive structure, or preparing the organic film only in the gaps of the second conductive structure, etc.), and the process window is larger, thereby further reducing the difficulty of process preparation.

[0080] In specific applications, the above-mentioned preparation method of the embodiment of the present invention can be applied to both the chip-level stacking packaging process and the wafer-level stacking packaging process. When applied to the chip-level stacking packaging process, before the pick-and-place process is used to stack the chips, the wafer needs to be diced into independent chips, while when applied to the wafer-level stacking packaging process, the dicing process can be performed after operation S5.

[0081] The following will take solder as an example of the first conductive structure to exemplify the process of preparing a three-dimensional chip stacking structure by applying the above three-dimensional chip stacking preparation method through three specific embodiments.

[0082] Example 1

[0083] Step 1: Make TSV inside the chip of the wafer and perform metallization filling. Prepare a metal rewiring layer on the second surface of the chip. Thin the wafer to expose the TSV and other structures. Make a rewiring layer on the first surface of the chip, including functional conductive pins and non-functional thermal conductive pins, to obtain the following pin layer: Figure 8 The chip structure including TSV 106 is shown, wherein the metal rewiring layer and the pin layer are not shown;

[0084] Step 2: Prepare a layer of photoresist on the first surface of the chip, and expose the preparation position of the solder ball through exposure and development processes to obtain Figure 3 The chip structure shown includes TSV 106 and a plurality of solder preparation locations 102 separated by photoresist 101;

[0085] Step 3: Prepare solder balls on the first surface of the chip through electroplating process to obtain Figure 4 The chip structure shown includes TSV 106 and solder balls 103 separated by photoresist 101;

[0086] Step 4: Remove the photoresist on the first surface of the chip through a film stripping process to obtain Figure 5 The chip structure shown includes TSV 106 and solder balls 103 arranged at intervals;

[0087] Step 5: Prepare a layer of negative photoresist on the first surface of the chip to obtain Fig. 9 The chip structure shown includes TSV 106 and solder balls 103 covered by negative photoresist 107;

[0088] Step 6: Through the exposure and development process, the solder balls on the first surface of the chip are exposed to obtain Fig.10 The chip structure shown includes TSV 106 and solder balls 103 separated by negative photoresist 107. Negative photoresist 107 is an organic film in a semi-cured state, which fills the gaps between solder balls 103.

[0089] Step 7: Repeat steps 1 and 2 to expose the preparation position of the metal bump, and then prepare the metal bump and the spurs above the metal bump on the second surface of the chip by electroplating, chemical plating and other processes. Specifically, prepare the copper metal bump by electroplating, and then prepare the nano copper wire on the copper metal bump by electroplating, and then chemically plate a layer of palladium and gold on the copper wire and the copper metal surface and side wall for passivation treatment, thereby preparing a second conductive structure with a metal protective film and an inert metal passivation layer, and obtaining the following Fig.11 The chip structure shown includes TSV 106 , solder balls 103 separated by negative photoresist 107 on the first surface 10A, and metal bumps 104 with protrusions 105 separated by photoresist 101 on the second surface 10B;

[0090] Step 8: Remove the photoresist on the first surface of the chip through the film stripping process to obtain Fig.12 The chip structure shown includes TSV 106, solder balls 103 separated by negative photoresist 107 on the first surface 10A, and metal bumps 104 with protrusions 105 arranged at intervals on the second surface 10B;

[0091] Step 9: Prepare a layer of negative photoresist on the second surface of the chip to obtain Fig.13 The chip structure shown includes TSV 106 , solder balls 103 separated by negative photoresist 107 on the first surface 10A, and metal bumps 104 with protrusions 105 covered by negative photoresist 107 on the second surface 10B;

[0092] Step 10: Through exposure, development and other processes, the metal bumps and protrusions on the second surface of the chip are exposed to obtain Fig.14 The chip structure shown includes TSV 106 , solder balls 103 separated by negative photoresist 107 on the first surface 10A, and metal bumps 104 with protrusions 105 separated by negative photoresist 107 on the second surface 10B;

[0093] Step 11: Pre-treat the chip structure obtained in step S10 with heated formic acid, and then fix the upper chip on the lower chip by pick and place method under vacuum environment through the solder balls of the upper chip and the metal bumps with thorns of the lower chip, so as to obtain Fig.15 The chip stacking structure shown includes two layers of chips 10, wherein Fig.15 As shown, the solder balls 103 of the upper chip 10 are fixed on the metal bumps 104 with spurs 105 of the lower chip 10;

[0094] Step 12: By repeating the process from step 1 to step 11, multiple layers of chips are stacked to obtain Fig.16 The multi-layer chip stacking structure 100 shown in FIG. Fig.16 As shown, in this structure, the upper and lower chips are only temporarily bonded, and there is still a gap 108, which means they are not completely bonded.

[0095] Step 13: Through vacuuming, reflow and other processes, the solder of the upper chip is completely bonded with the metal bumps of the lower chip, and the organic film is heated and cured to obtain Fig.17 The three-dimensional chip stacking structure 200 shown in FIG. Fig.17As shown, in this structure, after vacuuming and reflow, the solder diffuses and fills the gaps formed between the organic films, the solder of the upper chip is completely bonded to the metal bumps of the lower chip, and the organic film on the first surface of the upper chip is completely bonded to the organic film on the second surface of the lower chip, forming a stable interconnected three-dimensional chip stacking structure.

[0096] Example 2

[0097] Step 1-8: Same as step 1-8 of Example 1;

[0098] Step 9: Pre-treat with heated formic acid, and then fix the upper chip on the lower chip by pick and place method under vacuum environment through the solder balls of the upper chip and the metal bumps with thorns of the lower chip, so as to obtain Fig.18 The chip stacking structure shown includes upper and lower layers of chips 10, such as Fig.18 As shown, it is Fig.15 The difference of the structure shown is that, in this embodiment, no organic film isolation wall is prepared around the metal bumps on the second surface of the chip, that is, the metal bumps are not isolated by the organic film, and only the organic film isolation wall is prepared at the gap between the solder balls on the first surface;

[0099] Step 10: By repeating the processes of steps 1 to 9 above, multiple layers of chips are stacked to obtain Fig.19 The multi-layer chip stacking structure 100 shown in FIG. Fig.19 As shown, in this structure, the upper and lower chips are only temporarily bonded, and there is still a gap 108, which is not completely bonded. In addition, since no organic film is prepared on the second surface, the organic film on the first surface cannot be bonded to the second surface of the lower chip before vacuum reflow.

[0100] Step 11: The same as step 13 of Example 1, except that, in this embodiment, since no organic film is prepared on the second surface, after vacuum reflow, the organic film on the first surface is directly bonded to the second surface of the lower chip to achieve bonding between the chips.

[0101] Example 3

[0102] Step 1-4: same as step 1-4 of Example 1;

[0103] Steps 5-8: Same as steps 7-10 of Example 1;

[0104] Step 9: Pre-treat with heated formic acid, and then fix the upper chip on the lower chip by pick and place method under vacuum environment through the solder balls of the upper chip and the metal bumps with thorns of the lower chip, so as to obtain Fig. 20The chip stacking structure shown includes upper and lower layers of chips 10, such as Fig. 20 As shown, it is Fig.21 The difference of the structure shown is that, in this embodiment, no organic film isolation wall is prepared around the solder balls on the first surface of the chip, and only organic film isolation walls are prepared at the gaps between the metal bumps on the second surface;

[0105] Step 10: By repeating the processes of steps 1 to 9 above, multiple layers of chips are stacked to obtain Fig.21 The multi-layer chip stacking structure 100 shown in FIG. Fig.21 As shown, in this structure, the upper and lower chips are only temporarily bonded, there is still a gap, and they are not completely bonded. In addition, since no organic film is prepared on the first surface, the organic film on the second surface cannot be bonded to the first surface of the lower chip before vacuum reflow.

[0106] Step 11: The same as step 13 of Example 1, except that, in this embodiment, since no organic film is prepared on the first surface, after vacuum reflow, the organic film on the second surface is directly bonded to the first surface of the upper chip to achieve bonding between chips.

[0107] Fig. 22 A vertical cross-sectional view of a three-dimensional chip stacking structure 300 according to an embodiment of the present invention is schematically shown. Fig. 22 As shown, it includes a substrate 301, at least two chip layers 302 located on the substrate, at least two bonding structures 306 located between adjacent chip layers 302, and an organic film 304 located between adjacent chip layers 302 for bonding adjacent chip layers 302, and the organic film 304 isolates the adjacent bonding structures 306 from each other. Each chip layer 302 includes at least one chip 303, each chip is provided with a TSV 305 penetrating the chip, and the first surface 303A and the second surface 303B of each chip 303 are electrically connected through the TSV penetrating the chip. The first surface 303A refers to the surface of the chip or chip layer provided with the first conductive structure, and the second surface 303B refers to the surface of the chip or chip layer provided with the second conductive structure, and the bonding structure is formed by bonding the first conductive structure of the first surface of the chip located in the upper chip layer and the second conductive structure of the second surface of the chip located in the lower chip layer. Preferably, the second conductive structure is a metal bump with thorns, and the organic film is formed by heating the semi-cured organic film to fully cure it. Preferably, the organic film is formed based on a single material or a composite material such as polyimide, photoresist, or epoxy resin via a dry film method or a coating method, and the thickness of the organic film may be between 2-50 μm.

[0108] In some possible implementations, the material of the first conductive structure may be soft gold, indium, gallium, tin, tin-silver, tin-gold, other metals or alloys thereof. Using a soft metal or alloy to prepare the first conductive structure can make it easier to insert and fix the first conductive structure on the protrusion of the second conductive structure, thereby making it easier to achieve temporary bonding between chips.

[0109] In some other possible implementations, the material of the first conductive structure may also be nano to micron-scale solder. In other possible implementations, the material of the first conductive structure may also be nano to micron-scale linear or granular conductive porous dielectric materials of metals such as copper, silver, gold, and tin. Using such a metal or alloy to prepare the first conductive structure can make it easier for the first conductive structure to be inserted and fixed on the protrusions of the second conductive structure, thereby making it easier to achieve temporary bonding between chips. More preferably, nano-scale particles or mixed particles of nano and micron scales also have the characteristic of low melting point (nanoparticles have low melting point). Using such a material to prepare the first conductive structure can also make it easier for the first conductive structure to achieve complete bonding with the second conductive structure during reflow soldering, further reducing the difficulty of implementing the interlayer bonding process.

[0110] In some possible implementations, the material of the metal bumps of the second conductive structure is copper, nickel, gold, silver or other metals or alloys thereof, and the material of the protrusions of the second conductive structure is selected from nickel, copper, gold, silver or other metals. In other implementations, the material of the second conductive structure may also be other metals or alloys, as long as the hardness thereof is higher than that of the first conductive structure, so that the first conductive structure can be more easily inserted and fixed on the protrusions of the second conductive structure, thereby making it easier to achieve temporary bonding between chips.

[0111] As a possible implementation manner, the height of the metal bump is between 0.5 micrometers and 50 micrometers, and the height of the protrusion is between 0.05 micrometers and 10 micrometers.

[0112] In a preferred embodiment, a metal protective film can be prepared on the surface and sidewall of the metal bump to passivate and protect the metal bump to prevent it from being oxidized, thereby improving the reliability of the three-dimensional chip stacking structure. The metal used in the metal protective film can be silver, gold, nickel or palladium. Preferably, the metal used in the metal protective film is a metal different from the material of the metal bump.

[0113] As a possible implementation, the spurs on the metal bumps in the second conductive structure are formed by chemical or physical deposition. In a preferred implementation, the surface of the spurs may also be plated with an inert metal passivation layer such as palladium or gold to protect the spurs from oxidation.

[0114] As a preferred embodiment, the spurs can be formed into metal clusters in the shape of wires, rods, cones or other shapes, and the diameter of the smallest unit constituting the cluster is in the nanometer to micrometer level, so that the spurs can be more easily and firmly inserted into the first conductive structure, making the temporary bonding process easier to achieve.

[0115] The three-dimensional chip stacking structure of the embodiment of the present invention is easy to prepare and has a low packaging cost, and also has a higher yield and reliability, and can therefore be widely used in high-performance memories, high-capacity memories, high-bandwidth memories, and the like.

[0116] It should be noted that the number of chips in each chip layer can be selected according to needs and expectations. Each chip can be a chip that implements the same function or a chip that implements different functions. Each chip can be a chip on a wafer or an independent chip cut from a wafer. The embodiment of the present invention does not limit this. In addition, in specific applications, the number of the first conductive structure, TSV, and the second conductive structure can also be set according to needs and expectations. In specific applications, the first surface and the second surface of the chip can also be formed with a rewiring layer according to needs. The number of rewiring layers can be designed according to needs and expectations. In some embodiments, the first surface of the chip can also be formed with a pin layer according to needs.

[0117] As a preferred embodiment, Fig. 22 The three-dimensional chip stacking structure shown can be manufactured by the method of any of the aforementioned embodiments.

[0118] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present application, rather than to limit it. Although the present application has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or make equivalent replacements for some of the technical features therein. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present application.

Claims

1. Three-dimensional chip stacking preparation method, It is characterized in that include: Forming a conductive structure on the first surface and the second surface of the chip on which the TSV and the rewiring layer are prepared, wherein the conductive structure includes a first conductive structure located on the first surface of the chip and a second conductive structure located on the second surface of the chip, and the second conductive structure is a metal bump with a spur; Preparing a semi-cured organic film on the first surface and / or the second surface of the chip, and opening a window on the semi-cured organic film to expose the first conductive structure and / or the second conductive structure; The first conductive structure of the upper chip is sequentially fixed to the protrusion of the second conductive structure of the lower chip by a pick and place process to complete the stacking of the multi-layer chips; Applying pressure on the top of the stacked multi-layer chips, through a vacuum reflow process, wetting the protrusions and sidewalls of the metal bumps of the first conductive structure of the upper chip and the second conductive structure of the lower chip of the stacked multi-layer chips, so as to achieve complete bonding between the first conductive structure and the second conductive structure, and bonding the upper and lower chips through the semi-cured organic film; The organic film is heated and completely cured to form a three-dimensional chip stacking structure.

2. The method according to claim 1, It is characterized in that The material of the first conductive structure is soft gold, indium, gallium, tin, tin-silver, tin-gold, other metals or alloys thereof; Alternatively, the material of the first conductive structure is nano- to micron-scale solder; Alternatively, the material of the first conductive structure is a nano- to micron-scale linear or granular conductive porous dielectric material of metals such as copper, silver, gold, and tin.

3. The method according to claim 1, It is characterized in that The metal bumps of the second conductive structure are made of copper, nickel, gold, silver, or alloys thereof; and the height of the metal bumps is between 0.5 micrometers and 50 micrometers.

4. The method according to claim 3, It is characterized in that A layer of metal protection film is also prepared on the surface and side wall of the metal bump. The metal used in the metal protection film is silver, gold, nickel or palladium, and the metal used in the metal protection film is different from the material of the metal bump.

5. The method according to claim 1, It is characterized in that The protrusions on the metal bumps in the second conductive structure are formed by deposition by chemical or physical methods; The material of the protrusion is selected from nickel, copper, gold, or silver; the height of the protrusion is between 0.05 microns and 10 microns.

6. The method according to claim 5, It is characterized in that The surface of the spur is also plated with an inert metal passivation layer; The spurs are metal clusters in the shape of wires, rods, cones or other shapes, and the diameter of the smallest unit constituting the cluster is in the nanometer to micrometer level.

7. The method according to any one of claims 1 to 6, It is characterized in that The organic film is a negative photoresist, and the negative photoresist is prepared by a dry film method or a coating method using a single material or a composite material of polyimide, epoxy resin, or photoresist.

8. The method according to any one of claims 1 to 6, It is characterized in that Bonding the upper and lower chips by the semi-cured organic film includes: When the semi-cured organic film is prepared only in the gap of the first conductive structure, the semi-cured organic film located in the gap of the first conductive structure of the upper chip is bonded to the second surface of the lower chip after vacuum reflow, so as to achieve bonding of the upper and lower chips; When the semi-cured organic film is prepared only in the gap of the second conductive structure, the semi-cured organic film in the gap of the second conductive structure of the lower chip is bonded to the first surface of the upper chip after vacuum reflow, so as to achieve bonding of the upper and lower chips; When a semi-cured organic film is prepared in the gap between the first conductive structure and the second conductive structure at the same time, the semi-cured organic film in the gap between the first conductive structure of the upper chip and the semi-cured organic film in the gap between the second conductive structure of the lower chip are bonded to each other after vacuum reflow to achieve bonding of the upper and lower chips.

9. The method according to any one of claims 1 to 6, It is characterized in that Before fixing the first conductive structure of the upper chip on the protrusion of the second conductive structure of the lower chip, the method further includes: Pre-treat the chip using heated formic acid.

10. Application of the method according to any one of claims 1 to 9 in chip-level stacking or wafer-level stacking.

11. Three-dimensional chip stacking structure, It is characterized in that include: substrate; At least two chip layers are located on the substrate, each chip layer includes at least one chip; at least two bonding structures located between adjacent chip layers; An organic film located between adjacent chip layers for bonding adjacent chip layers, the organic film isolating adjacent bonding structures from each other, wherein the organic film is formed by heating the semi-cured organic film to fully cure it after the bonding structure is prepared; A TSV penetrating the chips in the chip layer, wherein the first surface and the second surface of each chip are connected via the TSV penetrating the chip; Wherein, the bonding structure is formed by the following method: The first conductive structure of the upper chip is fixed to the second conductive structure of the lower chip in sequence by a pick and place process to complete the stacking of the multi-layer chips, wherein the second conductive structure is a metal bump with spurs, and the first conductive structure is fixed to the spurs of the second conductive structure; Pressure is applied on the top of the stacked multi-layer chips, and through a vacuum reflow process, the protrusions and side walls of the metal bumps of the first conductive structure of the upper chip and the second conductive structure of the lower chip of the stacked multi-layer chips are wetted to achieve complete bonding of the first conductive structure and the second conductive structure, thereby forming the bonding structure.

12. The three-dimensional chip stacking structure according to claim 11, It is characterized in that The material of the first conductive structure is soft gold, indium, gallium, tin, tin-silver, tin-gold, other metals or alloys thereof; Alternatively, the material of the first conductive structure is nano- to micron-scale solder; Alternatively, the material of the first conductive structure is a nano- to micron-scale linear or granular conductive porous dielectric material of metals such as copper, silver, gold, and tin.

13. The three-dimensional chip stacking structure according to claim 11, It is characterized in that The metal bumps of the second conductive structure are made of copper, nickel, gold, silver, or alloys thereof; and the height of the metal bumps is between 0.5 micrometers and 50 micrometers.

14. The three-dimensional chip stacking structure according to claim 11, It is characterized in that The surface and side wall of the metal bump also include a metal protection film. The metal used in the metal protection film is silver, gold, nickel or palladium, and the metal used in the metal protection film is different from the material of the metal bump.

15. The three-dimensional chip stacking structure according to claim 11, It is characterized in that The protrusions on the metal bumps in the second conductive structure are formed by chemical or physical deposition.

16. The three-dimensional chip stacking structure according to claim 11, It is characterized in that The material of the protrusion is selected from nickel, copper, gold, or silver; the height of the protrusion is between 0.05 microns and 10 microns.

17. The three-dimensional chip stacking structure according to claim 16, It is characterized in that The surface of the spur is also plated with an inert metal passivation layer; The spurs are metal clusters in the shape of wires, rods, cones or other shapes, and the diameter of the smallest unit constituting the cluster is in the nanometer to micrometer level.

18. The three-dimensional chip stacking structure according to claim 11, It is characterized in that The organic film is a negative photoresist, and the negative photoresist is prepared by a dry film method or a coating method using a single material or a composite material of polyimide, epoxy resin, or photoresist.

19. The three-dimensional chip stacking structure according to claim 11, It is characterized in that The three-dimensional chip stacking structure is a chip-level stacking structure or a wafer-level stacking structure.

20. Three-dimensional chip stacking structure, It is characterized in that It is prepared by the method described in claim 1.

Citation Information

Patent Citations

  • Stacked semiconductor package and manufacturing thereof

    KR1020170052304A

  • Integrated circuit stacking structure and manufacturing method therefor, and electronic apparatus

    WO2022236640A1

  • Packaging method and packaging structure of multi-layer stacked high-bandwidth memory

    WO2023104093A1