A method for chemical silver plating of Ni-Cr high temperature alloy
By activating the surface of Ni-Cr superalloy and chemically plating it with silver, a dense and uniform silver plating layer is formed, which solves the corrosion problem of Ni-Cr superalloy in harsh environments, extends its service life and reduces the amount of precious metals used.
Patent Information
- Application Number
- CN202311179190.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-09-13
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2043-09-13
AI Technical Summary
Ni-Cr high-temperature alloys suffer from poor service life in high-temperature, high-pressure, supercritical or subcritical corrosive media due to the thin oxide passivation layer, which allows corrosive media to penetrate. Furthermore, the gap between the precious metal liner and the substrate is difficult to precisely fit.
By activating the surface of the Ni-Cr high-temperature alloy to remove the dense oxide passivation layer, electroless silver plating and heat treatment in an argon atmosphere are performed to form a dense and uniform silver plating layer, avoiding the presence of a precious metal lining and enhancing adhesion.
It extends the service life of Ni-Cr high-temperature alloys in harsh environments, reduces the amount of precious metals used, and improves reliability and economic benefits.
Smart Images

Figure CN117448798B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of chemical silver plating, and particularly relates to a method for chemical silver plating of a Ni-Cr high temperature alloy. Background Art
[0002] Ni-Cr high-temperature alloy is a Ni-Cr based solid solution strengthened high-temperature alloy with molybdenum and niobium as the main strengthening elements. It has good tensile and fatigue properties within the temperature range of 980°C, and has excellent processing and welding properties, good corrosion resistance and oxidation resistance. It is widely used in aerospace, petrochemical, marine and nuclear power fields.
[0003] Ni-Cr high-temperature alloys generally have good corrosion resistance under high temperature conditions because they can generate dense passivation protective layers such as chromium oxide on the surface. However, due to the relatively thin passivation layer, in high temperature (650°C), high pressure (200MPa), supercritical ammonia or subcritical ammonia corrosion harsh media, the surface oxides are corroded, the protective properties are lost, and then the substrate is corroded, affecting the service life. At present, the method of setting silver and other precious metal linings inside Ni-Cr high-temperature alloys is usually adopted to resist such harsh environments, but due to reasons such as processing accuracy, it is difficult to precisely match the lining and the high-temperature alloy substrate. Under high temperature, high pressure and supercritical working conditions, the corrosive medium can easily penetrate through the gap to the surface of the substrate, causing corrosion. Summary of the invention
[0004] The purpose of the present application is to provide a method for chemical silver plating of Ni-Cr high temperature alloy, which removes the dense oxide passivation layer on the surface of Ni-Cr high temperature alloy by activating Ni-Cr high temperature alloy, provides a highly active plating interface for subsequent chemical silver plating, and then prepares a silver-plated layer on the activated surface by chemical plating, and finally heat treats the silver-plated layer to obtain a silver-plated layer with uniform surface color, dense surface, and good adhesion to the substrate. The method described in the present invention overcomes the technical difficulties caused by the gap between the precious metal lining and the substrate, prolongs the service life of Ni-Cr high temperature alloy under high temperature, high pressure, supercritical or subcritical corrosive medium, reduces the amount of precious metals, simplifies the processing technology of precious metal products, and improves the reliability of use.
[0005] To achieve the above object, the present invention provides the following technical solutions:
[0006] The method for chemical silver plating of Ni-Cr high temperature alloy comprises the following steps:
[0007] 1) Pretreatment: alkali washing, water washing, acid washing, water washing, activation, and water washing of the alloy;
[0008] The activation step is to immerse the alloy in an activation solution at 40°C for 2-4 hours; the activation solution is composed of 8-12% H2 SO 4 200ml, 8-12% HNO 3 200ml, HF with a mass fraction of 15-30% is mixed and prepared;
[0009] 2) Chemical plating;
[0010] Chemical plating method: equal volumes of plating solution A and plating solution B are mixed evenly to obtain a mixed plating solution, the pre-treated alloy is quickly immersed in the mixed plating solution, plating for 3-10 minutes at room temperature, then taken out, washed with deionized water, dried naturally or heated to remove the deionized water on the surface;
[0011] 3) Heat treatment:
[0012] The alloy is heated at 300-500° C. in an argon atmosphere for 30-90 min.
[0013] The alkali washing in step 1) is: soaking the alloy in an alkali washing solution at a temperature of 80-90° C. for 30-40 minutes;
[0014] The alkaline washing solution is 60-100g of NaOH, 60-80g of Na 2 CO 3 , 15-30g of Na 3 PO 4 , 5-10g of Na 2 SiO 3 , 1-3g of alkylphenol polyoxyethylene ether OP-10 is added into 1L of deionized water and mixed well to prepare the product.
[0015] The OP-10 is alkylphenol polyoxyethylene ether (the same below).
[0016] The pickling in step 1) is as follows: the alloy is immersed in a pickling solution at a temperature of 70-80° C. for 30-40 minutes;
[0017] The pickling solution is 90-120g of 98% H 2 SO 4 , add 90-100g of potassium sodium tartrate to 1L of deionized water and mix well.
[0018] The water washing in step 1) is as follows: the alloy is immersed in deionized water and washed for 3-5 times, each time for 5-10 minutes.
[0019] Step 2) Preparation of the plating solution A: Take 3.0-3.5 g of AgNO 3Dissolve in 50-70ml deionized water, add 100ml of 2-3% NaOH solution, stir and mix evenly to produce brown precipitate, add 15-40ml of 25-28% ammonia water dropwise while stirring until the brown precipitate disappears and the solution becomes clear;
[0020] The preparation process of the plating solution B is as follows: 40-50 g of glucose, 3-5 g of tartaric acid, and 80-120 ml of anhydrous ethanol are respectively added into 1 L of deionized water, and stirred to mix evenly.
[0021] The time for rapidly immersing in the mixed plating solution in step 2) does not exceed 1 minute.
[0022] The heating temperature in step 2) is 105°C.
[0023] Step 3) The heat treatment method further comprises: heating the alloy at 300-500° C. in an air atmosphere for 30-90 minutes.
[0024] The Ni-Cr high temperature alloy includes Inconel 625, Inconel 706, Inconel 718, Incology 925 and other alloys.
[0025] Due to the adoption of the above technical solution, the present invention has the following advantages:
[0026] 1) The present invention completely removes the dense oxide passivation layer on the surface of the Ni-Cr high-temperature alloy through effective activation measures, thereby providing a highly active plating interface for subsequent chemical silver plating.
[0027] 2) The silver-plated layer is heated in an argon atmosphere to make the plating dense, fine in particle size, uniform in color, and have good adhesion to the substrate. There is no need to set a precious metal lining such as silver inside the Ni-Cr high-temperature alloy, which solves the problem of gaps between the precious metal lining and the substrate and difficulty in precise matching. At the same time, the good protective performance of the silver plating can extend the service life of the Ni-Cr high-temperature alloy in high temperature, high pressure, supercritical or subcritical corrosive media, improve the reliability of use, and have high economic benefits. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] Figure 1 This is the microscopic morphology of the silver-plated layer without heat treatment (magnification 10000);
[0029] Figure 2 This is the microscopic morphology of the silver-plated layer after heat treatment at 300°C for 60 minutes in air atmosphere (magnification 10000);
[0030] Figure 3 This is the microscopic morphology of the silver-plated layer after heat treatment at 300°C for 60 minutes in argon atmosphere (magnification 10000). DETAILED DESCRIPTION
[0031] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.
[0032] All reagents described in this example are commercial analytical grade reagents.
[0033] Embodiment 1:
[0034] Inconel 625 high temperature alloy is subjected to chemical silver plating (in this embodiment, no heat treatment is performed after silver plating), and the method is as follows:
[0035] Weigh 60g of NaOH, 60g of Na 2 CO 3 , 15g of Na 3 PO 4 , 5g of Na 2 SiO 3 , 1g of OP-10 was dissolved in 1L of deionized water to prepare an alkaline cleaning solution. At 80°C, the Inconel 625 high-temperature alloy was soaked in the alkaline cleaning solution for 40 minutes for alkaline cleaning. Then, it was soaked and cleaned with deionized water for 5 times, each time for 10 minutes, to complete the water washing.
[0036] Weigh 90g of H 2 SO 4 , 90g of potassium sodium tartrate was dissolved in 1L of deionized water to prepare the pickling solution. At 70℃, the Inconel625 high temperature alloy block was soaked in the pickling solution for 30min for pickling. Then, it was soaked and cleaned with deionized water for 5 times, each time for 10min, to complete the water washing.
[0037] Prepare 10% H 2 SO 4 Solution 200ml; 8% HNO 3 200ml of solution; 200ml of HF solution with a mass fraction of 20%; after mixing evenly, immerse the Inconel625 high-temperature alloy in the activation solution at 40℃ for 4h for activation. Then soak and wash it with deionized water for 5 times, each time for 10min, to complete the water washing.
[0038] 3.5 g of AgNO 3Dissolve in 70ml deionized water, then add 100ml of 3% NaOH solution, stir and mix evenly to produce brown flocculent precipitate; then add ammonia water dropwise while stirring, the ammonia content is 25-28%, the volume is 15-30ml, until the brown precipitate disappears and the solution becomes clear, stop adding ammonia water, and complete the preparation of component A of the plating solution.
[0039] Add 40 g of glucose, 3 g of tartaric acid, and 120 ml of anhydrous ethanol into 1 L of deionized water, stir to dissolve, and mix evenly to complete the preparation of component B of the plating solution.
[0040] After mixing equal volumes of plating solution A component and plating solution B component, quickly immerse the pre-treated Inconel625 high-temperature alloy in the mixed plating solution for no more than 1 minute. The plating is carried out at room temperature for 3 minutes. After the coating is rinsed with deionized water, it is heated and dried at 105°C.
[0041] The surface of the Inconel625 high-temperature alloy treated by the above method has a smooth silver-plated layer, uniform color, and bright silver-white. The adhesion of the silver-plated layer is weak, and its microscopic morphology is as follows: Figure 1 As shown, from Figure 1 It can be seen that there are relatively large particles on the surface of the high temperature alloy.
[0042] Embodiment 2:
[0043] Inconel 625 high temperature alloy is subjected to chemical silver plating (in this embodiment, heat treatment is performed in an air atmosphere after silver plating), and the method is specifically as follows:
[0044] Weigh 70g of NaOH, 70g of Na 2 CO 3 , 20g of Na 3 PO 4 , 10g of Na 2 SiO 3 , 1g of OP-10 was dissolved in 1L of deionized water to prepare an alkaline cleaning solution. At 80°C, the Inconel 625 high-temperature alloy was soaked in the alkaline cleaning solution for 40 minutes for alkaline cleaning. Then, it was soaked and cleaned with deionized water for 5 times, each time for 10 minutes, to complete the water washing.
[0045] Weigh 100g of 98% H 2 SO 4 100g potassium sodium tartrate was dissolved in 1L deionized water to prepare the pickling solution. At 70℃, the Inconel625 high temperature alloy was soaked in the pickling solution for 30min for pickling. Then, it was rinsed with deionized water for 5 times, each time for 10min.
[0046] Prepare 10% H 2 SO 4 Solution 200ml; HNO with a mass fraction of 10% 3 200ml of solution; 200ml of HF solution with a mass fraction of 20%; after mixing evenly, immerse the Inconel625 high-temperature alloy in the activation solution at 40℃ for 4h for activation. Then soak and wash it with deionized water for 5 times, each time for 10min, to complete the water washing.
[0047] 3 g of AgNO 3 Dissolve in 60ml deionized water, then add 100ml of 3% NaOH solution, stir and mix evenly to produce brown flocculent precipitate; then add ammonia water dropwise while stirring, the ammonia content is 25-28%, the volume is 15-30ml, until the brown precipitate disappears and the solution becomes clear, stop adding ammonia water, and complete the preparation of component A of the plating solution.
[0048] Add 40 g of glucose, 3 g of tartaric acid, and 120 ml of anhydrous ethanol into 1 L of deionized water, stir to dissolve, and mix evenly to complete the preparation of component B of the plating solution.
[0049] After mixing the components A and B of the plating solution in equal proportions, quickly immerse the pre-treated Inconel625 high-temperature alloy in the mixed plating solution for no more than 1 minute. The plating is carried out at room temperature for 3 minutes. After the coating is rinsed with deionized water, it is heated and dried at 105°C.
[0050] The silver-plated layer was heat treated at 300°C in air atmosphere for 60 min.
[0051] The silver-plated surface of Inconel625 high-temperature alloy is smooth, uniform in color, silvery white, and has enhanced adhesion. Its microscopic morphology is as follows: Figure 2 As shown, from Figure 2 It can be seen that relatively uniform particles appear on the surface of the coating. Although the particle size is reduced, pores with relatively uniform nanoscale distribution appear.
[0052] Embodiment 3:
[0053] Inconel 625 high temperature alloy is subjected to chemical silver plating (in this embodiment, heat treatment is performed in an argon atmosphere after silver plating), and the method is as follows:
[0054] Weigh 80g of NaOH and 80g of Na 2 CO 3 , 30g of Na 3 PO 4 , 10g of Na 2 SiO 3OP-102g was dissolved in 1L of deionized water to prepare an alkaline cleaning solution. At 80°C, the Inconel 625 high-temperature alloy was soaked in the alkaline cleaning solution for 40 minutes for alkaline cleaning. Then, it was soaked and cleaned with deionized water for 5 times, each time for 10 minutes, to complete the water washing.
[0055] Weigh 120g of 98% H 2 SO 4 , 100g potassium sodium tartrate was dissolved in 1L deionized water to prepare the pickling solution. At 70℃, the Inconel625 high temperature alloy was soaked in the pickling solution for 30min for pickling. Then, it was rinsed with deionized water for 5 times, each time for 10min.
[0056] Prepare 8% H 2 SO 4 Solution 200ml; 8% HNO 3 200ml of solution; 200ml of HF solution with a mass fraction of 25%; mix them evenly to prepare the activation solution, immerse the Inconel625 high-temperature alloy in the activation solution at 40℃ for 4h to activate it. Then soak and wash it with deionized water for 5 times, each time for 10min, to complete the water washing.
[0057] 3.5 g of AgNO 3 Dissolve in 70ml deionized water, then add 100ml of 3% NaOH aqueous solution, stir and mix evenly to produce brown flocculent precipitate; then add ammonia water dropwise while stirring, the ammonia content is 25-28%, the volume is 15-40ml, until the brown precipitate disappears and the solution is clear, stop adding ammonia water, and complete the preparation of component A of the plating solution.
[0058] Add 50g of glucose, 3g of tartaric acid, and 100ml of anhydrous ethanol to 1L of deionized water, stir to dissolve, and mix evenly to complete the preparation of component B of the plating solution.
[0059] After mixing equal volumes of component A and component B of the plating solution, quickly immerse the pre-treated Inconel625 high-temperature alloy in the mixed plating solution for no more than 1 minute. The plating is carried out at room temperature for 5 minutes. After the coating is rinsed with deionized water, it is heated and dried at 105°C.
[0060] The silver-plated layer was heat treated at 300°C in an argon atmosphere for 60 min.
[0061] The surface of the silver-plated layer on the surface of Inconel625 high-temperature alloy is smooth, uniform in color, and bright silver-white. The silver-plated layer adheres well to the substrate. Its microscopic morphology is as follows: Figure 3 As shown, from Figure 3It can be seen that the coating surface is dense, the number of particles is reduced, and the particle size is refined.
[0062] in conclusion:
[0063] The applicant has verified through experiments that the Inconel 625 high-temperature alloy treated by the method of the present invention has active chemical properties on the surface of the activated substrate, and after chemical plating, a silver-plated layer is obtained, the surface of the silver-plated layer is flat, the color is uniform, and it is bright silver-white. Among them, the coating without heat treatment has weak adhesion and obvious particles on the surface; after heat treatment, the adhesion is enhanced and the surface particles are refined. The reason is that the heat treatment process can eliminate the relaxed internal stress in the silver coating, and at the same time, the mutual diffusion and co-penetration between the silver coating and the substrate improves the adhesion strength between the silver coating and the alloy substrate.
[0064] Among them, the heat treatment in air atmosphere and argon atmosphere has the following differences due to the different atmospheres: in the air atmosphere, the silver plating is easily oxidized by oxygen to form relatively evenly distributed nanoscale gas channels, but there are evenly distributed nanoscale pores on the surface of the plating, which weakens its protective performance against the alloy matrix; after heat treatment in an inert gas (argon) atmosphere, the plating has no pores and is dense, and the adhesion strength is improved because no oxidation reaction occurs under the argon inert atmosphere heat treatment conditions, and the surface is no pores and is dense, the number of plating particles is significantly reduced, and the particle size is refined.
[0065] Therefore, chemical silver plating on the surface of Ni-Cr high-temperature alloy forms a dense, uniform silver coating with good adhesion strength after heat treatment at 300°C in argon atmosphere, which solves the problem of difficult precise matching due to the gap between the precious metal lining and the substrate. At the same time, the good protective performance of the silver coating can extend the service life of the alloy in high temperature, high pressure, supercritical or subcritical corrosive media, and reduce the amount of precious metal silver used, thereby improving the reliability and economic benefits of use.
[0066] Inconel 625 high temperature alloy can be replaced by Inconel706, Inconel718, Incology925 and other alloys. The above method can also be used to obtain a silver-plated layer with a smooth surface, uniform color, and bright silver-white alloy, and the silver-plated layer has good adhesion to the substrate.
Claims
1. A method for chemical silver plating of Ni-Cr high temperature alloy, characterized in that: The following steps are involved: 1) Pretreatment: alkali washing, water washing, acid washing, water washing, activation, and water washing of the alloy; The activation is performed by immersing the alloy in an activation solution at a temperature of 40° C. for 2-4 hours; the activation solution is prepared by mixing 200 ml of H2SO4 with a mass fraction of 8-12%, 200 ml of HNO3 with a mass fraction of 8-12%, and 200 ml of HF with a mass fraction of 15-30%; 2) Chemical plating; Chemical plating method: equal volumes of plating solution A and plating solution B are mixed evenly to obtain a mixed plating solution, the pre-treated alloy is quickly immersed in the mixed plating solution, plating for 3-10 minutes at room temperature, then taken out, washed with deionized water, dried naturally or heated to remove the deionized water on the surface; The preparation method of the plating solution A is as follows: 3.0-3.5 g of AgNO3 is dissolved in 50-70 ml of deionized water, 100 ml of a 2-3% NaOH solution is added, and the mixture is stirred to produce a brown precipitate. 15-40 ml of a 25-28% ammonia solution is added dropwise while stirring until the brown precipitate disappears and the solution becomes clear. Preparation process of the plating solution B: Take 40-50g of glucose, 3-5g of tartaric acid, and 80-120ml of anhydrous ethanol, add them into 1L of deionized water, and stir to mix evenly; 3) Heat treatment: The alloy is heated at 300-500° C. in an argon atmosphere for 30-90 min.
2. The method according to claim 1, characterized in that The alkaline washing in step 1) is as follows: soaking the alloy in an alkaline washing solution at a temperature of 80-90° C. for 30-40 minutes; The alkaline washing solution is prepared by adding 60-100g of NaOH, 60-80g of Na2CO3, 15-30g of Na3PO4, 5-10g of Na2SiO3, and 1-3g of OP-10 into 1L of deionized water and mixing well.
3. The method according to claim 1, characterized in that The pickling in step 1) is as follows: the alloy is immersed in a pickling solution at a temperature of 70-80° C. for 30-40 minutes; The pickling solution is prepared by adding 90-120 g of H2SO4 with a mass fraction of 98% and 90-120 g of potassium sodium tartrate to 1 L of deionized water and mixing them evenly.
4. The method according to claim 1, characterized in that: The water washing in step 1) is as follows: the alloy is immersed in deionized water and washed for 3-5 times, each time for 5-10 minutes.
5. The method according to claim 1, characterized in that The time for rapid immersion in the mixed plating solution in step 2) shall not exceed 1 minute.
6. The method according to claim 1, characterized in that Step 3) The heat treatment method further comprises: heating the alloy at 300-500° C. in an air atmosphere for 30-90 minutes.
7. The method according to claim 1, characterized in that The Ni-Cr high temperature alloy includes Inconel 625, Inconel 706, Inconel 718, and Incology 925 alloy.
Citation Information
Patent Citations
Process for producing magnesium alloy surface Ni-Ce-P / nano-TiO2 chemical composite plate
CN101492813A
Process for silver caating on surface of magnesium and magnesium alloy
CN1793424A