A high-strength and high-toughness automobile safety belt plastic buckle
Through the composite structure of polycarbonate resin and modified silicon nitride fiber and other materials, the problem of insufficient strength and toughness of the automotive seat belt buckle material is solved, and a high-strength, high-strength, high-strength and heat-resistant automotive seat belt plastic card is realized , improves security and user experience.
Patent Information
- Application Number
- CN202311575712.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-11-24
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2043-11-24
AI Technical Summary
The material strength and toughness of existing car seat belt buckles are insufficient, which is prone to permanent deformation due to creep, which affects the user experience and poses safety hazards.
Using a composite structure of polycarbonate resin, modified silicon nitride fiber, acrylonitrile-styrene-acrylate copolymer and other materials, the silicon nitride fiber is treated by surface modification, and flame retardant, toughener, and lubricant are added. and antioxidants to form high-strength, high-toughness, high-temperature resistant plastic snaps.
It improves the strength, toughness and heat resistance of the snap, reduces the possibility of creep, enhances the processability and performance of the material, and improves the safety and user experience of the seat belt.
Abstract
Description
Technical Field
[0001] The invention relates to the field of automobile accessories, and in particular to a high-strength and high-toughness automobile safety belt plastic buckle. Background Art
[0002] The car seat belt limit buckle is a buckle structure installed on the car seat belt for adjusting the positioning, usually made of plastic. The car seat belt is a necessary safety measure for people when riding in a car, and people of different body shapes need to adjust the length of the seat belt appropriately when using it. If the seat belt is too tight, it will cause discomfort, and if it is too loose, it will not play a safety protection role; the car seat belt limit buckle can be used to adjust and limit the seat belt to a suitable length.
[0003] In order to make it more convenient to use and enhance the hand feeling experience, most of the existing car seat belt buckles use some high-strength plastic products. However, due to the high frequency of use of car seat belt buckles, many current plastic products cannot fully meet the needs, such as insufficient strength or insufficient toughness leading to cracking, and easy to produce permanent deformation due to creep after long-term use, resulting in the buckle being unable to be assembled normally, etc. These situations not only greatly reduce people's use experience, but also cause greater safety hazards. Therefore, the current automotive market needs a car seat belt plastic buckle with high strength, strong toughness, good corrosion resistance, good creep resistance, and good heat resistance to improve the safety of car seat belts. Summary of the invention
[0004] In view of the problems existing in the prior art, the object of the present invention is to provide a high-strength and high-toughness automobile safety belt plastic buckle.
[0005] The purpose of the present invention is achieved by adopting the following technical solutions:
[0006] A high-strength and high-toughness automobile safety belt plastic buckle, the material components of which are calculated by weight and include:
[0007] 50-80 parts of polycarbonate resin, 12-24 parts of acrylonitrile-styrene-acrylate copolymer, 5-10 parts of modified silicon nitride fiber, 3-8 parts of flame retardant, 3-6 parts of toughening agent, 1-3 parts of lubricant, 0.1-0.4 parts of anti-dripping agent and 0.5-1 parts of antioxidant.
[0008] Preferably, the polycarbonate resin is Chimei PC-6600 with a specific gravity of 1.2 g / cm 3 , the melt index is 10g / 10min (300℃, 1.2kg).
[0009] Preferably, the acrylonitrile-styrene-acrylate copolymer is of Chimei PW-978B, with a specific gravity of 1.07 g / cm3 , the melt index is 13g / 10min (220℃, 10kg).
[0010] Preferably, the preparation method of the modified silicon nitride fiber comprises:
[0011] S1. Surface treatment of silicon nitride fiber:
[0012] Weigh silicon nitride fiber and 3-aminopropyltrimethoxysilane, mix them in deionized water, stir them at 70-80° C. for 6-10 hours, remove the liquid after the treatment, wash them three times with water, and dry them in an oven to obtain amino-treated silicon nitride fiber;
[0013] Wherein, the mass ratio of silicon nitride fiber, 3-aminopropyltrimethoxysilane and deionized water is 1:0.1-0.4:10;
[0014] S2. Synthesis of prepolymerization modification reaction solution:
[0015] Weigh trioxymethylene and dissolve it in N-methylpyrrolidone, then add a small amount of deionized water and mix well, stir at 70-80°C for half an hour to obtain a mixed solution A;
[0016] Wherein, the mass ratio of trioxymethylene, deionized water and N-methylpyrrolidone is 0.3-0.6:0.1-0.3:2-5;
[0017] The amino-modified silicon nitride fiber and 4,4'-(1,4-phenylenedioxy) dianiline are mixed in N-methylpyrrolidone and uniformly dispersed by ultrasonication at room temperature to obtain a mixed solution B;
[0018] Wherein, the mass ratio of the amino-modified silicon nitride fiber, 4,4'-(1,4-phenylenedioxy) dianiline and N-methylpyrrolidone is 1:0.2-0.4:4-10;
[0019] Heat the mixed solution B to 55-65°C, slowly add the mixed solution A, and add it all within half an hour, then continue stirring and reacting for half an hour to obtain the prepolymerization modification reaction solution;
[0020] Wherein, the mass ratio of mixed solution A to mixed solution B is 1:1;
[0021] S3. Synthesis of modified silicon nitride fiber:
[0022] The prepolymerized modified reaction liquid is placed in an oven, first heated to 100°C, kept warm for half an hour, then heated to 180°C, kept warm for half an hour, then heated to 220°C, kept warm for 1-2 hours, naturally cooled to room temperature, washed three times with acetone, and dried again to obtain modified silicon nitride fiber.
[0023] Preferably, the length of the silicon nitride fiber is 10±2 mm, the diameter of the silicon nitride fiber is 5±1 μm, and the density of the silicon nitride fiber is 2.45 g / cm 3 .
[0024] Preferably, the flame retardant is a nitrogen-based flame retardant, including one of melamine cyanurate (MCA), melamine polyphosphate (MPP), and melamine (MA).
[0025] Preferably, the toughening agent is a silicon-based toughening agent, including one of MR-502, M-577, and M-722.
[0026] Preferably, the lubricant is at least one of ethylene bisstearamide, calcium stearate, zinc stearate and polytetrafluoroethylene wax.
[0027] Preferably, the anti-dripping agent is polytetrafluoroethylene with a molecular weight of 350,000-550,000.
[0028] Preferably, the antioxidant includes one or more combinations of antioxidant 1076, antioxidant 1010, and antioxidant 168.
[0029] Preferably, the method for preparing the automobile safety belt plastic buckle comprises:
[0030] The first step is to weigh the polycarbonate resin, acrylonitrile-styrene-acrylate copolymer, toughening agent, lubricant, anti-drip agent and antioxidant in parts by weight and mix them evenly in a mixer;
[0031] In the second step, the raw materials mixed in the mixer are transferred to a twin-screw extruder, and the modified silicon nitride fiber is gradually added through the feed port. After melting, extrusion and granulation in the extruder, plastic masterbatch is obtained.
[0032] The third step is to injection mold the obtained plastic masterbatch in a mold to obtain a car seat belt plastic buckle.
[0033] Preferably, the mixing speed of the mixer in the first step is 200-500 r / min, and the mixing time is 10-20 min.
[0034] Preferably, the temperatures of the zones of the twin-screw extruder in the second step include: 245-255°C, 255-260°C, 260-270°C, 265-275°C, 260-265°C, 255-265°C, and the screw speed is 300-400r / min.
[0035] Preferably, the temperature of the injection molding in the third step is 275-285°C, the pressure is 70-110 MPa, and the mold temperature is 60-80°C.
[0036] The beneficial effects of the present invention are:
[0037] 1. The present invention prepares a plastic buckle for automobile safety belts, which adopts a composite modified material of polycarbonate and has the advantages of high strength, high toughness, high thermal stability, high wear resistance and the like.
[0038] 2. Among the components of the buckle material used in the present invention, the main material is polycarbonate resin, which has the advantages of high strength, high weather resistance and good high temperature resistance; acrylonitrile-styrene-acrylate copolymer and toughening agent can compositely improve the toughness and processability of the material; modified silicon nitride fiber is silicon nitride fiber that has undergone surface modification treatment, which not only has better compatibility but also can enhance the material performance to a great extent; in addition, flame retardants, lubricants and antioxidants are added to further improve the performance of the material.
[0039] 3. Although ordinary silicon nitride fibers have high strength and good high temperature resistance, they are relatively brittle, and have poor surface activity and poor compatibility with organic matter. This results in the inability to exert its advantages as a material additive, and even affects the performance of the material itself. The present invention prepares a silicon nitride fiber coated with polyhexahydrotriazine by surface modification of silicon nitride fibers, which has very good performance in the material.
[0040] 4. The preparation of modified silicon nitride fiber is to first activate the amino group on its surface, then mix it with 4,4'-(1,4-phenylenedioxy) dianiline, and under the action of formaldehyde, the surface is gradually coated with pre-polymerized hexahydrotriazine, and then cured by heating to obtain polyhexahydrotriazine composite modified silicon nitride fiber. In this process, the surface of silicon nitride fiber is treated with amino, which not only improves the dispersibility, but also allows it to participate in the reaction. The obtained product has better performance than directly immersing silicon nitride fiber in prepolymer and then curing it. DETAILED DESCRIPTION
[0041] The technical solution of the present invention is described below through specific examples. It should be understood that the one or more method steps mentioned in the present invention do not exclude the existence of other method steps before and after the combination step or the insertion of other method steps between these explicitly mentioned steps; it should also be understood that these embodiments are only used to illustrate the present invention and are not used to limit the scope of the present invention. Moreover, unless otherwise specified, the numbering of each method step is only a convenient tool for identifying each method step, and is not intended to limit the order of arrangement of each method step or to limit the scope of the present invention. The change or adjustment of the relative relationship thereof shall also be regarded as the scope of the present invention without substantially changing the technical content.
[0042] In order to better understand the above technical scheme, the exemplary embodiments of the present invention are described in more detail below. Although exemplary embodiments of the present invention are shown, it should be understood that the present invention can be implemented in various forms and should not be limited by the embodiments set forth herein. On the contrary, these embodiments are provided in order to enable a more thorough understanding of the present invention and to enable the scope of the present invention to be fully communicated to those skilled in the art.
[0043] The present invention will be further described below in conjunction with the following examples.
[0044] Example 1
[0045] A high-strength and high-toughness automobile safety belt plastic buckle, the material components of which are calculated by weight and include:
[0046] 65 parts of polycarbonate resin, 18 parts of acrylonitrile-styrene-acrylate copolymer, 8 parts of modified silicon nitride fiber, 5 parts of flame retardant, 4 parts of toughening agent, 2 parts of lubricant, 0.2 parts of anti-dripping agent and 0.8 parts of antioxidant.
[0047] The grade of polycarbonate resin is Chimei PC-6600, with a specific gravity of 1.2g / cm 3 The melt index is 10g / 10min (300℃, 1.2kg). The brand of acrylonitrile-styrene-acrylate copolymer is Chimei PW-978B, with a specific gravity of 1.07g / cm 3 , the melt index is 13g / 10min (220℃, 10kg).
[0048] The flame retardant is melamine cyanurate (MCA). The toughening agent is silicon toughening agent MR-502. The lubricant is ethylene bis stearic acid amide. The anti-drip agent is polytetrafluoroethylene with a molecular weight of 450,000. The antioxidant is antioxidant 1076.
[0049] The preparation method of modified silicon nitride fiber comprises:
[0050] S1. Surface treatment of silicon nitride fiber:
[0051] Weigh silicon nitride fiber and 3-aminopropyltrimethoxysilane and mix them in deionized water, stir them at 75°C for 8 hours, remove the liquid after treatment, wash them three times with water, and dry them in an oven to obtain amino-treated silicon nitride fiber; the length of the silicon nitride fiber is 10±2 mm, the diameter of the silicon nitride fiber is 5±1 μm, and the density of the silicon nitride fiber is 2.45 g / cm 3 , the mass ratio of silicon nitride fiber, 3-aminopropyltrimethoxysilane and deionized water is 1:0.1-0.4:10;
[0052] S2. Synthesis of prepolymerization modification reaction solution:
[0053] Weigh trioxymethylene and dissolve it in N-methylpyrrolidone, then add a small amount of deionized water and mix well, stir at 70-80°C for half an hour to obtain a mixed solution A; the mass ratio of trioxymethylene, deionized water and N-methylpyrrolidone is 0.4:0.2:3;
[0054] The aminated silicon nitride fiber and 4,4'-(1,4-phenylenedioxy) dianiline were mixed in N-methylpyrrolidone and uniformly dispersed by ultrasonication at room temperature to obtain a mixed solution B; the mass ratio of the aminated silicon nitride fiber, 4,4'-(1,4-phenylenedioxy) dianiline and N-methylpyrrolidone was 1:0.3:6;
[0055] The mixed solution B is heated to 60°C, and the mixed solution A is slowly added and the addition is completed within half an hour, and then the mixture is stirred and reacted for half an hour to obtain a prepolymerization modification reaction solution; the mass ratio of the mixed solution A to the mixed solution B is 1:1;
[0056] S3. Synthesis of modified silicon nitride fiber:
[0057] The prepolymerization modification reaction liquid is placed in an oven, first heated to 100°C, kept warm for half an hour, then heated to 180°C, kept warm for half an hour, then heated to 220°C, kept warm for 2 hours, naturally cooled to room temperature, washed three times with acetone, and dried again to obtain modified silicon nitride fiber.
[0058] The preparation method of the automobile safety belt plastic buckle comprises:
[0059] The first step is to weigh the polycarbonate resin, acrylonitrile-styrene-acrylate copolymer, toughening agent, lubricant, anti-dripping agent and antioxidant calculated by weight and mix them evenly in a mixer at a mixing speed of 300 r / min for 15 min.
[0060] In the second step, the mixed raw materials in the mixer are transferred to a twin-screw extruder, and then the modified silicon nitride fiber is gradually added through the feed port, and then melted, extruded, and granulated in the extruder. The temperatures in each zone include: 250°C, 255°C, 260°C, 270°C, 265°C, and 260°C, and the screw speed is 350r / min to obtain plastic masterbatch;
[0061] The third step is to injection mold the obtained plastic masterbatch in a mold at a temperature of 280°C, a pressure of 80MPa, and a mold temperature of 70°C to obtain a plastic buckle for a car seat belt.
[0062] Example 2
[0063] A high-strength and high-toughness automobile safety belt plastic buckle, the material components of which are calculated by weight and include:
[0064] 50 parts of polycarbonate resin, 12 parts of acrylonitrile-styrene-acrylate copolymer, 5 parts of modified silicon nitride fiber, 3 parts of flame retardant, 3 parts of toughening agent, 1 part of lubricant, 0.1 parts of anti-dripping agent and 0.5 parts of antioxidant.
[0065] The grade of polycarbonate resin is Chimei PC-6600, with a specific gravity of 1.2g / cm 3 The melt index is 10g / 10min (300℃, 1.2kg). The brand of acrylonitrile-styrene-acrylate copolymer is Chimei PW-978B, with a specific gravity of 1.07g / cm 3 , the melt index is 13g / 10min (220℃, 10kg).
[0066] The flame retardant is melamine polyphosphate (MPP). The toughening agent is silicon toughening agent M-577. The lubricant is calcium stearate. The anti-dripping agent is polytetrafluoroethylene with a molecular weight of 350,000. The antioxidant is antioxidant 1010.
[0067] The preparation method of modified silicon nitride fiber comprises:
[0068] S1. Surface treatment of silicon nitride fiber:
[0069] Weigh silicon nitride fiber and 3-aminopropyltrimethoxysilane and mix them in deionized water, stir them at 70°C for 6 hours, remove the liquid after treatment, wash them three times with water, and dry them in an oven to obtain amino-treated silicon nitride fiber; the length of the silicon nitride fiber is 10±2 mm, the diameter of the silicon nitride fiber is 5±1 μm, and the density of the silicon nitride fiber is 2.45 g / cm 3 , the mass ratio of silicon nitride fiber, 3-aminopropyltrimethoxysilane and deionized water is 1:0.1:10;
[0070] S2. Synthesis of prepolymerization modification reaction solution:
[0071] Weigh trioxymethylene and dissolve it in N-methylpyrrolidone, then add a small amount of deionized water and mix well, stir at 70°C for half an hour to obtain a mixed solution A; the mass ratio of trioxymethylene, deionized water and N-methylpyrrolidone is 0.3:0.1:2;
[0072] The aminated silicon nitride fiber and 4,4'-(1,4-phenylenedioxy) dianiline were mixed in N-methylpyrrolidone and uniformly dispersed by ultrasonication at room temperature to obtain a mixed solution B; the mass ratio of the aminated silicon nitride fiber, 4,4'-(1,4-phenylenedioxy) dianiline and N-methylpyrrolidone was 1:0.2:4;
[0073] The mixed solution B was heated to 55°C, and the mixed solution A was slowly added, and the addition was completed within half an hour, and then the stirring reaction was continued for half an hour to obtain a prepolymerization modification reaction solution; the mass ratio of the mixed solution A to the mixed solution B was 1:1;
[0074] S3. Synthesis of modified silicon nitride fiber:
[0075] The prepolymerization modified reaction liquid was placed in an oven, first heated to 100°C, kept warm for half an hour, then heated to 180°C, kept warm for half an hour, then heated to 220°C, kept warm for 1 hour, naturally cooled to room temperature, washed three times with acetone, and dried again to obtain modified silicon nitride fiber.
[0076] The preparation method of the automobile safety belt plastic buckle comprises:
[0077] The first step is to weigh the polycarbonate resin, acrylonitrile-styrene-acrylate copolymer, toughening agent, lubricant, anti-dripping agent and antioxidant calculated by weight and mix them evenly in a mixer at a mixing speed of 200 r / min for 10 min.
[0078] In the second step, the mixed raw materials in the mixer are transferred to a twin-screw extruder, and then the modified silicon nitride fiber is gradually added through the feed port, and then melted, extruded, and granulated in the extruder. The temperatures of each zone include: 245°C, 255°C, 260°C, 265°C, 260°C, 255°C, and the screw speed is 300r / min to obtain plastic masterbatch;
[0079] The third step is to injection mold the obtained plastic masterbatch in a mold at a temperature of 275°C, a pressure of 70MPa, and a mold temperature of 60°C to obtain a plastic buckle for a car seat belt.
[0080] Example 3
[0081] A high-strength and high-toughness automobile safety belt plastic buckle, the material components of which are calculated by weight and include:
[0082] 80 parts of polycarbonate resin, 24 parts of acrylonitrile-styrene-acrylate copolymer, 10 parts of modified silicon nitride fiber, 8 parts of flame retardant, 6 parts of toughening agent, 3 parts of lubricant, 0.4 parts of anti-dripping agent and 1 part of antioxidant.
[0083] The grade of polycarbonate resin is Chimei PC-6600, with a specific gravity of 1.2g / cm 3 The melt index is 10g / 10min (300℃, 1.2kg). The brand of acrylonitrile-styrene-acrylate copolymer is Chimei PW-978B, with a specific gravity of 1.07g / cm 3 , the melt index is 13g / 10min (220℃, 10kg).
[0084] The flame retardant is melamine (MA). The toughening agent is silicon toughening agent M-722. The lubricant is polytetrafluoroethylene wax. The anti-drip agent is polytetrafluoroethylene with a molecular weight of 550,000. The antioxidant is antioxidant 168.
[0085] The preparation method of modified silicon nitride fiber comprises:
[0086] S1. Surface treatment of silicon nitride fiber:
[0087] Weigh silicon nitride fiber and 3-aminopropyltrimethoxysilane and mix them in deionized water, stir them at 80°C for 10 hours, remove the liquid after treatment, wash them three times with water, and dry them in an oven to obtain amino-treated silicon nitride fiber; the length of the silicon nitride fiber is 10±2 mm, the diameter of the silicon nitride fiber is 5±1 μm, and the density of the silicon nitride fiber is 2.45 g / cm 3 , the mass ratio of silicon nitride fiber, 3-aminopropyltrimethoxysilane and deionized water is 1:0.4:10;
[0088] S2. Synthesis of prepolymerization modification reaction solution:
[0089] Weigh trioxymethylene and dissolve it in N-methylpyrrolidone, then add a small amount of deionized water and mix well, stir at 80°C for half an hour to obtain a mixed solution A; the mass ratio of trioxymethylene, deionized water and N-methylpyrrolidone is 0.6:0.3:5;
[0090] The aminated silicon nitride fiber and 4,4'-(1,4-phenylenedioxy) dianiline were mixed in N-methylpyrrolidone and uniformly dispersed by ultrasonication at room temperature to obtain a mixed solution B; the mass ratio of the aminated silicon nitride fiber, 4,4'-(1,4-phenylenedioxy) dianiline and N-methylpyrrolidone was 1:0.4:10;
[0091] The mixed solution B is heated to 65°C, and the mixed solution A is slowly added and the addition is completed within half an hour, and then the stirring reaction is continued for half an hour to obtain a prepolymerization modification reaction solution; the mass ratio of the mixed solution A to the mixed solution B is 1:1;
[0092] S3. Synthesis of modified silicon nitride fiber:
[0093] The prepolymerization modification reaction liquid is placed in an oven, first heated to 100°C, kept warm for half an hour, then heated to 180°C, kept warm for half an hour, then heated to 220°C, kept warm for 2 hours, naturally cooled to room temperature, washed three times with acetone, and dried again to obtain modified silicon nitride fiber.
[0094] The preparation method of the automobile safety belt plastic buckle comprises:
[0095] The first step is to weigh the polycarbonate resin, acrylonitrile-styrene-acrylate copolymer, toughening agent, lubricant, anti-dripping agent and antioxidant calculated by weight and mix them evenly in a mixer at a mixing speed of 500 r / min for 20 min.
[0096] In the second step, the mixed raw materials in the mixer are transferred to a twin-screw extruder, and then the modified silicon nitride fiber is gradually added through the feed port, and then melted, extruded, and granulated in the extruder. The temperatures in each zone include: 255°C, 260°C, 270°C, 275°C, 265°C, and 265°C, and the screw speed is 400r / min to obtain plastic masterbatch;
[0097] The third step is to injection mold the obtained plastic masterbatch in a mold at a temperature of 285°C, a pressure of 110MPa, and a mold temperature of 80°C to obtain a plastic buckle for a car seat belt.
[0098] Comparative Example 1
[0099] A plastic buckle for a car seat belt, compared with Example 1, the difference is that the modified silicon nitride fiber is replaced by silicon nitride fiber, the length of the silicon nitride fiber is 10±2 mm, the diameter of the silicon nitride fiber is 5±1 μm, and the density of the silicon nitride fiber is 2.45 g / cm 3 .
[0100] Comparative Example 2
[0101] A plastic buckle for a car safety belt, compared with Example 1, the difference is that the modified silicon nitride fiber is replaced by amino-treated silicon nitride fiber, and the preparation process is the same as that of Example 1.
[0102] Comparative Example 3
[0103] A plastic buckle for a car safety belt, compared with Example 1, the difference is that the preparation process of the modified silicon nitride fiber is different.
[0104] The preparation process of modified silicon nitride fiber includes:
[0105] S1. Synthesis of prepolymerization modification reaction solution:
[0106] Weigh trioxymethylene and dissolve it in N-methylpyrrolidone, then add a small amount of deionized water and mix well, and stir at 70-80°C for half an hour to obtain a mixed solution A; the mass ratio of trioxymethylene, deionized water and N-methylpyrrolidone is 0.4:0.2:3; dissolve 4,4'-(1,4-phenylenedioxy) diphenylamine in N-methylpyrrolidone, and disperse it evenly by ultrasonic at room temperature to obtain a mixed solution B; the mass ratio of 4,4'-(1,4-phenylenedioxy) diphenylamine and N-methylpyrrolidone is 0.3:6;
[0107] The mixed solution B is heated to 60°C, and the mixed solution A is slowly added and the addition is completed within half an hour, and then the mixture is stirred and reacted for half an hour to obtain a prepolymerization modification reaction solution; the mass ratio of the mixed solution A to the mixed solution B is 1:1;
[0108] S2. Synthesis of modified silicon nitride fibers:
[0109] Add silicon nitride fiber to the prepolymerization modification reaction liquid, the mass ratio of silicon nitride fiber to prepolymerization modification reaction liquid is 1:10, mix evenly and place in an oven, first heat to 100°C, keep warm for half an hour, then heat to 180°C, keep warm for half an hour, then heat to 220°C, keep warm for 2 hours, cool naturally to room temperature, wash three times with acetone, and dry again to obtain modified silicon nitride fiber.
[0110] The performance of the automobile seat belt plastic buckle materials prepared in Example 1 and Comparative Examples 1-3 were tested. The tensile strength standard was GB / T1040; the notched impact strength standard was IOS 7391-2; the creep resistance was to age the material at 180°C for 10 minutes, then return to room temperature, and test the strain after 8 hours of treatment at 12MPa through an electromagnetic fatigue test; and the test results are shown in Table 1.
[0111] Table 1 Performance test results of plastic buckle materials
[0112] Example 1 Comparative Example 1 Comparative Example 2 Comparative Example 3 Tensile strength(MPa) 132.2 116.8 121.5 127.6 Heat deformation temperature(℃) 163 141 143 155 Hardness (HRA) 98 86 89 93 <![CDATA[Notched impact strength (kJ / m 2 )]]> 78.5 63.2 67.7 72.3 Creep resistance (%) 0.02 0.29 0.15 0.08
[0113] It can be seen from Table 1 that the tensile strength, heat resistance, hardness, impact strength and creep resistance of Example 1 of the present invention are much higher than those of other comparative examples, indicating that the plastic buckle material prepared in Example 1 of the present invention has the advantages of high strength, high toughness, high thermal stability and high wear resistance.
[0114] In the description of this specification, the description with reference to the terms "one embodiment", "some embodiments", "example", "specific example", or "some examples" etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms should not be understood as necessarily being directed to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described may be combined in any one or more embodiments or examples in a suitable manner. In addition, those skilled in the art may combine and combine different embodiments or examples described in this specification.
[0115] Although the embodiments of the present invention have been shown and described above, it is to be understood that the above embodiments are exemplary and are not to be construed as limitations of the present invention. A person skilled in the art may change, modify, replace and vary the above embodiments within the scope of the present invention.
Claims
1. A high-strength and high-toughness plastic buckle for car seat belts. It is characterized in that The material composition is calculated by weight and includes: 50-80 parts of polycarbonate resin, 12-24 parts of acrylonitrile-styrene-acrylate copolymer, 5-10 parts of modified silicon nitride fiber, 3-8 parts of flame retardant, 3-6 parts of toughening agent, 1-3 parts of lubricant, 0.1-0.4 parts of anti-dripping agent and 0.5-1 parts of antioxidant; The preparation method of the modified silicon nitride fiber comprises: S1, using 3-aminopropyltrimethoxysilane to perform amination treatment on the surface of the silicon nitride fiber; S2, weigh trioxymethylene and dissolve it in N-methylpyrrolidone, then add a small amount of deionized water and mix well, stir at 70-80°C for half an hour to obtain a mixed solution A; blend the amino silicon nitride fiber and 4,4'-(1,4-phenylenedioxy) dianiline in N-methylpyrrolidone, and disperse them uniformly by ultrasonication at room temperature to obtain a mixed solution B; heat the mixed solution B to 55-65°C, slowly add the mixed solution A, and add it all within half an hour, and then continue to stir and react for half an hour to obtain a pre-polymerized modified reaction solution; S3. Place the prepolymerization modified reaction liquid in an oven, first heat it to 100°C, keep it warm for half an hour, then heat it to 180°C, keep it warm for half an hour, then heat it to 220°C, keep it warm for 1-2 hours, cool it naturally to room temperature, wash it three times with acetone, and dry it again to obtain modified silicon nitride fiber.
2. A high-strength and high-toughness automobile safety belt plastic buckle according to claim 1, It is characterized in that The polycarbonate resin is Chimei PC-6600 with a specific gravity of 1.2 g / cm 3 , the melt index is 10 g / 10 min at 300°C and 1.2 kg.
3. A high-strength and high-toughness automobile safety belt plastic buckle according to claim 1, It is characterized in that The acrylonitrile-styrene-acrylate copolymer is branded as Chimei PW-978B, with a specific gravity of 1.07 g / cm 3 The melt index is 13 g / 10 min at 220°C and 10 kg.
4. A high-strength and high-toughness automobile safety belt plastic buckle according to claim 1, It is characterized in that The flame retardant is a nitrogen-based flame retardant, including one of melamine cyanurate, melamine polyphosphate and melamine.
5. A high-strength and high-toughness automobile safety belt plastic buckle according to claim 1, It is characterized in that The toughening agent is a silicon-based toughening agent, including one of MR-502, M-577, and M-722.
6. A high-strength and high-toughness automobile safety belt plastic buckle according to claim 1, It is characterized in that The lubricant is at least one of ethylene bis stearamide, calcium stearate, zinc stearate and polytetrafluoroethylene wax.
7. A high-strength and high-toughness automobile safety belt plastic buckle according to claim 1, It is characterized in that The anti-dripping agent is polytetrafluoroethylene with a molecular weight of 350,000-550,000.
8. A high-strength and high-toughness automobile safety belt plastic buckle according to claim 1, It is characterized in that The antioxidant includes one or more combinations of antioxidant 1076 , antioxidant 1010 , and antioxidant 168 .
9. A high-strength and high-toughness automobile safety belt plastic buckle according to claim 1, It is characterized in that The preparation method of the automobile safety belt plastic buckle comprises: The first step is to weigh the polycarbonate resin, acrylonitrile-styrene-acrylate copolymer, toughening agent, lubricant, anti-drip agent and antioxidant in parts by weight and mix them evenly in a mixer; In the second step, the raw materials mixed in the mixer are transferred to a twin-screw extruder, and the modified silicon nitride fiber is gradually added through the feed port. After melting, extrusion and granulation in the extruder, plastic masterbatch is obtained. The third step is to injection mold the obtained plastic masterbatch in a mold to obtain a car seat belt plastic buckle.