Methods for manufacturing membrane rolls and protrusion adjustment systems used in membrane roll manufacturing

By adjusting the number and position of protrusions through localized heating on the membrane surface, the problems of orientation angle variation and roll-shaped failure in the manufacturing of large membrane rolls were solved, achieving membrane roll stability and damage resistance, and making it suitable for wide-width membrane processing.

CN117460611BActive Publication Date: 2026-11-17KONICA MINOLTA INC
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
CN202280040193.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2021-06-09
Filing Date
2022-03-14
Publication Date
2026-11-17
Estimated Expiration
2042-03-14

AI Technical Summary

Technical Problem

Existing technologies struggle to effectively suppress orientation angle variations and avoid roll-shaped defects when manufacturing large membrane rolls, leading to membrane damage and non-uniformity in the width direction.

Method used

The number, position, and height of the protrusions are adjusted by local heating on the membrane surface to ensure they are arranged continuously along the length. The number of protrusions is controlled to be 1 to 10 per 1m, and the height is controlled to be within the range of 0.05 to 0.50μm. An infrared heater is used to configure the heat source in the width and length directions to control the tilt angle of the protrusions, thereby avoiding protrusion overlap and uneven air layer incorporation.

Benefits of technology

It enables the suppression of orientation angle variations during film roll manufacturing, avoids roll-shaped defects, improves the stability and damage resistance of film rolls, and is suitable for wide-width film processing.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117460611B_ABST
    Figure CN117460611B_ABST
Patent Text Reader

Abstract

The present invention addresses the problem of providing a method for manufacturing a film roll suitable for wide-width film processing that prevents roll-up defects and minimizes orientation angle variations, and a protrusion adjustment system used in the manufacturing of the film roll. The manufacturing method is a method for manufacturing a film roll using a solution or melt casting method, characterized by comprising at least: a film forming step, a protrusion adjustment step in the width direction of the film surface, a trimming step at both ends of the film, and a winding step of the film trimmed by the trimming step. The protrusion adjustment step is a step of adjusting the number, height, and position of the protrusions by applying localized heating to the film, thereby ensuring that the number of protrusions is in the range of 1 to 10 per 1m in the width direction, the height of the protrusions is in the range of 0.05 to 0.50 μm, and adjusting the position of the protrusions so that they can move continuously in the length direction of the film surface.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to a method for manufacturing film rolls and a protrusion adjustment system used in the manufacturing of film rolls. More specifically, it relates to a method for manufacturing film rolls suitable for wide-width film processing and a protrusion adjustment system used in the manufacturing of film rolls that prevents roll-shaped defects and minimizes orientation angle variations. Background Technology

[0002] In recent years, as the applications of display devices have expanded, there has been a demand for higher image quality and greater detail. Recently, 4K TVs (TVs with approximately four times the number of pixels of Full HD TVs) have become available on the market.

[0003] In addition, future display devices such as 8K TVs will be needed to enable even higher contrast ratios.

[0004] Furthermore, there is an urgent need for larger display devices, and regarding the film used in such displays, there is also a need to increase the width of the supplied film rolls. There is an urgent need to provide films with less film damage associated with roll failures and smaller changes in the orientation angle in the width direction of the film.

[0005] Regarding the manufacturing method of the membrane roll, Patent Document 1 discloses the following technology: after the membrane is stretched and before trimming, vibration cutting is performed (in the pre-winding process, edge cutting is performed by moving the membrane substrate in the width direction at the substrate edge cutting section).

[0006] However, it is not sufficient to minimize orientation angle variation without causing roll-up faults.

[0007] On the other hand, Patent Document 2 discloses the following technology: In order to improve the above-mentioned defects, by trimming and stretching both ends of a long strip of pre-stretched film under vibration (e.g., periodically moving the device supporting the transported film), and then trimming it again, a roll of stretched film (called a "film roll") is produced that can suppress defects caused by continuous thickness unevenness such as strap and lateral warping, and can minimize orientation angle variation.

[0008] However, in response to the initial requirements, the inventors used the disclosed technology to manufacture large film rolls and found that, according to the disclosed technology, there were residual disturbances in the orientation angle variation, and there was room for improvement.

[0009] Existing technical documents

[0010] Patent documents

[0011] Patent Document 1: Japanese Patent Application Publication No. 2002-255409

[0012] Patent Document 2: Japanese Patent Application Publication No. 2015-123605 Summary of the Invention

[0013] The problem that the invention aims to solve

[0014] The present invention was made in view of the above-mentioned problems and conditions, and its solution is to provide a method for manufacturing film rolls suitable for wide-width film processing that does not cause roll-shaped defects and can suppress small changes in orientation angles, and a protrusion adjustment system used in the manufacturing of film rolls.

[0015] Methods for solving problems

[0016] In order to solve the above-mentioned problems, the inventors studied the causes of the problems and found that: during the manufacturing of the film roll, by locally heating the film, the number, height and position of the protrusions in the width direction of the film surface are adjusted, and the position of the protrusions is adjusted by continuously moving them in the length direction of the film surface, thereby solving the above-mentioned problems and completing the present invention.

[0017] That is, the aforementioned problems involved in this invention are solved by the following means.

[0018] 1. A method for manufacturing a membrane roll, which is a method for manufacturing a membrane roll using a solution or melt casting method, characterized in that it includes at least: a membrane forming step, a protrusion adjustment step in the width direction of the membrane surface, a trimming step at both ends of the membrane, and a winding step of the membrane trimmed by the trimming step, wherein the protrusion adjustment step is a step of adjusting the number, height, and position of the protrusions, and the protrusions are adjusted by applying local heating to the membrane so that the number of protrusions is in the range of 1 to 10 per 1m in the width direction, the height of the protrusions is in the range of 0.05 to 0.50μm, and the position of the protrusions is adjusted by continuously moving them in the length direction of the membrane surface.

[0019] 2. The method for manufacturing a membrane roll according to claim 1, characterized in that, in the trimming step, before trimming the two ends of the membrane, the membrane is not vibrated in the width direction.

[0020] 3. The method for manufacturing a film roll according to claim 1 or 2, characterized in that, in the protrusion adjustment step, the position of the protrusion is adjusted by locally heating the film so that the protrusions are arranged in a generally straight line along the length direction of the film surface, and the absolute value of the inclination angle of the generally straight line with respect to the length direction of the film surface is in the range of 0.01 to 0.6°.

[0021] 4. The method for manufacturing a film roll according to any one of claims 1 to 3, characterized in that the local heating is performed using infrared heaters arranged in both the width and length directions of the film, wherein the heat source portions of the infrared heaters are arranged at intervals of 10 to 100 mm in the width direction of the film, and the heat source portions are arranged at positions different from the width positions in the length direction of the film, and the arranged heat source portions E A and E B The average angle of inclination of the connecting straight lines is in the range of 2 to 45° relative to the length direction.

[0022] 5. The method for manufacturing a film roll according to any one of items 1 to 4, characterized in that the average value B of the heat A at the central portion of the infrared heater and the heat B at the ends of the infrared heater satisfies the following formula (1).

[0023] Equation (1): 0.2 < (B / A) < 0.6.

[0024] 6. The method for manufacturing a film roll according to any one of claims 1 to 5, characterized in that, after the finishing step, the film is not subjected to knurling.

[0025] 7. The method for manufacturing a membrane roll according to any one of claims 1 to 6, characterized in that the maximum height difference (PV) of the average membrane thickness at each width position measured in the order of steps 1 to 3 in a direction inclined relative to the width direction of the membrane is in the range of 0.02 to 0.40 μm.

[0026] Step 1:

[0027] After measuring the film thickness at any position at the end of the membrane, at each measurement, the film thickness is measured at a position moved 10 mm in the width direction and 30 mm in the length direction from the arbitrary position. The width position, length position, and film thickness value are recorded. This process is repeated until the end of another membrane is reached.

[0028] Step 2:

[0029] After step 1 is completed, the same measurements as in step 1 are performed until the total distance of the movement along the length direction reaches 1000m.

[0030] Step 3:

[0031] Based on the large amount of film thickness data obtained from steps 1 and 2, the film thickness values ​​at the same width position are averaged to obtain the average film thickness value at each width position, and the height difference (PV) between the maximum and minimum values ​​is calculated from them.

[0032] 8. A protrusion adjustment system for manufacturing a membrane roll, which is used in manufacturing a membrane roll having a protrusion adjustment process that adjusts the number, height, and position of protrusions in the width direction of the membrane surface, characterized in that it comprises: a membrane thickness acquisition means for obtaining the membrane thickness profile of the membrane midway through or after the protrusion adjustment process; a determination means for determining whether the number of protrusions in the width direction is within an ideal range of 1 to 10 per 1m and whether the height of the protrusions in the width direction is within an ideal range of 0.05 to 0.50 μm, based on the membrane thickness profile data; and a means for locally heating the membrane using an infrared heater so that both the number of protrusions and the height of the protrusions are within the ideal range when either the number of protrusions or the height of the protrusions is outside the ideal range in the determination means.

[0033] Invention Effects

[0034] By employing the above-described means of the present invention, it is possible to provide a method for manufacturing film rolls suitable for wide-width film processing that does not produce roll-shaped defects and can minimize orientation angle variations, as well as a protrusion adjustment system used in the manufacturing of film rolls.

[0035] The mechanism by which the effects of this invention are manifested or function is not yet clear, but speculation is offered as follows.

[0036] The inventors have investigated the techniques disclosed in Patent Documents 1 and 2 above, which involve vibrating the membrane before and after stretching to improve membrane performance.

[0037] According to Patent Document 1, vibration is performed after the film is stretched, i.e., when the orientation angles are consistent, thereby causing the orientation angles to become disordered.

[0038] In Patent Document 2, vibration operation was performed before the film was stretched, i.e. before the orientation angle was aligned, thereby suppressing the disorder of the orientation angle. Even so, the disorder of the orientation angle still remained.

[0039] The so-called vibration operation is a technique that causes the position of the unevenness in the width direction of the film surface to change, for example, to prevent the overlap of the protrusions when forming the roll. The film using this technique has air unevenly drawn into the film roll during winding, and the air slowly detaches over time, causing deformation of the roll, such as chain deformation. This results in creases or damage in the film, which can be problematic when assembled into a display device.

[0040] Therefore, the inventors have solved the problem of this application by controlling the number and height of the protrusions in the width direction of the film surface within a certain range and adjusting the position of the protrusions so that they move continuously in the length direction of the film surface, thereby preventing the overlap of the protrusions of the film during winding. This allows for highly controlled control of the amount of air taken in the film roll. Attached Figure Description

[0041] Figure 1 This is a diagram showing the relationship between the convex portion and the film thickness profile in the width direction.

[0042] Figure 2 A flowchart illustrating the manufacturing process of this invention.

[0043] Figure 3 This is a schematic diagram of an apparatus for manufacturing films using a solution casting method.

[0044] Figure 4A This is a schematic diagram illustrating the continuous arrangement and adjustment of the protrusion in a straight line along its length.

[0045] Figure 4B This is a schematic diagram illustrating the continuous arrangement and adjustment of the protrusion in a straight line along its length.

[0046] Figure 4C This is a schematic diagram illustrating the arrangement and adjustment of the protrusion along a curve in the length direction.

[0047] Figure 5 A diagram that approximates a straight line to represent the position of the convex part.

[0048] Figure 6A This is a diagram showing the infrared heaters arranged in one column along the length of the membrane.

[0049] Figure 6B This is a diagram showing the infrared heaters arranged in two columns along the length of the membrane.

[0050] Figure 6C This is a diagram showing the infrared heaters arranged in 5 columns along the length of the membrane.

[0051] Figure 7A A diagram showing the average inclination of each heat source section relative to the straight line formed by the length direction.

[0052] Figure 7B A diagram showing the average inclination of each heat source section relative to the straight line formed by the length direction.

[0053] Figure 8 This is a cross-sectional view of the tensioning device from above, showing the plane perpendicular to the membrane.

[0054] Figure 9A schematic diagram of the nozzle and heater arrangement in the three zones inside the tensioning device when viewed from the front.

[0055] Figure 10 This is a side view of the three areas inside the tensioning device.

[0056] Figure 11 This is a cross-sectional view of the tensioning device from above, showing the plane perpendicular to the membrane.

[0057] Figure 12 This is a schematic diagram illustrating the process of winding the film and a cross-section of the film roll of the present invention after winding.

[0058] Figure 13 This is a schematic diagram of an apparatus for manufacturing optical films using the melt casting method.

[0059] Figure 14 This is an example of a heatmap used to confirm continuity. Detailed Implementation

[0060] The method for manufacturing a film roll according to the present invention is a method for manufacturing a film roll using a solution or melt casting method, characterized in that it includes at least: a film forming step, a protrusion adjustment step in the width direction of the film surface, a trimming step at both ends of the film, and a winding step of the film trimmed by the trimming step. The protrusion adjustment step is a step of adjusting the number, height, and position of the protrusions. By applying local heating to the film, the number of protrusions is made to be in the range of 1 to 10 per 1m in the width direction, and the height of the protrusions is made to be in the range of 0.05 to 0.50μm. The position of the protrusions is adjusted by continuously moving them in the length direction of the film surface.

[0061] This feature is a common or corresponding technical feature of the following implementation methods (solutions).

[0062] As an embodiment of the present invention, from the viewpoint of the effect of the present invention, it is preferable that, in the trimming process, the membrane is not vibrated in the width direction before trimming the two ends of the membrane.

[0063] From the viewpoint that the protrusions of the film do not overlap during the winding process and do not generate excess air layers, it is more preferable that, in the protrusion adjustment process, the position of the protrusions is adjusted so that they are arranged in a generally straight line along the length direction of the film surface by local heating of the film, and the absolute value of the tilt angle of the generally straight line with respect to the length direction of the film surface is in the range of 0.01 to 0.6°.

[0064] From the viewpoints of film thickness control and stability, and from the viewpoint of ensuring appropriate spacing between heat sources, it is preferable to use infrared heaters arranged in both the width and length directions of the film for the localized heating. In the width direction, the heat sources of the infrared heaters are arranged at intervals of 10 to 100 mm, and in the length direction, these heat sources are arranged at positions different from their width positions. Each of the arranged heat sources E... A and E B The average angle of inclination of the connecting straight lines is in the range of 2 to 45° relative to the length direction.

[0065] From the viewpoint of the effects of the present invention, it is preferable that the average value of the heat A in the central part of the infrared heater and the heat B at the end of the infrared heater satisfies the above formula (1).

[0066] From the viewpoint of suppressing excessive air intake, it is preferable that the membrane is not knurled after the finishing process.

[0067] From the viewpoint of demonstrating the effects of the present invention, it is preferable that the maximum height difference (PV) of the average film thickness at each width position of the film thickness value measured in the order of steps 1 to 3 above in a direction inclined relative to the width direction of the film is within the range of 0.02 to 0.40 μm.

[0068] The protrusion adjustment system used in the manufacturing of the membrane roll of the present invention is a protrusion adjustment system used in the manufacturing of a membrane roll having a protrusion adjustment process for adjusting the number, height, and position of protrusions in the width direction of the membrane surface. It is characterized by having: a membrane thickness acquisition means for obtaining the membrane thickness profile of the membrane midway through or after the protrusion adjustment process; a determination means for determining whether the number of protrusions in the width direction is within an ideal range of 1 to 10 per 1m and whether the height of the protrusions in the width direction is within an ideal range of 0.05 to 0.50 μm, based on the membrane thickness profile data; and a means for locally heating the membrane using an infrared heater so that both the number of protrusions and the height of the protrusions are within the ideal range when either the number of protrusions or the height of the protrusions is outside the ideal range in the determination means.

[0069] Thus, the effects of the present invention become apparent, and it is able to solve the problem.

[0070] The present invention, its constituent elements, and the forms and methods for carrying out the invention will be described in detail below. It should be noted that in this application, "~" is used to mean the lower and upper limits of the numerical values ​​included before and after it.

[0071] [Summary of the method for manufacturing the membrane roll of the present invention]

[0072] The method for manufacturing a film roll according to the present invention is a method for manufacturing a film roll using a solution or melt casting method, characterized in that it includes at least: a film forming step, a protrusion adjustment step in the width direction of the film surface, a trimming step at both ends of the film, and a winding step of the film trimmed by the trimming step. The protrusion adjustment step is a step of adjusting the number, height, and position of the protrusions. By applying local heating to the film, the number of protrusions is in the range of 1 to 10 per 1m in the width direction, and the height of the protrusions is in the range of 0.05 to 0.50μm. The position of the protrusions is adjusted by continuously moving them in the length direction of the film surface.

[0073] In this invention, by employing the above-mentioned means, an air layer can be appropriately incorporated into the film roll during the film winding process, suppressing uneven air intake. Therefore, a small amount of contact is appropriately generated on the entire surface of the film facing each other, preventing defects such as chain-like defects and preventing winding deviation during transport.

[0074] The film preparation method of the present invention is solution casting or melt casting. In particular, solution casting is preferred in order to obtain a uniform surface.

[0075] First, the meanings of the main terms involved in this invention will be explained below.

[0076] <Definitions of terms related to protrusions>

[0077] In this invention, the term "convex portion" refers to the portion of the mountain and valley shape in which the thickness of the optical film is measured and observed by film thickness measurement is higher than the average film thickness, i.e., thicker.

[0078] Details are as follows.

[0079] Regarding the measurement and evaluation of the convexity's condition, after measuring the film thickness at any position at the end of the film, the film thickness is measured at a position 10 mm wide and 30 mm long from that arbitrary position during each measurement. This process is repeated until the end of another film. A Gaussian filter is used to remove noise, resulting in a film thickness profile in the width direction. The condition of the convexity is then measured and evaluated based on this profile (the final number, height, and position of the convexities are measured at the end of the film after the cutting process, as described later).

[0080] To clarify, in this invention, the term "end of the membrane" refers to the area within 15 to 30 mm inside the end of the membrane (roll) in the width direction, and the term "membrane roll" refers to a membrane wound into a roll.

[0081] (Number of protrusions)

[0082] The average film thickness is determined by averaging the measured values ​​of each film thickness in the width direction obtained through the above-described operation. Figure 1 The portion of the film thickness profile shown in the width direction that is thicker than the average film thickness and is continuously longer than 50 mm in the width direction is designated as a protrusion, and the number of such portions is designated as the number of protrusions.

[0083] If there are too many protrusions, the protrusions become sharp and the membrane deforms. If there are too few, stress will be too concentrated on the few protrusions during membrane winding, causing twisting and other problems.

[0084] Therefore, by making the number of the protrusions within the range of 1 to 10 per 1m in the width direction, the effects of the present invention can be expected.

[0085] (Position and height of the protrusion)

[0086] In addition, among the protrusions determined by the above method, the position of the protrusion with the maximum value is set as the position of the protrusion, and the value obtained by subtracting the average film thickness in the width direction from the maximum value of the protrusion is set as the height h of each protrusion.

[0087] If the height of the protrusions is too high, a chain-like structure will form at the foot of the membrane roll after it has been left for a long time. If the height of the protrusions is too low, the membrane thickness dispersion effect will disappear.

[0088] Therefore, by making the height of the protrusion within the range of 0.05 to 0.50 μm, the effects of the present invention can be expected.

[0089] Furthermore, regarding the position of the protrusions, they are adjusted by continuously moving them along the length of the film surface, so that the protrusions do not overlap during film winding, thereby further improving the effect of adjusting the number and height of the protrusions.

[0090] It should be noted that the above film thickness was measured using an online delayed film thickness measuring device RE-200L2T-Rth+ (manufactured by Otsuka Electronics Co., Ltd.).

[0091] 1. A method for manufacturing film rolls using solution casting.

[0092] A flowchart illustrating the manufacturing process of the method for manufacturing the film roll of the present invention is shown below. Figure 2 .

[0093] In the following solution casting method, while referring to... Figure 2 and Figure 3 While explaining.

[0094] The method for manufacturing a film roll using the solution casting method of the present invention includes a film forming step (S1), a protrusion adjustment step (S2), a trimming step (S3), and a winding step (S4).

[0095] (1.1) Membrane formation process (S1)

[0096] (1.1.1) Preparation of adhesive paste

[0097] In the film forming process (S1), firstly, the resin and solvent are stirred in the stirring tank 1a of the stirring device 1 to prepare a slurry that is cast on the support 3 (annular belt).

[0098] Hereinafter, as an embodiment of the present invention, an example will be described in which a cyclic olefin resin (hereinafter also referred to as "COP") is used as a thermoplastic resin to prepare a paste, but the present invention is not limited thereto.

[0099] In a solvent that is primarily a good solvent for cyclic olefin resins (COP), the COP is dissolved in a dissolving vessel while being stirred, and other compounds are stirred as needed, to prepare a paste. Alternatively, a paste is prepared by sometimes mixing solutions of other compounds in the COP solution to serve as the main solvent.

[0100] (Resin concentration)

[0101] Details regarding the types of resins will be discussed later.

[0102] A high concentration of cyclic olefin resin (COP) in the adhesive is preferred as it can reduce the drying load after casting on the support.

[0103] However, if the COP concentration is too high, the filtration load will increase and the accuracy will decrease.

[0104] The preferred concentration, which balances both factors, is in the range of 10 to 35% by mass, and more preferably in the range of 15 to 30% by mass.

[0105] (solvent)

[0106] The solvent used is a mixture of good and bad solvents.

[0107] The solvents used in the adhesive can be used alone or in combination of two or more. In terms of production efficiency, it is preferable to use a mixture of good and bad solvents for cyclic olefin resins (COP). In terms of COP solubility, it is preferable to use more good solvents.

[0108] Regarding the preferred range of the mixing ratio of good solvent and bad solvent, the good solvent is in the range of 70 to 98% by mass, and the bad solvent is in the range of 2 to 30% by mass.

[0109] To clarify, in this invention, the terms "good solvent" and "bad solvent" refer to solvents that dissolve the cyclic olefin resin (COP) used alone, and solvents that swell or do not dissolve alone, respectively.

[0110] Therefore, based on the average degree of substitution of COP, good solvents and bad solvents change.

[0111] There are no particular limitations on the good solvents used in this invention, and examples include organic halides such as dichloromethane, dioxolane, acetone, methyl acetate, and methyl acetoacetate.

[0112] Particularly preferred examples include dichloromethane or methyl acetate.

[0113] Furthermore, there are no particular limitations on the unsuitable solvents used in this invention; for example, methanol, ethanol, n-butanol, cyclohexane, cyclohexanone, etc., are preferred.

[0114] In addition, it is preferable that the adhesive contains 0.01 to 2% by mass of water.

[0115] In addition, regarding the solvent used in the dissolution of cyclic olefin resins (COP), the solvent removed from the membrane during the membrane fabrication process will be recovered and reused.

[0116] The recycled solvent sometimes contains trace amounts of additives added to COP, such as plasticizers, UV absorbers, polymers, monomer components, etc. Even if these are present, it can be preferably reused, and can also be refined and reused as needed.

[0117] As described above, the method for dissolving COP during the preparation of the adhesive can be achieved using a general method.

[0118] Specifically, preferred methods include those performed at atmospheric pressure, those performed below the boiling point of the main solvent, and those performed under pressure above the boiling point of the main solvent. If heating and pressure are combined, it is possible to heat to above the boiling point at atmospheric pressure.

[0119] Furthermore, a method of heating and stirring to dissolve the solvent at a temperature above its boiling point under normal pressure and within a range where the solvent does not boil under pressure is preferred to prevent the formation of gels, or lumpy undissolved substances called lumps.

[0120] Alternatively, the following method is also preferred: mixing cycloolefin resin (COP) with a poor solvent, wetting or swelling it, and then adding a good solvent and dissolving it.

[0121] Pressurization can be achieved by injecting inactive gases such as nitrogen, or by heating the solvent to increase its vapor pressure.

[0122] Heating is preferably performed externally, such as in jacketed heating systems where temperature control is easier.

[0123] From the perspective of the solubility of cyclic olefin resins (COP), it is preferable to add solvent at a higher heating temperature. If the heating temperature is too high, the required pressure will increase and the productivity will decrease.

[0124] The preferred heating temperature is in the range of 30 to 120°C, more preferably in the range of 60 to 110°C, and even more preferably in the range of 70 to 105°C.

[0125] Additionally, adjust the pressure so that the solvent does not boil at the set temperature.

[0126] Alternatively, a cooling dissolution method is preferred, which allows cyclic olefin resins (COPs) to be dissolved in solvents such as methyl acetate.

[0127] (filter)

[0128] Secondly, it is preferable to use appropriate filter materials such as filter paper to filter the cyclic olefin resin (COP) solution (in dissolution or after dissolution).

[0129] As a filter material, a small absolute filtration precision is preferred in order to remove insoluble substances, but if the absolute filtration precision is too small, the filter material is prone to clogging.

[0130] Therefore, filter media with an absolute filtration accuracy of less than 0.008 mm are preferred, filter media in the range of 0.001 to 0.008 mm are more preferred, and filter media in the range of 0.003 to 0.006 mm are even more preferred.

[0131] There are no special restrictions on the material of the filter media. Common filter media can be used, and filter media made of plastics such as polypropylene and Teflon (registered trademark) or metals such as stainless steel are preferred due to their non-fiber shedding properties.

[0132] It is preferable to remove or reduce impurities, especially bright spots, contained in the cyclic olefin resin (COP) of the raw material through filtration.

[0133] A bright spot or foreign object refers to a point (foreign object) visible when light is shone from one side of a polarizer and observed from the other side, caused by light leakage from the opposite side when two polarizers are arranged in an orthogonal Nicol configuration with a film or similar material placed between them. Preferably, the number of bright spots with a diameter of 0.01 mm or more is 200 per cm. 2 the following.

[0134] More preferably 100 pieces / cm 2 The following is a further preferred option: 50 units / m 2 The following is more preferred: 0 to 10 per cm. 2the following.

[0135] In addition, there are fewer bright spots smaller than 0.01mm.

[0136] The filtration of the adhesive can be carried out using conventional methods. However, the method of filtration while heating is preferred because it is above the boiling point of the solvent at normal pressure and within the range where the solvent does not boil under pressure. This method results in a small increase in the pressure difference (called pressure differential) before and after filtration.

[0137] The preferred temperature range is 30–120°C, more preferably 45–70°C, and even more preferably 45–55°C.

[0138] The preferred filter pressure is low.

[0139] Specifically, it is preferably 1.6 MPa or less, more preferably 1.2 MPa or less, and even more preferably 1.0 MPa or less.

[0140] (1.1.2) Spreading of adhesive

[0141] Regarding the adhesive paste being cast on the support body 3, it is transported to the casting die 2 via a conduit using a pressurized quantitative gear pump or the like, and the adhesive paste is cast from the casting die 2 to the casting position on the support body 3, which is made of a rotating stainless steel annular belt that is continuously moved.

[0142] At this time, the tilt angle of the casting die 2, that is, the discharge direction of the adhesive from the casting die 2 to the support body 3, can be appropriately set so that the angle relative to the normal of the surface of the support body 3 (the surface on which the adhesive is cast) is within the range of 0 to 90°.

[0143] At this point, the support 3 is heated to evaporate the solvent until the cast film 5 can be peeled off from the support 3 using a peeling roller (also called a "roller") 4.

[0144] Furthermore, the cast film 5 is cured to become a peelable cast film, which is simply referred to as "film".

[0145] (Solvent evaporation method)

[0146] The evaporation described above is preferably carried out in an atmosphere within the range of 5 to 75°C.

[0147] When the solvent evaporates, there are methods such as spraying warm air onto the surface of the cast film and / or using liquid heat transfer from the back of the support 3, and using radiant heat to transfer heat from the back of the surface, etc. The method of using radiant heat to transfer heat from the back of the surface has good drying efficiency and is preferred.

[0148] Alternatively, it is preferable to use a method that combines them.

[0149] (Width of the flow)

[0150] From a productivity point of view, the width of the casting is preferably 1.3m or more.

[0151] More preferably, it is in the range of 1.3 to 4.0 m.

[0152] If the width of the cast tape does not exceed 4.0m, no streaks will be generated during the manufacturing process, and the stability in the subsequent handling process will be increased.

[0153] From the perspective of transportability and productivity, a range of 1.3 to 3.0 m is preferred.

[0154] (Support body)

[0155] The support 3 in the casting of the adhesive is preferably a support with a mirror-finished surface, and is held by a pair of rollers 3a and 3b and a plurality of rollers located between them.

[0156] A drive device is provided on one or both of rollers 3a and 3b to apply tension to the support body 3, thereby using the support body 3 in a tensioned state.

[0157] As the support body 3, it is preferable to use a stainless steel strip or a drum whose surface has been plated and finished using castings.

[0158] The surface temperature of the support 3 in the casting of the adhesive is in the range of -50°C to the boiling point of the solvent. A higher temperature can accelerate the drying speed of the cast film, so it is preferred.

[0159] The preferred support temperature is within the range of 0 to 55°C, and more preferably within the range of 22 to 50°C.

[0160] There are no particular restrictions on the method of controlling the temperature of the support body 3, such as spraying warm or cold air or making warm water come into contact with the back side of the support body.

[0161] When using warm water, heat transfer is efficient, so the time until the support reaches a certain temperature is short, which is preferable.

[0162] When using warm air, sometimes the air temperature is higher than the target temperature.

[0163] <Methods for controlling film thickness in the film formation process>

[0164] In the method for manufacturing the membrane roll of the present invention, from the viewpoint of demonstrating the effects of the present invention, it is preferable that the maximum height difference (PV) of the average membrane thickness at each width position of the membrane thickness value measured in the order of steps 1 to 3 below in a direction inclined relative to the width direction of the membrane is within the range of 0.02 to 0.40 μm.

[0165] Step 1:

[0166] After measuring the film thickness at any position at the end of the membrane, the film thickness is measured at a position 10 mm away in the width direction and 30 mm away in the length direction from the arbitrary position during each measurement. The width position, length position, and film thickness value are recorded, and this process is repeated until the end of another membrane is reached.

[0167] Step 2:

[0168] After step 1 is completed, the same measurement as in step 1 is performed until the total distance of the movement in the length direction reaches 1000m.

[0169] Step 3:

[0170] The film thickness data obtained from steps 1 and 2 are averaged at the same width position to calculate the length-average film thickness value at each width position. The height difference (PV) between the largest and smallest values ​​is then calculated.

[0171] In order to adjust the maximum height difference (PV) of the average film thickness at each width position of the film thickness value measured in the order of steps 1 to 3 in a direction inclined relative to the width direction of the film involved in the present invention to be the desired value, the following three film thickness control means can be listed as examples in the film forming process.

[0172] In addition, during the protrusion adjustment process, adjustments can be made to make the maximum height difference (PV) of the average film thickness over the length reach the desired value, which will be described later in the protrusion adjustment process.

[0173] Alternatively, they can be combined.

[0174] (Film thickness control method 1: Pump pulsation spacing control)

[0175] The film thickness is controlled by adjusting the spacing of the pump pulsations.

[0176] It is known that a high-precision gear pump is used in the delivery of resin (extrusion of resin in the case of molten resin) in the piping up to the casting die head. The gear pump can control the pump rotation speed according to its gear ratio, thereby controlling the spacing of the pump pulsation. The pulsation of the pump during delivery has a large impact on the film thickness in the length direction and the average maximum height difference (PV) of the length-average film thickness.

[0177] Here, we would like to provide further explanation regarding the pump's liquid delivery capacity.

[0178] In the casting of adhesive, if the length of the piping from the pump to the casting die is not too short, it will not be affected by the pump's rotation speed, and the pulsation will not increase. If it is not too long, the pressure loss will not increase excessively, thus preventing the pump's delivery capacity from exceeding the lower limit and decreasing.

[0179] In addition, if the pump's rotation speed is not too slow, it can prevent a decrease in the liquid delivery capacity; if it is not too fast, the pressure loss will not increase excessively, thus preventing a decrease in the liquid delivery capacity.

[0180] Based on the above viewpoint, it is preferable to adjust the gear ratio of the gear pump used for resin delivery (resin extrusion in the case of molten resin) within the range of 50 to 100 m in the length of the piping from the pump to the casting die, so that the pump rotation speed is within the range of 10 to 50 rpm.

[0181] (Film thickness control method 2: film thickness control using hot bolts)

[0182] The initial discharge film thickness is controlled by using hot bolts on the casting die.

[0183] In order to improve the uniformity of film thickness in the casting of adhesive, those skilled in the art can cite methods for controlling the slit gap of the die lip portion of the casting die in both solution casting and melt casting methods.

[0184] For example, the following method is used: when extruding a high-viscosity adhesive (including melt), a deviation in the width of the aforementioned slit gap occurs. To prevent this deviation, multiple hot bolts are installed to control the slit gap by the width.

[0185] However, this method has the problem of a physical limit to the number of hot bolts.

[0186] In addition, in order to suppress the pressure variation in width that causes the aforementioned slit gap width deviation, there is a method to change the internal structure of the casting die in width. However, the casting die must be replaced for each product, which involves time and cost.

[0187] The casting die head is equipped with a mechanism that adjusts the width of the slit that discharges the resin (extrusion of the resin in the molten state).

[0188] Here, we would like to provide supplementary explanations regarding the method of controlling the initial discharge film thickness of the cast film by adjusting the gap of the slit through the hot bolt adjustment of the casting die.

[0189] In the casting of adhesive paste, the use of a hot bolt on the casting die head, if the gap in the width of the slit that discharges the adhesive paste is not too small, makes the preparation relatively easy and time-saving.

[0190] In addition, if the gap in the width of the slit for discharging the adhesive is too large, the initial discharge film thickness of the cast film cannot be flattened.

[0191] Based on the above viewpoints, it is preferable to use the hot bolts of the casting die head in the casting process described later to adjust the gap of the slit width of the adhesive discharge to a range of 1.0 to 5.0% relative to the overall casting film thickness after discharge, so as to control the initial discharge film thickness of the casting film.

[0192] Here, the part of the slit from which the slurry comes out of the casting die is called the die lip. A casting die that can adjust the shape of the slit in the die lip and makes it easy to make the film thickness uniform is preferred.

[0193] Among casting molds, hanger-type molds and T-type molds are preferred.

[0194] It should be noted that in this invention, the term "cast film" refers to the adhesive film cast from the aforementioned die lip portion.

[0195] In order to increase the film-making speed of the film involved in this invention, two or more of the above-mentioned casting dies can be set on the support body to divide and stack the adhesive paste.

[0196] Alternatively, a co-casting method in which multiple adhesive pastes are cast simultaneously is preferred to obtain a laminated film roll.

[0197] The slit is narrowed by manually turning a hot bolt to press it in, thus thinning the film, or conversely, it is opened to thicken the film.

[0198] The method of pressing in a hot bolt by applying voltage is also common, but it is usually used in combination.

[0199] Alternatively, a push-pull method can also be used.

[0200] However, the bolt spacing cannot always be narrowed in the casting die mechanism. In the case of high viscosity slurry (including molten slurry), the die lip when the casting die is discharged may sometimes experience a deviation in film thickness in the width direction, such as high pressure load, a sharp drop in load after discharge, and increased film thickness (balance effect).

[0201] Therefore, based on the internal structure of the casting die, it becomes necessary to design the die lip of the casting die to avoid excessive load.

[0202] (Film thickness control method 3: film thickness control using hot air)

[0203] By spraying hot air onto the cast film, the heat is used to flatten the protrusions, thereby controlling the film thickness.

[0204] During the casting of the adhesive, hot air can be sprayed on the surface of the cast film on the reverse side of the tape while the film is still forming, or hot air can be sprayed immediately after the cast film is peeled off from the tape.

[0205] At this point, the interior of the cast film is softened due to the presence of solvent, and the protrusions are flattened. Therefore, by measuring the non-uniformity in the width direction of the cast film online, the temperature, speed, or volume of the drying air can be adjusted, and the amount of residual solvent can be adjusted, thereby controlling the film thickness.

[0206] Here, we provide supplementary information regarding the temperature, wind speed or volume of the drying air, and the amount of residual solvent.

[0207] As long as the temperature of the drying air is not too low, the wind speed is not too low, or the air volume is not too small, the film thickness can be properly controlled.

[0208] In addition, as long as the temperature is not too high, the wind speed is too high, or the air volume is too large, the film thickness will not be locally out of control.

[0209] If the amount of residual solvent is not too small, the film will not become less flexible and unable to flatten, which is closer to the state of a cast film than a cast film.

[0210] In addition, if the amount is not excessive, there will be no deviation in film thickness during planarization.

[0211] Therefore, by making it an appropriate amount of residual solvent, planarization can be performed while a thin film is formed on the surface.

[0212] Based on the above viewpoints, the temperature of the drying air is preferably in the range of 10 to 80°C, and the wind speed is preferably in the range of 5 to 40 m / s.

[0213] In addition, the residual solvent content is preferably 150 to 550% by mass.

[0214] Furthermore, if the above operation is performed on the surface of the cast film before the film has been formed on the reverse side, streaks will form and the interior will be dry, which is not preferable.

[0215] During the casting process of the adhesive, the non-uniformity of the film thickness deviation in the width direction of the cast film is measured online. To reduce this non-uniformity, hot air is sprayed and the film thickness is controlled by adjusting the temperature.

[0216] (1.1.3) Membrane peeling

[0217] The solvent is evaporated on the support 3 until the cast film 5 becomes a peelable film strength. After it is dried and cured or cooled and solidified, the film is peeled off from the support 3 in a self-supporting state using a peeling roller 4 before the film wraps around the support 3 once.

[0218] To clarify, the cast film 5, after being cured into a peelable cast film, is referred to simply as "film".

[0219] At this point, from the viewpoints of surface quality, moisture permeability, and peelability, it is preferable to peel the membrane from the support within the range of 30 to 600 seconds.

[0220] To clarify, the position where the film is peeled off from the support is called the peeling point, and the roller that assists in peeling is called the peeling roller.

[0221] The temperature at the peeling location on the support is preferably set in the range of -50 to 40°C, more preferably in the range of 10 to 40°C, and most preferably in the range of 15 to 30°C.

[0222] (Residual solvent amount during membrane peeling)

[0223] The amount of residual solvent on the film on the support 3 during peeling is appropriately adjusted by the strength of the drying conditions, the length of the support 3, etc.

[0224] It also depends on the thickness of the membrane. If there is too much residual solvent at the peeling point, the membrane may become too soft and difficult to peel, sometimes damaging the planarity, or becoming prone to lateral warping, uneven surface, and longitudinal stripes caused by peeling tension.

[0225] Conversely, if the amount of residual solvent is too small, sometimes part of the membrane peels off midway through the process.

[0226] To ensure good membrane planarity, a residual solvent content of 10–50% by mass is preferred from the perspective of balancing economy, speed, and quality.

[0227] As a method to increase film formation speed (by peeling off when there is as much residual solvent as possible, thus increasing film formation speed), there is the gel casting method (gel casting) which can peel off even when there is a large amount of residual solvent.

[0228] As examples of this method, there are methods such as adding a solvent that is unfavorable to cyclic olefin resins (COP) to the adhesive paste and gelling the cast film after the adhesive paste is cast; and methods such as cooling the support to gelle the cast film and peeling it off in a state containing a large amount of residual solvent.

[0229] Alternatively, there is a method of adding metal salts to the adhesive.

[0230] As described above, gelling the cast film on the support strengthens the film, thereby accelerating peeling and increasing the film production speed.

[0231] It should be noted that the amount of residual solvent is defined by the following formula.

[0232] Residual solvent content (mass%) = {(MN) / N} × 100

[0233] To clarify, M represents the mass of the sample taken at any time during or after the manufacture of the cast film or film, and N represents the mass of the sample of mass M after heating at 115°C for 1 hour.

[0234] (peel tension)

[0235] The peeling tension when separating the support and the membrane is preferably below 300 N / m.

[0236] More preferably, the range is 196 to 245 N / m. In cases where wrinkles are easily generated during peeling, a tension peeling of 190 N / m or less is preferred.

[0237] (1.1.4) Shrinkage within the membrane surface

[0238] The membrane is stretched and thus contracted by applying tension in the transport direction (Machine Direction, hereinafter also referred to as "MD direction") to the membrane after it has been peeled from the support.

[0239] In this case, the membrane contracts in the width direction (Traverse Direction, hereinafter also referred to as the "TD direction") orthogonal to the MD direction within the membrane surface.

[0240] Through the above operations, entanglement between polymer molecules (matrix molecules) in the thickness direction of the film is promoted. During the fabrication of the polarizer, even when the film is bonded through the polarizer layer and the adhesive, the adhesive can easily penetrate into the interior of the film through the entangled portion (cross-linked portion) between the matrix molecules.

[0241] As a result, the membrane can be firmly fixed to the polarizer layer via adhesive, which can improve the peel strength of the membrane to the polarizer layer.

[0242] That is, it can ensure good adhesion between the membrane and the polarizer layer.

[0243] In addition to the above, methods for shrinking the membrane include, for example, subjecting the membrane to high-temperature treatment without maintaining its width to increase the membrane density; and methods for drastically reducing the amount of residual solvent in the membrane.

[0244] (Membrane shrinkage rate)

[0245] In this invention, the shrinkage rate is defined by the following formula.

[0246] Formula: Shrinkage rate [%] = Width of the film after shrinkage [mm] / Width of the film at the start of shrinkage [mm] × 100

[0247] If the membrane shrinkage rate is too small, the effect of promoting entanglement between matrix molecules becomes insufficient; if it is too large, there is a concern that the membrane's production efficiency will decrease.

[0248] Therefore, the shrinkage rate of the membrane is preferably in the range of 1 to 40%, and more preferably in the range of 5 to 20%.

[0249] (Methods for determining and calculating shrinkage rate)

[0250] In this invention, the width of the membrane is measured using an LS-9000 manufactured by KEYENCE Corporation.

[0251] To clarify, the shrinkage rate of the membrane involved in this invention is obtained by substituting the average value of the membrane width measured at 1 second for 5 minutes (300 seconds) using the measuring instrument described above into the above formula. It is not necessarily limited to the above method. For example, the width of the membrane can also be read from a scale and substituted into the above formula.

[0252] (1.1.5) Drying of the membrane

[0253] The membrane is heated on the support using drying device 6 to evaporate the solvent, thereby further drying the membrane.

[0254] The temperature of the support structure can be uniform or vary depending on its location.

[0255] In membrane drying, roller drying (a method in which the membrane is alternately passed through multiple rollers arranged above and below to dry it) and stretching method are generally used to dry the membrane while it is being transported.

[0256] In the above-mentioned stretching method, when using a stretching device, it is preferable to use a device that allows independent control of the film holding length (the distance from the start of holding to the end of holding) by the left and right holding means of the stretching device.

[0257] In the above Figure 3 In the drying device 6, multiple transport rollers arranged in a serrated pattern when viewed from the side are used to transport the film and dry it in between.

[0258] There are no particular restrictions on the drying method in the drying device 6. Generally, hot air, infrared rays, heating rollers, microwaves, etc. are used to dry the film. From the perspective of simplicity, the method of drying the film with hot air is preferred.

[0259] Alternatively, combining them is also preferred.

[0260] Furthermore, the above operations can be performed as needed.

[0261] If the membrane is thin, it dries quickly, but excessively rapid drying can damage the planarity of the finished membrane.

[0262] (Residual solvent content during membrane drying)

[0263] When using high temperature for drying, the amount of residual solvent must be considered. By ensuring that the amount of residual solvent is not excessive, problems caused by solvent foaming can be prevented.

[0264] Regarding the residual solvent content mentioned above, it is advisable to keep it below 30% by mass, and the overall drying should be carried out in the range of approximately 30 to 250°C.

[0265] It is particularly preferred to dry the product in the range of 35 to 200°C, and the drying temperature is preferably increased in stages.

[0266] Furthermore, the amount of residual solvent on the support 3 during membrane peeling is appropriately adjusted by the strength of the drying conditions, the length of the support 3, etc. Regarding the shrinkage within the membrane surface and the amount of residual solvent during membrane drying, the membrane thickness, resin, etc. have a significant impact, and therefore there is a range that overlaps with the preferred range of residual solvent amount.

[0267] (1.2) Convex adjustment process (S2)

[0268] (1.2.1) Overview of the convex part adjustment process

[0269] The manufacturing method of the present invention involves a process for adjusting the number, height, and position of the protrusions on the membrane surface in the width direction. The process is characterized by adjusting the number, height, and position of the protrusions by applying local heating to the membrane, thereby making the number of the protrusions range from 1 to 10 per 1m in the width direction, and the height of the protrusions range from 0.05 to 0.50μm, and adjusting the position of the protrusions so that they can move continuously in the length direction of the membrane surface.

[0270] In this invention, the membrane is locally heated as a means of adjusting the protrusion.

[0271] Examples of localized heating methods include infrared (IR) heaters and hot air. There are no particular limitations on heat treatment, and other methods can also be used for heat treatment.

[0272] Hot air film has the advantage of providing ample film thickness adjustment capability regardless of the material.

[0273] On the other hand, continuous movement control of the valley is slightly more difficult, but by properly controlling the temperature, air volume, nozzle pressure, etc., the convex part can be made to move continuously.

[0274] In this invention, from the viewpoint of film thickness control and stability, it is preferable to use an infrared heater arranged in the width and length directions of the film for the local heating.

[0275] In the convex part adjustment process, the membrane is stretched while being locally heated inside the stretching device.

[0276] In addition, at this time, the online delay film thickness measuring device RE-200L2T-Rth+ film thickness (manufactured by Otsuka Electronics Co., Ltd.) is used to measure the film thickness profile in the width direction of the target film. The difference between the film thickness profile and the target film thickness profile is used to calculate the set temperature of each infrared heater on the computer. The set temperature of each heat source is output via PLC KV-8000 (manufactured by KEYENCE Co., Ltd.). The protrusion is adjusted, and the film thickness is automatically and repeatedly adjusted automatically.

[0277] (1.2.2) Membrane stretching

[0278] Regarding membrane stretching, the membrane can be stretched only in the MD direction within the membrane surface, or only in the TD direction, or both the MD and TD directions, or it can be stretched in an inclined direction.

[0279] Furthermore, there is no limitation on the stretching direction, but from the viewpoint of obtaining a wide film, it is preferable to stretch at least in the width direction.

[0280] As a stretching method at this time, in order to improve the performance, productivity, flatness and dimensional stability of the film, it is preferable to set the circumferential speed difference of the roller to stretch in the transport direction (the length direction of the film; the film forming direction; the casting direction; the MD direction); and to use a clamp or the like to fix the two sides of the film F to stretch in the width direction (the orthogonal direction in the film surface; the TD direction).

[0281] Furthermore, in the case of the so-called stretching method, if the clamping part is driven in a linear drive manner, smooth stretching can be performed, which can reduce the risk of breakage, etc., and is therefore preferred.

[0282] The width maintenance or lateral stretching in the film-making process is preferably performed using a tenter frame stretching device, which can be a needle plate tenter frame or a clamp tenter frame.

[0283] Furthermore, in addition to stretching, drying can be carried out inside the tensioning device 7.

[0284] (Stretch ratio)

[0285] To ensure a high phase difference, a wide width, and to promote adhesive penetration during bonding with the polarizer layer, it is preferable to stretch the film at a high ratio during the stretching process.

[0286] However, if the stretching ratio is too high, sometimes cracks may be generated in the membrane due to tensile stress, or the entanglement between matrix molecules that maintain the membrane strength may disintegrate, making the membrane fragile.

[0287] Therefore, the stretching ratio of the membrane is preferably in the range of 1.1 to 5.0 times, and more preferably in the range of 1.3 to 3.0 times.

[0288] Furthermore, in the case of multiple stretching operations, it is preferable to perform the stretching at the highest ratio, which carries the highest risk of dissociation of matrix molecules in the multiple stretching operations, in the final stretch.

[0289] (Residual solvent content during membrane stretching)

[0290] The amount of residual solvent in the film during stretching is preferably less than 20% by mass, and more preferably less than 15% by mass.

[0291] (1.2.3) Definitions of terms used in the convex part adjustment process

[0292] (Definitions of terms related to protrusions)

[0293] Definitions of terms related to convex parts have already been described above and are therefore omitted.

[0294] (Continuity of the convex part in the length direction: adjustment of the position of the convex part in the length direction)

[0295] Regarding the position of the protrusion adjusted in the protrusion adjustment process of the present invention, the adjustment is carried out in a manner that the protrusion moves continuously along the length direction of the film surface. The position of the protrusion is determined according to the definition described later. If the positions of the protrusions are connected to each other, then, for example, as shown in the figure... Figure 4A and Figure 4B The trajectory is roughly a straight line, as shown. Or, draw a line like... Figure 4C The trajectory shown is a curve with curvature that changes at approximately a certain rate of change.

[0296] Furthermore, Figure 4A , Figure 4B and Figure 4C In order to make the present invention easier to understand, the scale width in the width and length directions is changed for convenience.

[0297] Therefore, the description of "continuous movement along the length of the membrane surface" in this invention, as stated above, means that when connecting the positions of the protrusions to each other, a trajectory is drawn that is either a generally straight line or a curve with curvature changing at a generally constant rate of change. Furthermore, this generally straight line or the curve with curvature changing at a generally constant rate of change may be periodic.

[0298] Furthermore, regarding Figure 4A , Figure 4B and Figure 4C It is a connection of periodic convex parts, but it is not limited to being periodic.

[0299] The term "roughly straight line" refers to... Figure 5As shown, the width direction of the membrane is set as the horizontal axis (x-axis) and the length direction of the membrane is set as the vertical axis (y-axis). When drawing the center point of each convex part, due to the control conditions of the convex part adjustment process and the fluctuation of the membrane properties, it is also included in the strictly defined points that escape from the straight line. It refers to the line that can be basically regarded as a straight line.

[0300] Furthermore, when the approximate straight line is used as the approximate straight line obtained by the least squares method, the absolute value of the correlation coefficient of the linear expression representing the approximate straight line is preferably 0.8 or higher.

[0301] In addition, "a roughly constant rate of change" refers to the rate of change within a range of ±10% of the average value.

[0302] (The angle of inclination θ′ relative to the approximate straight line along the length of the membrane surface)

[0303] In the protrusion adjustment process of the present invention, from the viewpoint of the effect of the present invention, it is preferable to adjust the position of the protrusion by locally heating the membrane so that the protrusions are arranged in a substantially straight line along the length direction on the membrane surface.

[0304] By controlling the protrusions as described above, the film thickness profile does not change drastically in the longitudinal direction of the film. By maintaining the continuity of the protrusions, the effectiveness of the present invention is further improved.

[0305] Furthermore, from the viewpoint of demonstrating the effects of the present invention, it is preferable that the absolute value of the inclination angle of the generally straight line is within the range of 0.01 to 0.6°.

[0306] The tilt angle θ′ of the approximate straight line relative to the length direction of the membrane surface involved in this invention is confirmed as described below.

[0307] like Figure 5 As shown, the position of the protrusion is calculated based on the film thickness profile and average film thickness measured using the online delay film thickness measuring device RE-200L2T-Rth+ (manufactured by Otsuka Electronics Co., Ltd.), with the width direction of the film set as the horizontal axis (x-axis) and the length direction of the film set as the vertical axis (y-axis).

[0308] When the position of the protrusion at any point on the end of the membrane is set as P0(x0, y0), the coordinates of the other protrusions are plotted as P1(x1, y1), P2(x2, y2), ..., P n (x n y n (n is an integer greater than or equal to 1).

[0309] The approximate linear relationship between the plotted graph and the position of the protrusion obtained by the above operations is shown in the figure. Figure 5 .

[0310] Based on the trajectory of the convex part drawn above, set the position of the convex part at any position at the end of the membrane as P0(x0, y0) = P0(0, 0), draw a straight line y = ax (x and y are variables) with a slope of a linear function (correlation coefficient R is 0.9 or higher) obtained by the least squares method, and find the angle θ [°] corresponding to the slope a at this time.

[0311] At this point, the tilt angle θ′[°] relative to the approximate straight line along the length direction of the membrane surface becomes θ′[°]=(90-θ)[°].

[0312] (Heat source section E) A and E B The average angle θ of the connecting lines relative to the length direction of the line. E ′)

[0313] In this invention, from the viewpoint of demonstrating the effects of the invention, it is preferable that the heat source portions of the infrared heaters are arranged at intervals of 10 to 100 mm in the width direction of the film, and that these heat source portions are arranged at positions different from their width positions in the length direction of the film. Each of the arranged heat source portions E A and E B The average inclination angle θ of the connecting straight lines E The angle is within the range of 2 to 45° relative to the length direction.

[0314] Regarding the spacing of the heat source section of the infrared heater mentioned above, a smaller spacing allows for minor contour adjustments, but the effective configuration range is as described above without excessively degrading the cost-effectiveness.

[0315] Furthermore, infrared heaters on the membrane, for example... Figure 6A , Figure 6B and Figure 6C They are arranged regularly in one or more columns along the length of the membrane. Figure 6A In the longitudinal direction of the membrane, there is one column. Figure 6B There are two columns along the length of the membrane. Figure 6C (There are 5 columns along the length of the membrane).

[0316] In Figure 6, P1, P2 and P3 represent the spacing between the heat source sections of each infrared heater.

[0317] Among them, observation Figure 6A , Figure 6B and Figure 6C It can be seen that each heat source part in the infrared heater is the central part of each infrared heater.

[0318] Furthermore, there is no limitation on the shape of the infrared heater in this invention. The heat source part of the actual infrared heater can be dot-shaped, line-shaped, or surface-shaped. When the actual infrared heater takes any shape such as dot-shaped, line-shaped, or surface-shaped, the "heat source part of the infrared heater" in this invention refers to the central part of the heat source part of the actual infrared heater.

[0319] In addition, the infrared heater is positioned 30 to 120 mm away from the membrane surface.

[0320] In addition, the heating width is set within the range of 100 to 250 mm.

[0321] Furthermore, the heat source section of the infrared heater is spaced within a range of 10 to 100 mm.

[0322] Each heat source part of the infrared heater is set within the range of 180-350°C, with a power of 100-1000W.

[0323] The following is a detailed explanation of the positional relationships of each heat source.

[0324] In order to determine the various heat source units E configured according to the present invention A and E B The average inclination angle θ of the connecting straight lines E At ′ time, heat source E A With E B The positional relationship is the closest positional relationship that makes the coordinates in the width direction different from the coordinates in the length direction (see Figure 6).

[0325] Specifically, for example, can be listed as Figure 7A , Figure 7B This is the positional relationship.

[0326] Furthermore, the various heat source units E that are configured A and E B The average angle θ of the connecting lines relative to the length direction of the line. E The following is an example of exporting.

[0327] The following uses Figure 7A Please provide an explanation.

[0328] like Figure 7A As shown, when the x-axis is taken in the width direction of the membrane and the y-axis is taken in the length direction, the heat source E is... A The coordinates are set to (x1, y1), and the heat source E is... B Let the coordinates be (x2, y2).

[0329] The angle θ is derived by setting |x2-x1| as the base of the triangle and |y2-y1| as the height of the triangle.E The value of [°] (0°≤θ≤90°) is calculated, and 90-θ is obtained. E The value of [°] is used to derive the average tilt angle θ of the line. E ′.

[0330] <Methods for controlling film thickness in the protrusion adjustment process>

[0331] (Method 4 for controlling film thickness)

[0332] Thickness control in the protrusion adjustment process can be achieved by, for example, changing the furnace temperature in the stretching device or the timing of heat treatment.

[0333] Furthermore, in this invention, the above-mentioned heat treatment is performed using an infrared (IR) heater, but other methods may also be used for heat treatment.

[0334] Furthermore, the aforementioned film thickness control method 4 can be implemented even outside the stretching apparatus by changing the furnace temperature, ambient temperature, and timing of heat treatment in other processes.

[0335] (Stretching and tensioning device)

[0336] [Furnace temperature]

[0337] The furnace temperature specified in this application refers to the temperature of the film measured at a position 100 mm above the center of the film immediately before it passes through the stretching zone (which will be described later) inside the stretching apparatus. The values ​​of each temperature are measured at 1-minute intervals for 1 hour, and their average value is calculated.

[0338] If the temperature difference between the furnace and the heat treatment is neither too small nor too large, the adjustment of the protrusion becomes easy.

[0339] Based on the above viewpoints, the temperature difference between the furnace and the heat treatment temperature is preferably within the range of 100 to 200°C.

[0340] Typically, the furnace temperature is preferably in the range of 120 to 220°C, and more preferably in the range of 120 to 180°C.

[0341] Among the multiple zones, when a temperature gradient is applied along the length direction, the zone undergoing heat treatment is taken as the object.

[0342] [Residual solvent amount immediately before the membrane passes through the stretching zone]

[0343] The amount of residual solvent in the membrane immediately before it passes through the stretching zone is preferably less than 20% by mass, and more preferably less than 15% by mass.

[0344] [Internal Components of the Tensioning Device 1]

[0345] A stretching device is a device that stretches a film by holding the two ends of the film in the width direction with clamps and expanding the gap while moving the clamps and the film together. It is usually divided into multiple zones (preheating zone, stretching zone and heat-fixing zone), and the timing of heat treatment is changed in the above three zones as needed.

[0346] In the heat treatment described above, infrared (IR) heaters are used, and the number of infrared (IR) heaters is appropriately set in each area as needed.

[0347] However, heat treatment methods other than infrared (IR) heaters can also be used as the heat treatment method in this invention.

[0348] The following is for reference Figure 8 The apparatus used as the tensioning device 7 will be described.

[0349] Figure 8 The plan view schematically showing the internal structure of the tenter frame is a cross-sectional view of the plane of the tenter frame perpendicular to the film surface, viewed from above.

[0350] Furthermore, Figure 8 This indicates that the cover has been removed; the cover is represented by a two-dot dash.

[0351] The tensioning device 40 includes a plurality of clamps 42 holding both ends of the membrane F in the width direction, and the clamps 42 are installed on the annular chain 48 at certain intervals.

[0352] The annular chain 48 clamps the membrane F on both sides, each hanging between the driving sprocket 50 on the inlet side and the driven sprocket 52 on the outlet side.

[0353] The drive sprocket 50 is connected to a motor (not shown), which drives the drive sprocket 50 to rotate.

[0354] As a result, the annular chain 48 travels around the driving sprocket 50 and the driven sprocket 52, and thus the clamp 42 mounted on the annular chain 48 travels around.

[0355] A track 54 for guiding the annular chain 48 (or clamp 42) is provided between the driving sprocket 50 and the driven sprocket 52.

[0356] The track 54 clamps the membrane F on both sides, and the spacing between the track 54 is configured such that the downstream side is wider than the upstream side in the transport direction of the membrane F.

[0357] As the clamps 42 move around, the spacing between them increases, thus allowing the optical film F held by the clamps 42 to be stretched laterally in the width direction.

[0358] Open components 56 are installed on the driving sprocket 50 and the driven sprocket 52 respectively.

[0359] The opening member 56 is a device for displacing the baffle (not shown) of the clamp 42 described later from the holding position to the open position. The opening member 56 automatically performs the holding and opening actions of the membrane F.

[0360] [Internal Components of the Tensioning Device 2]

[0361] like Figure 8 As shown, the interior of the tensioning device 40 is provided with a preheating zone, a (transverse) tensioning zone, and a heat-fixing zone.

[0362] The areas are separated from each other by windproof curtains (not shown).

[0363] In addition, within each zone, hot air is supplied to membrane F from above or below, or both.

[0364] Hot air is uniformly ejected along the width of membrane F while being managed at a specified temperature in each area.

[0365] This allows the internal temperature of each zone to be controlled to the desired level.

[0366] The following is an explanation of each region.

[0367] The preheating zone is the area where the membrane F is preheated without increasing the spacing of the clamps 42.

[0368] The preheated membrane F in the preheating zone moves to the transverse stretching zone.

[0369] The transverse stretching zone is the area in which the membrane F is stretched laterally in the width direction by widening the spacing of the clamps 42.

[0370] The stretching ratio in the transverse stretching process is preferably in the range of 1.0 to 2.5 times, more preferably in the range of 1.05 to 2.3 times, and even more preferably in the range of 1.1 to 2 times.

[0371] The membrane F, which is stretched laterally in the transverse stretching zone, moves to the heat-fixing zone.

[0372] Furthermore, in this embodiment, the interior of the tenter frame 40 is divided into a preheating zone, a (transverse) stretching zone, and a heat-fixing zone, but the types and configurations of the zones are not limited to these. For example, a cooling zone for cooling the film F can be provided after the transverse stretching zone.

[0373] In addition, a heat-relieving zone can be set in the heat-fixing zone.

[0374] Furthermore, in this embodiment, 40 tenters were stretched laterally using a tenter frame, and they can also be stretched simultaneously in the length direction.

[0375] In this case, the spacing between the clamps 42 (the distance between the clamps 42 in the transport direction) can be changed as the clamps 42 move.

[0376] As a mechanism for changing the spacing of the clamp 42, a scaling mechanism or a linear guide mechanism can be used, for example.

[0377] [Internal Components of the Tensioning Device 3]

[0378] Figure 9 This is a schematic diagram of the nozzle and heater arrangement in the three areas inside the tenter frame when viewed from the front.

[0379] Additionally, as an example of installing infrared (IR) heaters in various areas, in Figure 10 The image shows a side view of three areas within the tensioning device when the infrared (IR) heater is positioned in the preheating zone.

[0380] like Figure 9 As shown, the infrared (IR) heater is only positioned above the nozzle so that the membrane does not come into contact with the infrared (IR) heater when the membrane breaks.

[0381] In addition, when the infrared (IR) heater is brought close to the membrane, the radiative energy generated by the infrared (IR) heater can be concentrated in a narrower range. Therefore, the infrared (IR) heater can be brought as close to the membrane as possible without interfering with the widening operation of the fixture.

[0382] exist Figure 9 In the middle, the distance H from the membrane to the infrared (IR) heater A The preferred range is 30–120 mm.

[0383] In addition, regarding the heating width of the infrared (IR) heater mentioned above, a heating width of 100 to 250 mm is preferred.

[0384] Furthermore, the "heating width" mentioned above refers to the width heated by the infrared (IR) heater when the heating intensity directly below the infrared (IR) heater is set to 1 until its heating intensity becomes 0.2.

[0385] The spacing (pitch) of the infrared (IR) heaters is preferably 10 to 100 mm, and they are preferably heated in the range of 150 to 400°C at 100 to 1000 W.

[0386] In this invention, the film thickness profile in the width direction of the film is measured at various locations. The difference between the target film thickness profile and the current film thickness profile is used to calculate the set temperature of each infrared (IR) heater on a computer. The set temperature is output to each infrared (IR) heater via KEYENCE PLCKV-8000. By automatically repeating these operations, the protrusion is adjusted.

[0387] exist Figure 9 The heat treatment shown is mainly from the central nozzle. In this embodiment, heat treatment using the end nozzles is not performed, but it is possible to use them in this embodiment.

[0388] In a tensioning device, such as Figure 10 As shown, when the infrared (IR) heater is exposed from the nozzle gap, the radiative energy can be transferred to the membrane without waste.

[0389] Figure 11 To be different from the top side Figure 8 The viewpoint is a cross-sectional view of the tensioning device viewed from a plane perpendicular to the membrane surface.

[0390] like Figure 11 As shown, in the membrane before stretching, infrared (IR) heaters are arranged in a row in a manner that allows the entire width to be heated.

[0391] Furthermore, the heater can be configured in a serrated shape along its length.

[0392] (The relationship between the heat A in the central part of the infrared heater and the average heat B at the ends of the infrared heater)

[0393] In the protrusion adjustment process (S2), from the viewpoint of achieving the desired effect, it is preferable to use an infrared (IR) heater for local heating, and the average value of the heat A in the central part of the infrared (IR) heater and the heat B at the end of the infrared (IR) heater 75 mm away from the central part satisfies the following formula (1).

[0394] Equation (1): 0.2 < (B / A) < 0.6

[0395] If the heat generated by the infrared irradiation light produced by the infrared heater described above has good convergence, more subtle film thickness profile adjustments can be made. Therefore, considering the yield to a degree where thermal control is not too difficult, the above-mentioned range is effective in this invention.

[0396] It should be noted that the "central part of the infrared (IR) heater" mentioned above refers to each heat source part in Figure 6 above.

[0397] In addition, the "infrared (IR) heater end" mentioned above refers to a position 75mm in width from the center.

[0398] In this invention, the average value B of the heat A in the central part of the infrared (IR) heater and the heat at the end of the infrared heater is calculated by measuring the temperature distribution using an infrared thermal imager (VIM-640G2ULC manufactured by Visual Center Co., Ltd.), and taking the average value. This is the same when other heat treatment methods are used.

[0399] The principles and calculation methods are explained in detail below.

[0400] The membrane is heated using the infrared (IR) heater described above.

[0401] The temperature variation of the heated portion is accumulated along the length direction, and the central part of its width is set as heat A. The average value at a position of 75mm along the width direction is set as the average value of the heat at the end of the infrared heater, B.

[0402] Based on the above values, calculate the heat ratio (B / A) between the heat A in the central part of the infrared (IR) heater and the average heat B at the end of the infrared (IR) heater.

[0403] At this time, when (B / A) is too large, the infrared (IR) heater is not designed to precisely narrow the infrared irradiation range. When (B / A) is too small, the range of (B / A) value can be controlled by increasing the number of infrared (IR) heaters installed in the width direction.

[0404] Infrared (IR) heater

[0405] The details of the infrared (IR) heater used in this invention will be described.

[0406] As an infrared (IR) heater that can be used in the implementation of the present invention, unlike a general infrared (IR) heater, it is preferable to use a reflector that reflects infrared light, thereby setting it in a way that can precisely narrow the irradiation range of infrared light.

[0407] Examples of reflectors that reflect infrared light include cold reflectors (manufactured by Sigma Optical Co., Ltd.) and infrared aluminum anti-reflective mirrors (manufactured by Novo Optics Co., Ltd.).

[0408] The reflector used in the embodiment of the present invention is an infrared aluminum antireflector (manufactured by Novo Optics Co., Ltd.) which is an aluminum reflector.

[0409] The infrared irradiation range of a conventional infrared (IR) heater is, for example, 500 mm in the width direction at MCHNNS3 and irradiation energy of 400 W (manufactured by Misumi Co., Ltd.), while the infrared (IR) heater used in the embodiment of the present invention has an infrared irradiation range of 100 to 150 mm in the width direction at irradiation energy of 550 W (manufactured by Heattech Co., Ltd.).

[0410] (1.3) Finishing process (S3)

[0411] In the trimming process (S3), the cutting section 8, which is composed of a longitudinal cutting mechanism, cuts (trims) both ends of the stretched film F in the width direction.

[0412] From the viewpoint of the effectiveness of the present invention, it is preferable not to vibrate the membrane prior to the above-described modifications.

[0413] To clarify, in this specification, "vibration" refers to the movement of the membrane itself in the width direction.

[0414] In membrane F, the remaining portion after cutting off both ends of the membrane constitutes the product part of the membrane product.

[0415] On the other hand, the portion cut from membrane F can be recycled and reused again as part of the raw materials in membrane manufacturing.

[0416] After the finishing process, the membrane may also be knurled. However, from the viewpoint of suppressing excessive air intake, it is preferable not to knurl the membrane after the finishing process.

[0417] (1.4) Winding process (S4)

[0418] Finally, in the winding process (S4), the membrane F is wound up using the winding device 13 to obtain a membrane roll.

[0419] That is, in the winding process, the film roll is manufactured by transporting the film F while winding it onto the core.

[0420] The preferred range for the initial tension during the winding process when winding the film is 20 to 300 N / m.

[0421] (Amount of residual solvent immediately before winding)

[0422] More specifically, the process of winding the membrane using the winding device 12 after the residual solvent content in the membrane is reduced to 2% by mass or less is achieved by reducing the residual solvent content to 0.4% by mass or less, thereby obtaining a membrane with good dimensional stability.

[0423] In particular, it is preferred to roll up the solvent in the range of 0.00 to 0.20% by mass.

[0424] (Roll-up method)

[0425] Regarding the winding method of film F, a commonly used winding machine can be used. There are methods for controlling tension, such as constant torque method, constant tension method, taper tension method, and programmed tension control method with constant internal stress. These methods can be used in different ways.

[0426] Before winding, the ends of the film are longitudinally cut to the width of the finished product. To prevent sticking and scratching during winding, the ends of the film can be surface modified.

[0427] (After rolling)

[0428] The membrane rolls involved in this invention are preferably long strip membranes, specifically, membranes in the range of about 100 to 10,000 m, and are usually provided in roll form.

[0429] <Details of the membrane winding method>

[0430] The membrane involved in this invention is preferably wound using the following winding method.

[0431] The winding method preferably includes: a straight winding process in which the film is wound onto a core with the side edges of the film aligned; and a vibration winding process in which the film or the core is periodically vibrated in the width direction of the film to wind the film onto the core, with the side edges periodically deviating from the width direction of the film within a certain range.

[0432] Specifically, it is preferable that the roll length of the membrane is in the range of 1% to 30% of the total roll length of the membrane, and when the predetermined roll length is reached for replacement, the process switches from the straight winding process to the vibratory winding process.

[0433] The film winding device preferably includes: a film winding section for rotating a core to wind the film onto the core; a vibration section for vibrating the film or the core in conjunction with the film winding, in a manner that causes the film to periodically deviate within a certain range in the width direction of the film on the core; and a switching section for switching the film winding from straight winding to vibration winding when the film winding length reaches a predetermined switching winding length.

[0434] Details regarding vibration winding are omitted below.

[0435] Figure 12 This is a schematic diagram illustrating the process of winding the film and a cross-section of the film roll according to the present invention after winding.

[0436] exist Figure 11In the process, the film 31 after film preparation is wound up by roller 32 and touch roller 33 to form film roll 30.

[0437] 2. Manufacturing method of film rolls using melt casting method

[0438] The membrane involved in this invention can also be formed using the melt casting method.

[0439] The so-called "melt casting film method" refers to a method of heating and melting a composition containing thermoplastic resin and the above-mentioned additives until it reaches a temperature that shows fluidity, and then casting the fluid melt containing thermoplastic resin.

[0440] As a molding method involving heating and melting, it can be specifically classified into melt extrusion molding, compression molding, blow molding, injection molding, blow molding, stretch molding, etc.

[0441] Among these molding methods, melt extrusion is preferred in terms of mechanical strength and surface precision.

[0442] The following process flow for the melt casting method is also applicable to the solution casting method described above. Figure 2 The same process will be explained.

[0443] in addition, Figure 13 This is a schematic diagram of an apparatus for manufacturing optical films using the melt casting method.

[0444] The following refers to the solution casting method for film formation. Figure 2 and Figure 13 Please provide an explanation.

[0445] The manufacturing method of the film roll using the melt casting method of the present invention includes: a film forming process (S1), a protrusion adjustment process (S2), a trimming process (S3), and a winding process (S4).

[0446] (2.1) Membrane formation process (S1)

[0447] (2.1.1) Melt extrusion of resin

[0448] The resin is melted and extruded using an extruder 14 and then formed on a casting drum 16.

[0449] Details of the resins that can be used in this invention will be described later. It is preferable to pre-mix and granulate the resins, and granulation can be carried out using known methods.

[0450] For example, by feeding dried resin, plasticizer, and other additives into an extruder using a feeder, mixing them using a single-screw or twin-screw extruder, extruding them into filaments from a casting die, and then water-cooling or air-cooling them before cutting them, granulation can be achieved.

[0451] The additive can be mixed into the resin before being fed to the extruder, or the additive and resin can be fed to the extruder separately using separate feeders.

[0452] In addition, for small amounts of additives such as particles and antioxidants, it is preferable to mix them in the resin beforehand in order to ensure uniform mixing.

[0453] When feeding pellets from the feed hopper into the extruder, it is preferable to feed them under dry conditions, vacuum or reduced pressure, or in an inert gas atmosphere to prevent oxidation and decomposition.

[0454] In terms of extruders, in order to suppress shear force and granulate without resin degradation (molecular weight reduction, coloring, gel formation, etc.), it is preferable to process at low temperature.

[0455] For example, in the case of a twin-screw extruder, it is preferable to use a deep-groove screw that rotates in the same direction.

[0456] Based on the uniformity of the mixture, the interlocking type is preferred.

[0457] When the resin or granules are melted, it is preferable to use a disc-type filter or similar filter to remove foreign matter.

[0458] The granules obtained as described above are used to form a film.

[0459] Of course, it is also possible to directly feed the raw resin (powder, etc.) into the extruder through a feeder without granulation and directly form a film.

[0460] (2.1.2) Casting and molding of molten resin granules

[0461] Molten resin granules are cast into a film through a conduit via a pressurized quantitative gear pump or similar device from a casting die 15. The molten resin granules are cast from the casting die 15 at the casting position on a rotating stainless steel annular casting drum 16 that is moved indefinitely.

[0462] Then, the molten resin granules are molded on the casting drum 16 to form a film F.

[0463] The tilt angle of the casting die 15, that is, the discharge direction of the molten resin granules from the casting die 15 to the support 16, is appropriately set in a range of 0 to 90° relative to the normal of the surface of the casting drum 16 (the surface on which the molten resin granules are cast).

[0464] The touch roller 16a and the cooling drum 17 of the auxiliary casting drum 16 may be formed into film F individually or in combination, as appropriate.

[0465] The methods for controlling film thickness and other matters in the film formation process are the same as those for the manufacturing process of film rolls using the solution casting method described above. The descriptions of residual solvent amount, shrinkage rate and drying method are also repeated, so they are omitted.

[0466] (2.2) Convex adjustment process (S2)

[0467] For the outline of the convex adjustment process, details of the convex adjustment process, film stretching, definitions of various terms in the convex adjustment process, film thickness control methods in the convex adjustment process, and other matters, the same descriptions as those for the film roll manufacturing process using the solution casting method described above are omitted.

[0468] In the protrusion adjustment process, if the membrane is locally heated, the membrane is simultaneously stretched.

[0469] The above-mentioned membrane F is stretched using the stretching device 19.

[0470] Drying can be performed inside the stretching device 19, in addition to stretching.

[0471] (2.3) Finishing process (S3)

[0472] In the trimming process (S3), the cutting section 20, which is composed of a longitudinal cutting mechanism, cuts (trims) both ends of the film in the width direction of the film F.

[0473] During the above-described modifications, from the viewpoint of demonstrating the effects of the present invention, it is preferable not to cause the membrane to vibrate or not to cause the membrane to vibrate in the width direction of the membrane.

[0474] In membrane F, the remaining portion after cutting off both ends of the membrane constitutes the product part of the membrane product.

[0475] On the other hand, the portion cut from membrane F can be recycled and reused again as part of the raw materials in membrane manufacturing.

[0476] After the finishing process, the membrane can also be knurled. From the viewpoint of the effectiveness of the present invention, it is preferable not to knurl the membrane after the finishing process.

[0477] (2.4) Winding process (S4)

[0478] Finally, in the winding process (S4), the membrane F is wound up using the winding device 23 to obtain a membrane roll.

[0479] That is, in the winding process, the film F is wound onto the core while being transported, thereby manufacturing the film roll.

[0480] Regarding the winding method of film F, a commonly used winding machine can be used. There are methods for controlling tension, such as constant torque method, constant tension method, taper tension method, and programmed tension control method with constant internal stress. These methods can be used in different ways.

[0481] 3. Protrusion Adjustment System in Membrane Roll Manufacturing

[0482] The protrusion adjustment system used in the manufacturing of the membrane roll of the present invention is a protrusion adjustment system used in the manufacturing of a membrane roll having a protrusion adjustment process for adjusting the number, height, and position of protrusions in the width direction of the membrane surface. It is characterized by having: a membrane thickness acquisition means for obtaining the membrane thickness profile of the membrane in the protrusion adjustment process; a determination means for determining whether the number of protrusions in the width direction is within an ideal range of 1 to 10 per 1m and whether the height of the protrusions in the width direction is within an ideal range of 0.05 to 0.50 μm, based on the membrane thickness profile data; and a means for locally heating the membrane using an infrared heater so that both the number of protrusions and the height of the protrusions are within the ideal range when either the number of protrusions or the height of the protrusions is outside the ideal range in the determination means.

[0483] (3.1)Means for obtaining film thickness

[0484] (Method 1)

[0485] As a means of obtaining the film thickness in the protrusion adjustment system during the manufacturing of the film roll of the present invention, the film thickness is measured using an online delay film thickness measuring device RE-200L2T-Rth+ film thickness (manufactured by Otsuka Electronics Co., Ltd.).

[0486] Details regarding the definitions of terms related to convex parts, as described above, are omitted here.

[0487] (Method 2)

[0488] In the convex part adjustment process, the membrane is locally heated and stretched in the stretching device.

[0489] (3.2) Judgment methods

[0490] Based on the film thickness profile data, determine whether the number of protrusions in the width direction is within the ideal range of 1 to 10 per 1m and whether the height of the protrusions in the width direction is within the ideal range of 0.05 to 0.50μm.

[0491] (3.3) Method of local heating of the membrane using an infrared heater

[0492] When the number of protrusions and the height of the protrusions are outside the ideal range, the set temperature of each infrared heater is calculated on the computer based on the difference from the current film thickness profile, and each set temperature is output. The infrared heaters are used to locally heat the film, thereby adjusting the protrusions and automatically and repeatedly adjusting the film thickness.

[0493] 4. Resins that make up the membrane

[0494] (4.1) Thermoplastic resin

[0495] The thermoplastic resin material used in the film of this invention is not limited as long as it is used as a material for film roll processing after film making.

[0496] For example, thermoplastic resins used for polarizing applications can include cellulose ester resins such as triacetyl cellulose (TAC), cellulose acetate propionate (CAP), and diacetyl cellulose (DAC), cyclic olefin resins such as cyclic olefin polymers (COP) (hereinafter also referred to as cyclic olefin resins), polypropylene resins such as polypropylene (PP), acrylic resins such as polymethyl methacrylate (PMMA), and polyester resins such as polyethylene terephthalate (PET).

[0497] In particular, in films with low elastic modulus, such as resins with an elastic modulus of less than 3.0 GPa, it is difficult to alleviate the stress involved in multiple parts of the film when forming the film roll. It becomes difficult to stretch and contract in the width and length directions. The film cannot fully absorb stress in the plane when rolled up, and is prone to winding offset.

[0498] Furthermore, from another perspective, if there is a height difference between the high and low points of the membrane along its length, the difference between the stretching at the high point and the stretching at the low point becomes larger.

[0499] Therefore, in embodiments of the present invention, it is preferable to control the maximum height difference (PV) of the length-average film thickness within the range of 0.02 to 0.40 μm, which is effective in film rolls using cyclic olefin polymers (cyclic olefin resins (COP)) and polymethyl methacrylate (acrylic resins (PMMA)) as thermoplastic resins, which are resins with low elastic modulus.

[0500] However, cyclic olefin resins (COP) are preferred in terms of ease of control over tensile properties and crystallinity, ease of adhesive penetration, and ability to ensure better adhesion to the polarizer layer.

[0501] Furthermore, the above-mentioned membrane can undergo surface modification treatment after manufacturing.

[0502] Furthermore, the effects of this invention enhance its value in the field of thin films.

[0503] The membrane thickness is preferably in the range of 5 to 80 μm, more preferably in the range of 10 to 65 μm, and even more preferably in the range of 10 to 45 μm.

[0504] If the membrane thickness is greater than 5 μm, the membrane roll has high rigidity, making it easier to maintain the roll shape.

[0505] If the film thickness is below 80 μm, the mass is not excessively increased, and it is easy to produce long strips of film.

[0506] (4.1.1) Cycloolefin resins

[0507] The cyclic olefin resin contained in the film rolls involved in this invention is preferably a polymer of cyclic olefin monomers, or a copolymer of cyclic olefin monomers and other comonomers.

[0508] As a cyclic olefin monomer, a cyclic olefin monomer having a norbornene skeleton is preferred, and a cyclic olefin monomer having a structure represented by the following general formula (A-1) or (A-2) is more preferred.

[0509] [Chemistry 1]

[0510] General form (A-1)

[0511]

[0512] In general formula (A-1), R 1 ~R 4 Each can independently represent a hydrogen atom, a hydrocarbon group with 1 to 30 carbon atoms, or a polar group. p represents an integer from 0 to 2. However, R... 1 ~R 4 All of them cannot simultaneously represent hydrogen atoms, R 1 and R 2 It will not simultaneously represent hydrogen atoms, R 3 and R 4 It cannot simultaneously represent hydrogen atoms.

[0513] In general formula (A-1), as R 1 ~R 4 The hydrocarbon group representing 1 to 30 carbon atoms is preferably a hydrocarbon group representing 1 to 10 carbon atoms, and more preferably a hydrocarbon group representing 1 to 5 carbon atoms.

[0514] Hydrocarbon groups with 1 to 30 carbon atoms may further have connecting groups, for example, containing halogen atoms, oxygen atoms, nitrogen atoms, sulfur atoms, or silicon atoms.

[0515] Examples of such linking groups include divalent polar groups such as carbonyl, imino, ether, silyl ether, and thioether.

[0516] Examples of hydrocarbon groups with 1 to 30 carbon atoms include methyl, ethyl, propyl, and butyl.

[0517] In general formula (A-1), R 1 ~R 4 Examples of polar groups include carboxyl, hydroxyl, alkoxy, alkoxycarbonyl, aryloxycarbonyl, amino, amide, and cyano.

[0518] Among them, carboxyl, hydroxy, alkoxycarbonyl and aryloxycarbonyl are preferred. From the viewpoint of ensuring solubility during solution film formation, alkoxycarbonyl and aryloxycarbonyl are preferred.

[0519] From the viewpoint of improving the heat resistance of the membrane, p in the general formula (A-1) is preferably 1 or 2.

[0520] This is because if p is 1 or 2, the resulting polymer becomes bulky, and the glass transition temperature is easily increased.

[0521] [Chemistry 2]

[0522] General form (A-2)

[0523]

[0524] In general formula (A-2), R 5 R represents a hydrogen atom, a hydrocarbon group having 1 to 5 carbon atoms, or an alkylsilyl group having 1 to 5 carbon atoms. 6 This indicates a carboxyl, hydroxyl, alkoxycarbonyl, aryloxycarbonyl, amino, amide, cyano, or halogen atom (fluorine, chlorine, bromine, or iodine). p represents an integer from 0 to 2.

[0525] R in general formula (A-2) 5 Preferably, the hydrocarbon group represents 1 to 5 carbon atoms, and more preferably, the hydrocarbon group represents 1 to 3 carbon atoms.

[0526] R in general formula (A-2) 6 The preferred groups are carboxyl, hydroxyl, alkoxycarbonyl, and aryloxycarbonyl. From the viewpoint of ensuring solubility during solution film formation, alkoxycarbonyl and aryloxycarbonyl are more preferred.

[0527] In general formula (A-2), p is preferably represented as 1 or 2 from the viewpoint of improving the heat resistance of the membrane.

[0528] This is because if p represents 1 or 2, the resulting polymer becomes bulky, and the glass transition temperature is easily increased.

[0529] From the perspective of improving solubility in organic solvents, cyclic olefin monomers having a structure represented by general formula (A-2) are preferred.

[0530] Generally, organic compounds have reduced crystallinity due to the destruction of symmetry, thus increasing their solubility in organic solvents.

[0531] Regarding R in general formula (A-2) 5 and R 6 In contrast, cyclic olefin monomers, which have a structure represented by the general formula (A-2), are substituted by carbon atoms of a ring on only one side of the molecular axis of symmetry. Therefore, the symmetry of the molecule is low. Thus, cyclic olefin monomers are highly soluble and suitable for manufacturing films by solution casting.

[0532] The proportion of cyclic olefin monomers having a structure represented by general formula (A-2) in the polymer of cyclic olefin monomers relative to the total number of all cyclic olefin monomers constituting the cyclic olefin resin may be, for example, 70 mol% or more, preferably 80 mol% or more, and more preferably 100 mol%.

[0533] If the resin contains a certain number or more cyclic olefin monomers with a structure represented by the general formula (A-2), the orientation of the resin is improved, and therefore the phase difference (retardation) value tends to increase.

[0534] The following examples of cyclic olefin monomers having a structure represented by general formula (A-1) are illustrated in Examples 1 to 14, and examples of cyclic olefin monomers having a structure represented by general formula (A-2) are illustrated in Examples 15 to 34.

[0535] [Chemistry 3]

[0536]

[0537] Examples of comonomers that can copolymerize with cyclic olefin monomers include comonomers that can undergo ring-opening copolymerization with cyclic olefin monomers and comonomers that can undergo addition copolymerization with cyclic olefin monomers.

[0538] Examples of comonomers that can undergo ring-opening copolymerization include cyclic olefins such as cyclobutene, cyclopentene, cycloheptene, cyclooctene, and dicyclopentadiene.

[0539] Examples of addit-copolymerizable comonomers include compounds containing unsaturated double bonds, vinyl cyclic hydrocarbon monomers, and (meth)acrylates.

[0540] Examples of compounds containing unsaturated double bonds include olefinic compounds with 2 to 12 carbon atoms (preferably 2 to 8), including ethylene, propylene, and butene.

[0541] Examples of vinyl cyclic hydrocarbon monomers include vinylcyclopentene monomers such as 4-vinylcyclopentene and 2-methyl-4-isopropenylcyclopentene.

[0542] Examples of (meth)acrylates include alkyl (meth)acrylates with 1 to 20 carbon atoms, such as methyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, and cyclohexyl (meth)acrylate.

[0543] The proportion of cyclic olefin monomers in the copolymer of cyclic olefin monomers and copolymeric monomers relative to the total number of monomers constituting the copolymer can be, for example, in the range of 20 to 80 mol%, preferably in the range of 30 to 70 mol%.

[0544] As described above, cyclic olefin resins are polymers obtained by polymerizing or copolymerizing cyclic olefin monomers having a norbornene backbone, preferably cyclic olefin monomers having a structure represented by general formula (A-1) or (A-2), and in some cases include polymers of the following (1) to (7).

[0545] (1) Ring-opening polymers of cyclic olefin monomers

[0546] (2) Ring-opening copolymers of cyclic olefin monomers and comonomers that can be ring-opened copolymerized with them

[0547] (3) The hydride of the ring-opening (co)polymer of (1) or (2) above

[0548] (4) The hydrogenated (copolymer) formed by cyclizing the ring-opening (co)polymer of (1) or (2) above using the Fourier Crafts reaction.

[0549] (5) Saturated copolymers of cycloolefin monomers and compounds containing unsaturated double bonds

[0550] (6) Addition copolymers of cyclic olefin monomers with vinyl cyclic hydrocarbon monomers and their hydrides

[0551] (7) Alternating copolymers of cyclic olefin monomers and (meth)acrylates

[0552] The polymers described in (1) to (7) above can be obtained by any known method, such as the methods described in Japanese Patent Application Publication No. 2008-107534 and Japanese Patent Application Publication No. 2005-227606.

[0553] For example, the catalyst and solvent used in the ring-opening copolymerization in (2) above can be those described in paragraphs 0019 to 0024 of Japanese Patent Application Publication No. 2008-107534.

[0554] The catalysts used in the hydrides of (3) and (6) above can be, for example, the catalysts described in paragraphs 0025 to 0028 of Japanese Patent Application Publication No. 2008-107534.

[0555] The acidic compound used in the Friedel-Crafts reaction described above (4) can be, for example, the acidic compound described in paragraph 0029 of Japanese Patent Application Publication No. 2008-107534.

[0556] The catalyst used in the addition polymerization of (5) to (7) above can be, for example, the catalyst described in paragraphs 0058 to 0063 of Japanese Patent Application Publication No. 2005-227606.

[0557] The alternating copolymerization reaction described in (7) above can be carried out by, for example, the method described in paragraphs 0071 and 0072 of Japanese Patent Application Publication No. 2005-227606.

[0558] Among them, the polymers of (1) to (3) and (5) above are preferred, and the polymers of (3) and (5) above are more preferred.

[0559] That is, from the perspective of increasing the glass transition temperature of the obtained cycloolefin resin and increasing the light transmittance, the cycloolefin resin preferably contains at least one of the structural units represented by the following general formula (B-1) and the structural units represented by the following general formula (B-2), more preferably it contains only the structural unit represented by general formula (B-2), or contains both the structural units represented by general formula (B-1) and the structural units represented by general formula (B-2).

[0560] The structural unit represented by general formula (B-1) is derived from the structural unit of the cyclic olefin monomer represented by general formula (A-1) mentioned above, and the structural unit represented by general formula (B-2) is derived from the structural unit of the cyclic olefin monomer represented by general formula (A-2) mentioned above.

[0561] [Chemistry 4]

[0562] General form (B-1)

[0563]

[0564] In general formula (B-1), X represents -CH=CH- or -CH2CH2-. 1 ~R 4 And p are respectively related to R in general formula (A-1) 1 ~R 4 Synonymous with p.

[0565] [Chemistry 5]

[0566] General form (B-2)

[0567]

[0568] In general formula (B-2), X represents -CH=CH- or -CH2CH2-. 5 ~R 6 And p are respectively related to R in general formula (A-2) 5 ~R 6 Synonymous with p.

[0569] The cyclic olefin resins involved in this invention are commercially available products.

[0570] Examples of commercially available cycloolefin resins include Arton G (e.g., G7810), Arton F, Arton R (e.g., R4500, R4900, and R5000), and Arton RX manufactured by JSR Corporation.

[0571] The intrinsic viscosity [η]inh of cycloolefin resins, measured at 30°C, is preferably 0.2–5 cm⁻¹. 3 Within the range of / g, more preferably 0.3 to 3cm 3 Within the range of / g, it is further preferred to be 0.4 to 1.5 cm. 3 Within the range of / g.

[0572] The number-average molecular weight (Mn) of the cyclic olefin resin is preferably in the range of 8,000 to 100,000, more preferably in the range of 10,000 to 80,000, and even more preferably in the range of 12,000 to 50,000.

[0573] The weight-average molecular weight (Mw) of the cyclic olefin resin is preferably in the range of 20,000 to 300,000, more preferably in the range of 30,000 to 250,000, and even more preferably in the range of 40,000 to 200,000.

[0574] The number-average molecular weight and weight-average molecular weight of cyclic olefin resins can be determined by polystyrene conversion in gel permeation chromatography (GPC).

[0575] (Gel permeation chromatography)

[0576] Solvent: dichloromethane

[0577] Columns: Shodex K806, K805, K803G (manufactured by Showa Denko Co., Ltd., 3-column connection)

[0578] Column temperature: 25℃

[0579] Sample concentration: 0.1% by mass

[0580] Detector: RI Model 504 (manufactured by GL Science)

[0581] Pump: L6000 (manufactured by Hitachi, Ltd.)

[0582] Flow rate: 1.0 ml / minute

[0583] Calibration curves: Calibration curves were obtained using 13 samples of standard polystyrene (Tosoh Corporation) with a Mw range of 500 to 2,800,000. The 13 samples were preferably used at approximately equal intervals.

[0584] If the intrinsic viscosity [η]inh, number-average molecular weight, and weight-average molecular weight are within the above ranges, the heat resistance, water resistance, chemical resistance, mechanical properties, and processability as a film of the cycloolefin resin become good.

[0585] The glass transition temperature (Tg) of cycloolefin resins is typically above 110°C, preferably in the range of 110 to 350°C, more preferably in the range of 120 to 250°C, and even more preferably in the range of 120 to 220°C.

[0586] If the glass transition temperature (Tg) is above 110℃, deformation under high temperature conditions can be easily suppressed.

[0587] On the other hand, if the glass transition temperature (Tg) is below 350°C, molding becomes easier and it is also easier to suppress the degradation of the resin caused by heat during molding.

[0588] The content of cycloolefin resin relative to the membrane is preferably 70% by mass or more, and more preferably 80% by mass or more.

[0589] (4.1.2) Acrylic resins

[0590] The acrylic resins involved in this invention are polymers of acrylates or methacrylates, and also include copolymers with other monomers.

[0591] Therefore, the acrylic resins involved in this invention also include methacrylic resins.

[0592] There are no particular limitations on the resin, but resins with methyl methacrylate units in the range of 50 to 99% by mass and other monomer units that can be copolymerized with it in the range of 1 to 50% by mass are preferred.

[0593] Other units constituting acrylic resins formed by copolymerization include alkyl methacrylates with 2 to 18 carbon atoms, alkyl acrylates with 1 to 18 carbon atoms, isobornyl methacrylate, 2-hydroxyethyl acrylate and other hydroxyalkyl acrylates, acrylic acid, methacrylic acid and other α,β-unsaturated acids, acrylamide, N-hydroxyphenylmethylacrylamide and other acrylamides, N-vinylpyrrolidone, maleic acid, fumaric acid, itaconic acid and other divalent carboxylic acids containing unsaturated groups, styrene, α-methylstyrene and other aromatic vinyl compounds, acrylonitrile, methacrylonitrile and other α,β-unsaturated nitriles, maleic anhydride, maleimide, N-substituted maleimide, glutarimide and glutaric anhydride, etc.

[0594] Monomers that can be copolymerized to form units excluding glutarimide and glutaric anhydride from the above units can be listed as monomers corresponding to the above units.

[0595] That is, examples include alkyl methacrylates with 2 to 18 carbon atoms, alkyl acrylates with 1 to 18 carbon atoms, isobornyl methacrylate, 2-hydroxyethyl acrylate and other hydroxyalkyl acrylates, acrylic acid, methacrylic acid and other α,β-unsaturated acids, acrylamide, N-hydroxyphenylmethylacrylamide and other acrylamides, N-vinylpyrrolidone, maleic acid, fumaric acid, itaconic acid and other divalent carboxylic acids containing unsaturated groups, styrene, α-methylstyrene and other aromatic vinyl compounds, acrylonitrile, methacrylonitrile and other α,β-unsaturated nitriles, maleic anhydride, maleimide and N-substituted maleimide and other monomers.

[0596] In addition, the glutarimide unit can be formed by, for example, reacting an intermediate polymer having (meth)acrylate units with a primary amine (imidizing agent) to form an imidized unit (see Japanese Patent Application Publication No. 2011-26563).

[0597] The glutaric anhydride unit can be formed, for example, by heating an intermediate polymer having (meth)acrylate units (see Japanese Patent No. 4961164).

[0598] In the acrylic resins of the present invention, from the viewpoint of mechanical strength, the above-mentioned structural units particularly preferably include isobornyl methacrylate, acryloylmorpholine, N-hydroxyphenylmethylacrylamide, N-vinylpyrrolidone, styrene, hydroxyethyl methacrylate, maleic anhydride, maleimide, N-substituted maleimide, glutaric anhydride or glutarimide.

[0599] Regarding the acrylic resins involved in this invention, from the viewpoints of controlling dimensional changes relative to changes in ambient temperature and humidity, peelability from the metal support during film production, drying properties of organic solvents, heat resistance, and improved mechanical strength, a weight-average molecular weight (Mw) in the range of 50,000 to 1,000,000 is preferred, more preferably in the range of 100,000 to 1,000,000, and particularly preferably in the range of 200,000 to 800,000 is preferred.

[0600] If the value is above 50,000, the heat resistance and mechanical strength are excellent; if the value is below 1,000,000, the peelability from the metal support and the drying properties of organic solvents are excellent.

[0601] There are no particular limitations on the method for manufacturing the acrylic resin involved in this invention, and any known method such as suspension polymerization, emulsion polymerization, bulk polymerization, or solution polymerization can be used.

[0602] Among them, as a polymerization initiator, conventional peroxide-based and azo-based polymerization initiators can be used, and redox-based initiators can also be used.

[0603] Regarding polymerization temperature, it can be carried out in the range of 30 to 100°C in suspension or emulsion polymerization, and in the range of 80 to 160°C in bulk or solution polymerization.

[0604] To control the reduced viscosity of the resulting copolymer, chain transfer agents such as alkyl thiols can also be used to carry out polymerization.

[0605] From the viewpoint of maintaining the mechanical strength of the film, the glass transition temperature (Tg) of the acrylic resin is preferably in the range of 80 to 120°C.

[0606] As the acrylic resin involved in this invention, commercially available products can be used.

[0607] Examples include DELPET 60N, 80N, 980N, SR8200 (all manufactured by Asahi Kasei Chemicals Co., Ltd.), Diannal BR52, BR80, BR83, BR85, BR88, EMB-143, EMB-159, EMB-160, EMB-161, EMB-218, EMB-229, EMB-270, EMB-273 (all manufactured by Mitsubishi Rayon Co., Ltd.), KT75, TX400S, and IPX012 (all manufactured by Denki Kagaku Kogyo Co., Ltd.).

[0608] Acrylic resins can also be used in combination with two or more types.

[0609] The acrylic resin involved in this invention preferably contains additives. As an example of an additive, in order to improve the mechanical strength of the film and adjust the dimensional change rate, it preferably contains acrylic particles (rubber elastomer particles) as described in International Publication No. 2010 / 001668.

[0610] Examples of commercially available multilayer acrylic granular composites include "METABLEN W-341" manufactured by Mitsubishi Rayon Co., Ltd., "KaneAce" manufactured by Kaneka Corporation, "PARALOID" manufactured by Gou Co., Ltd., "Acreide" manufactured by Rohm and Haas Co., Ltd., "STAPHYLOID" manufactured by AICA Co., Ltd., Chemisnow MR-2G, MS-300X (all manufactured by Soken Chemical Co., Ltd.), and "PARAPET SA" manufactured by Kuraray Co., Ltd. These can be used alone or in combination with two or more other products.

[0611] The volume average particle size of the acrylic particles is less than 0.35 μm, preferably in the range of 0.01 to 0.35 μm, and more preferably in the range of 0.05 to 0.30 μm.

[0612] If the particle size is above a certain value, the film can be easily stretched under heating; if the particle size is below a certain value, the transparency of the resulting film is not easily damaged.

[0613] From the viewpoint of flexibility, the membrane involved in this invention preferably has a flexural modulus (JIS K7171) of 10.5 GPa or less.

[0614] The flexural modulus is more preferably 1.3 GPa or less, and even more preferably 1.2 GPa or less.

[0615] The flexural modulus varies depending on the type and amount of acrylic resin and rubber elastomer particles in the film. For example, the higher the content of rubber elastomer particles, the lower the flexural modulus generally is.

[0616] Furthermore, as an acrylic resin, the flexural modulus is generally smaller when using copolymers of alkyl methacrylate and alkyl acrylate, etc., compared to homopolymers using alkyl methacrylate.

[0617] (4.1.3) Cellulose ester resins

[0618] In the film rolls involved in this invention, cellulose ester resins are also preferably used.

[0619] The cellulose ester used in this invention refers to a cellulose acylated resin in which some or all of the hydrogen atoms of the hydroxyl groups (-OH) at the 2, 3, and 6 positions of the β-1,4-linked glucose units constituting cellulose are replaced by acyl groups.

[0620] There are no particular limitations on the cellulose esters used, but esters of carboxylic acids with a straight chain or branching carbon number of about 2 to 22 are preferred.

[0621] The carboxylic acids that make up esters can be aliphatic carboxylic acids, can form rings, or can be aromatic carboxylic acids.

[0622] Examples of cellulose esters include those in which the hydrogen atom of the hydroxyl moiety is replaced by an acyl group with 2 to 22 carbon atoms, such as acetyl, propionyl, butyryl, isobutyryl, valeryl, neovaleryl, hexanoyl, octanoyl, lauroyl, and stearyl.

[0623] The carboxylic acid (acyl group) that makes up an ester may have substituents.

[0624] The carboxylic acid constituting the ester is particularly preferably a lower fatty acid with 6 or fewer carbon atoms, and more preferably a lower fatty acid with 3 or fewer carbon atoms.

[0625] Furthermore, the acyl group in cellulose esters can be a single acyl group or a combination of multiple acyl groups.

[0626] In preferred examples of cellulose esters, in addition to cellulose acetate such as diacetylcellulose (DAC) and triacetylcellulose (TAC), mixed fatty acid esters of cellulose such as cellulose acetate propionate (CAP), cellulose acetate butyrate, and cellulose acetate propionate butyrate, which contain propionate or butyrate groups in addition to acetyl groups, can be listed.

[0627] These cellulose esters can be used individually or in combination.

[0628] (Type of acyl group and degree of substitution)

[0629] By adjusting the type and degree of substitution of acyl groups in cellulose esters, the humidity variation of phase difference can be controlled within the required range, thereby improving the uniformity of film thickness.

[0630] The lower the degree of substitution of the acyl group in cellulose ester, the higher the manifestation of phase difference, thus enabling thin film formation.

[0631] On the other hand, if the substitution of the acyl group is too small, the durability may deteriorate and it is not preferred.

[0632] On the other hand, the greater the degree of substitution of the acyl group in the cellulose ester, the less the phase difference will be apparent. Therefore, the stretching ratio must be increased during film formation. However, it is difficult to stretch the film uniformly at a high stretching ratio, thus increasing (worsening) the film thickness deviation.

[0633] Furthermore, the Rt humidity variation, which is a delay (phase difference) in the thickness direction, is caused by water molecules coordinating with the carbonyl group of cellulose. Therefore, the higher the degree of substitution of the acyl group, that is, the more carbonyl groups in the cellulose, the worse the Rt humidity variation tends to be.

[0634] The cellulose ester is preferably in the range of 2.1 to 2.5 degrees of total substitution.

[0635] By setting it to this range, the uniformity of film thickness can be improved while suppressing environmental variations (especially Rt variations caused by humidity).

[0636] More preferably, from the viewpoint of further improving the castability and stretchability during film formation and the uniformity of film thickness, the value is in the range of 2.2 to 2.45.

[0637] More specifically, the cellulose ester satisfies both formulas (a) and (b) below. In formulas (a) and (b) below, X is the degree of substitution of the acetyl group, and Y is the degree of substitution of the propionyl or butyryl group, or a mixture thereof.

[0638] Equation (a): 2.1 ≤ X + Y ≤ 2.5

[0639] Equation (b): 0 ≤ Y ≤ 1.5

[0640] Cellulose esters are more preferably cellulose acetate (Y=0) and cellulose acetate propionate (CAP) (Y: propionyl group, Y>0), and from the perspective of reducing film thickness deviation, cellulose acetate with Y=0 is even more preferred.

[0641] From the perspective of making the phase difference manifestation, Rt humidity variation, and film thickness deviation within the desired range, it is particularly preferred to use cellulose acetate diacetate (DAC) with a content of 2.1≤X≤2.5 (more preferably, 2.15≤X≤2.45).

[0642] In addition, when Y > 0, the cellulose acetate propionate (CAP) used is particularly preferred to have the following properties: 0.95 ≤ X ≤ 2.25, 0.1 ≤ Y ≤ 1.2, and 2.15 ≤ X + Y ≤ 2.45.

[0643] By using the aforementioned cellulose acetate or cellulose acetate propionate, a membrane roll with excellent delay, mechanical strength, and environmental adaptability is obtained.

[0644] Furthermore, the degree of substitution of the acyl group indicates the average number of acyl groups per glucose unit, representing the number of hydrogen atoms of the hydroxyl groups at positions 2, 3, and 6 of a glucose unit that are substituted by acyl groups.

[0645] Therefore, the maximum degree of substitution is 3.0, which means that all the hydrogen atoms of the hydroxyl groups at positions 2, 3, and 6 are replaced by acyl groups.

[0646] These acyl groups can be substituted at the 2, 3, and 6 positions of the glucose unit, or they can be substituted in a distributed manner.

[0647] The degree of substitution was determined using the method specified in ASTM-D817-96.

[0648] To obtain the desired optical properties, cellulose acetate with different degrees of substitution can be mixed.

[0649] In the above cases, there are no particular limitations on the mixing ratio of different cellulose acetates.

[0650] Regarding the number-average molecular weight (Mn) of cellulose esters, if it is 2 × 10⁻⁶ 4 ~3×10 5 Within the range, and further 2×10 4 ~1.2×10 5 Within the range, and further 4×10 4 ~8×10 4 Within the range, the preferred option is selected from the perspective of increasing the mechanical strength of the resulting membrane roll.

[0651] The number-average molecular weight Mn of the cellulose ester was calculated by gel permeation chromatography (GPC) under the above-described determination conditions.

[0652] Regarding the weight-average molecular weight (Mw) of cellulose esters, if it is 2 × 10⁻⁶... 4 ~1×10 6 Within the range, and further 2×10 4 ~1.2×10 5 Within the range, and further 4×10 4 ~8×10 4 Within the range, the preferred option is selected from the perspective of increasing the mechanical strength of the resulting membrane roll.

[0653] There are no particular limitations on the raw material cellulose for cellulose esters; examples include cotton linter, wood pulp, and kenaf.

[0654] Furthermore, the cellulose esters obtained from these can be mixed and used in any proportion.

[0655] Cellulose esters such as cellulose acetate and cellulose acetate propionate can be manufactured using known methods.

[0656] Generally, cellulose raw materials are mixed with specified organic acids (acetic acid, propionic acid, etc.) and acid anhydrides (acetic anhydride, propionic anhydride, etc.) and catalysts (sulfuric acid, etc.) to esterify the cellulose and react until cellulose triesters are produced.

[0657] In the triester, the three hydroxyl groups of the glucose unit are replaced by the acyl groups of the organic acid.

[0658] If two organic acids are used at the same time, it is possible to produce mixed ester-type cellulose esters, such as cellulose acetate propionate and cellulose acetate butyrate.

[0659] Next, cellulose ester resins with the desired degree of acyl substitution are synthesized by hydrolyzing the cellulose triester.

[0660] Then, through processes such as filtration, sedimentation, washing, dehydration, and drying, the cellulose ester resin is completed. Specifically, it can be synthesized according to the method described in Japanese Patent Application Publication No. 10-45804.

[0661] (4.2) Other additives

[0662] In the case of the film rolls involved in this invention, in addition to the thermoplastic resins described above, the following additives may be included as other additives.

[0663] (4.2.1) Plasticizers

[0664] The film rolls involved in this invention, for example, in order to impart processability to polarizer protective films, preferably contain at least one plasticizer.

[0665] Plasticizers are preferably used alone or in combination of two or more.

[0666] From the viewpoint of effectively controlling moisture permeability and compatibility with base resins such as cellulose esters, plasticizers containing at least one selected from sugar esters, polyesters, and styrene compounds are preferred.

[0667] From the viewpoint of balancing improved resistance to damp heat and compatibility with base resins such as cellulose esters, the plasticizer preferably has a molecular weight of 15,000 or less, and more preferably 10,000 or less.

[0668] When the compound with a molecular weight of 10,000 or less is a polymer, it is preferable that the weight-average molecular weight (Mw) is 10,000 or less.

[0669] The preferred range for weight-average molecular weight (Mw) is 100 to 10,000, and more preferably 400 to 8,000.

[0670] In particular, in order to obtain the effects of the present invention, the compound having a molecular weight of less than 1500 is preferably contained in the range of 6 to 40 parts by weight relative to 100 parts by weight of the base resin, and more preferably in the range of 10 to 20 parts by weight.

[0671] It is preferred to contain within the above-mentioned range, thereby achieving both effective control of moisture permeability and compatibility with the substrate resin.

[0672] <Glycoesters>

[0673] In order to prevent hydrolysis, the membrane rolls involved in this invention may contain sugar ester compounds.

[0674] Specifically, as a sugar ester compound, a sugar ester can be used that has at least one pyranose structure or a furanose structure, and all or part of the OH groups of that structure are esterified.

[0675] <Polyester>

[0676] The film rolls involved in this invention may also contain polyester.

[0677] There are no particular limitations on polyesters; polymers with terminal hydroxyl groups (polyester polyols) obtained by condensation reaction of dicarboxylic acids or their ester-forming derivatives with diols, or polymers in which the terminal hydroxyl groups of the polyester polyol are blocked by monocarboxylic acids (terminated polyesters) can be used.

[0678] The ester-forming derivatives mentioned here are esters of dicarboxylic acids, chlorides of dicarboxylic acids, and anhydrides of dicarboxylic acids.

[0679] <Styrene compounds>

[0680] In the membrane rolls involved in this invention, styrene-based compounds may also be used in addition to or in place of the aforementioned sugar esters and polyesters to improve the water resistance of the membrane.

[0681] Styrene compounds can be homopolymers of styrene monomers or copolymers of styrene monomers with other comonomers.

[0682] Regarding the proportion of structural units derived from styrene monomers in styrene compounds, in order to achieve a certain or greater volume in the molecular structure, it is preferably in the range of 30 to 100 mol%, and more preferably in the range of 50 to 100 mol%.

[0683] Examples of styrene monomers include styrene; alkyl-substituted styrene such as α-methylstyrene, β-methylstyrene, and p-methylstyrene; halogen-substituted styrene such as 4-chlorostyrene and 4-bromostyrene; hydroxystyrene such as p-hydroxystyrene, α-methyl-p-hydroxystyrene, 2-methyl-4-hydroxystyrene, and 3,4-dihydroxystyrene; vinylbenzyl alcohols; alkoxy-substituted styrene such as p-methoxystyrene, p-tert-butoxystyrene, and m-tert-butoxystyrene; 3-vinylbenzoic acid, 4-ethyl Vinylbenzoic acids such as alkenylbenzoic acid; 4-vinylbenzyl acetate; 4-acetoxystyrene; acylaminostyrene such as 2-butyrylaminostyrene, 4-formylaminostyrene, and p-sulfonylaminostyrene; aminostyrene such as 3-aminostyrene, 4-aminostyrene, 2-isopropenylaniline, and vinylbenzyldimethylamine; nitrostyrene such as 3-nitrostyrene and 4-nitrostyrene; cyanostylstyrene such as 3-cyanostylstyrene and 4-cyanostylstyrene; vinylphenylacetonitrile; arylstyrene such as phenylstyrene; indene, etc.

[0684] Styrene monomers can be one type or a combination of two or more types.

[0685] (4.2.2) Any component

[0686] The film rolls involved in this invention may contain other optional components such as antioxidants, colorants, ultraviolet absorbers, matting agents, acrylic particles, hydrogen-binding solvents, and ionic surfactants.

[0687] These components can be added in the range of 0.01 to 20 parts by weight relative to 100 parts by weight of the base resin.

[0688] (Antioxidants)

[0689] The film rolls involved in this invention can use commonly known antioxidants as antioxidants.

[0690] In particular, compounds of lactone, sulfur, phenol, double bond, hindered amine, and phosphorus types can be preferentially used.

[0691] Regarding these antioxidants, they are added in the range of 0.05 to 20% by mass, preferably 0.1 to 1% by mass, relative to the resin, which is the main raw material of the membrane.

[0692] These antioxidants, compared to using only one type, can achieve a synergistic effect by using several different systems of compounds together.

[0693] For example, a combination of lactone-based, phosphorus-based, phenolic, and double-bond-based compounds is preferred.

[0694] (Coloring agent)

[0695] With respect to the film rolls involved in this invention, colorants are preferably included to adjust the hue, without impairing the effects of the invention.

[0696] The term "colorant" refers to dyes and pigments. In this invention, it refers to a colorant that has the effect of making the hue of the liquid crystal display screen cyan or adjusting the yellow index and reducing haze.

[0697] As a coloring agent, it can be used with various dyes and pigments, such as anthraquinone dyes, azo dyes, and phthalocyanine pigments.

[0698] (UV absorber)

[0699] Since the film roll involved in this invention can also be used on the visible side and backlight side of a polarizer, it may contain an ultraviolet absorber in order to impart ultraviolet absorption function.

[0700] There are no particular limitations on what constitutes a UV absorber; examples include benzotriazole, 2-hydroxybenzophenone, and phenyl salicylate UV absorbers.

[0701] Examples of triazoles include 2-(5-methyl-2-hydroxyphenyl)benzotriazole, 2-[2-hydroxy-3,5-bis(α,α-dimethylbenzyl)phenyl]-2H-benzotriazole, 2-(3,5-di-tert-butyl-2-hydroxyphenyl)benzotriazole, and benzophenones include 2-hydroxy-4-methoxybenzophenone, 2-hydroxy-4-octoxybenzophenone, and 2,2'-dihydroxy-4-methoxybenzophenone.

[0702] The aforementioned ultraviolet absorbers can be used alone or in combination of two or more.

[0703] The amount of ultraviolet absorber used varies depending on the type of ultraviolet absorber and the conditions of use. Generally, it is added in the range of 0.05% to 10% by mass, preferably 0.1% to 5% by mass, relative to the base resin.

[0704] (particle)

[0705] With regard to the membrane rolls involved in this invention, it is preferable to add microparticles that impart slip properties to the membrane rolls.

[0706] In particular, from the viewpoint of improving the slipperiness of the film surface involved in this invention, improving slipperiness during winding, preventing damage and adhesion, the addition of microparticles is effective.

[0707] As for the microparticles, either inorganic or organic microparticles are acceptable, provided that they have heat resistance during melting without compromising the transparency of the resulting film roll, but inorganic microparticles are preferred.

[0708] These particles can be used alone or in combination of two or more.

[0709] By using particles with different sizes and shapes (such as needle-like and spherical), it is also possible to achieve a high degree of both transparency and slipperiness.

[0710] Among the compounds constituting the above-mentioned particles, silica, which has excellent transparency (haze) due to its refractive index being close to that of the cyclic olefin resins, acrylic resins, and cellulose ester resins, is particularly preferred.

[0711] As specific examples of silica, commercially available products with trade names such as AEROSIL (registered trademark) 200V, AEROSIL (registered trademark) R972V, AEROSIL (registered trademark) R972, R974, R812, 200, 300, R202, OX50, TT600, NAX50 (all manufactured by AEROSIL Corporation of Japan), SEAHOSTAR (registered trademark) KEP-10, SEAHOSTAR (registered trademark) KEP-30, SEAHOSTAR (registered trademark) KEP-50 (all manufactured by Nippon Shokubai Co., Ltd.), SYLOPHOBIC (registered trademark) 100 (manufactured by Fuji Silicon Chemical Co., Ltd.), Nipsi l (registered trademark) E220A (manufactured by Nippon Silica Industry Co., Ltd.), and ADMAFINE (registered trademark) SO (manufactured by Yaduma Co., Ltd.) are preferred.

[0712] As for the shape of the particles, there are no particular restrictions on using amorphous, needle-shaped, flat, spherical, etc. In particular, if spherical particles are used, the resulting film roll has good transparency, so it is preferred.

[0713] If the size of the particles is close to the wavelength of visible light, light scattering will occur and transparency will decrease. Therefore, it is preferable that the particle size is smaller than the wavelength of visible light, and more preferably less than half the wavelength of visible light.

[0714] If the particle size is too small, it may not improve the sliding properties, so a size of 80 to 180 nm is particularly preferred.

[0715] Furthermore, the size of a particle, in the case of a condensation of primary particles, refers to the size of the condensation.

[0716] In addition, when the particle is not spherical, it refers to the diameter of a circle whose projected area is equivalent to that of the particle.

[0717] Regarding the microparticles, they are preferably added in the range of 0.05 to 10% by mass, and more preferably in the range of 0.1 to 5% by mass, relative to the base resin.

[0718] (Applications of membranes)

[0719] The film fed from the film roll of the present invention is used as an optical film, preferably as a protective film for polarizers, and can be used in various optical measuring devices and display devices such as liquid crystal display devices and organic electroluminescent display devices.

[0720] Example

[0721] The present invention will be specifically described below with reference to specific embodiments, but the present invention is not limited thereto. Furthermore, the use of the terms "parts" or "%" in the embodiments, unless otherwise specified, indicates "parts by mass" or "% by mass".

[0722] [Made with membrane rolls]

[0723] (The making of membrane roll No. 1)

[0724] Solution casting is used in membrane fabrication.

[0725] <Membrane Formation Process (S1)>

[0726] (Preparation of adhesive paste)

[0727] <Synthesis of Cyclic Polyolefin Polymer (P-1)>

[0728] 100 parts by weight of refined toluene and 100 parts by weight of methyl norborneol carboxylate were added to the stirring device.

[0729] Next, 25 mmol% (relative to monomer mass) of ethyl hexanoate-Ni dissolved in toluene, 0.225 mol% (relative to monomer mass) of tri(pentafluorophenyl)boron, and 0.25 mol% (relative to monomer mass) of triethylaluminum dissolved in toluene were added to the stirring apparatus.

[0730] React at room temperature with stirring for 18 hours.

[0731] After the reaction is complete, excess ethanol is added to the reaction mixture to form a polymer precipitate.

[0732] The cyclic polyolefin polymer (P-1) obtained by precipitation purification was dried under vacuum at 65°C for 24 hours.

[0733] <Preparation of the adhesive (D-1)>

[0734] The following composition 1 is added to a mixing tank and stirred to dissolve the components. The mixture is then filtered through filter paper with an average pore size of 34 μm and a sintered metal filter with an average pore size of 10 μm to prepare a paste (D-1).

[0735] (Composition 1)

[0736] Cyclic polyolefin polymer (P-1) 150 parts by weight

[0737] 380 parts by weight of dichloromethane

[0738] 70 parts by weight of methanol

[0739] Next, the following (composition 2), which contains the cyclic polyolefin solution (gel (D-1)) prepared by the above method, is fed into a disperser as an additive to prepare a particulate dispersion (M-1).

[0740] (Composition 2)

[0741]

[0742] Mix 100 parts by weight of the above cyclic polyolefin solution (D-1) and 0.75 parts by weight of the particulate dispersion (M-1) to prepare a film-forming paste (resin composition cyclic olefin resin COP1).

[0743] (Spraying of adhesive)

[0744] The prepared film-forming paste (resin composition cycloolefin resin COP1) is delivered to the casting die via a conduit using a pressurized quantitative gear pump. The paste is then cast from the casting die at a casting position on a support consisting of an infinitely moving rotating stainless steel annular belt, with a width of 1800 mm. The paste is heated on the support until it becomes self-supporting. The solvent is evaporated until the cast film can be peeled off from the support using a peeling roller, thereby drying to form a film.

[0745] The conditions for casting the above-mentioned adhesive are as follows.

[0746] <condition>

[0747] Set the length of the piping from the pump to the casting die to be 60m, and adjust the gear ratio of the gear pump used for dispensing the adhesive to make the pump's rotation speed 20rpm.

[0748] The width of the slit for discharging the adhesive paste is adjusted by using the hot bolts of the casting die to ensure that the thickness deviation of the film immediately after discharge is 1.5% relative to the overall cast film thickness, thus controlling the initial discharge thickness of the cast film.

[0749] The film is made by drying until the residual solvent content of the cast film on the belt reaches 200% by mass. After the film is formed on the surface, warm air at a speed of 16 m / s (40°C) is sprayed to flatten the protrusions.

[0750] (Membrane peeling)

[0751] After the film is formed, it is peeled off from the support in a self-supporting state by a peeling roller.

[0752] (Shrinkage within the membrane surface)

[0753] The membrane is subjected to high-temperature treatment without maintaining its width to increase its density, thereby causing the membrane to shrink in the width direction at a shrinkage rate of 7%.

[0754] (Membrane drying)

[0755] Then, the membrane is heated on a support to evaporate the solvent.

[0756] The residual solvent content of the membrane was determined using the following method, and the result was less than 5% by mass.

[0757] (Determination of residual solvent content)

[0758] Regarding the amount of residual solvent, gas chromatography was used for quality analysis as described below.

[0759] That is, take any membrane from any location, and to prevent the evaporation of residual solvent in the membrane, quickly ensure that a stopper is placed on the vial.

[0760] Next, a needle was inserted into the vial, and quality analysis was performed using gas chromatography (manufactured by Agilent Technologies, Inc.).

[0761] It should be noted that the amount of residual solvent is defined by the following formula.

[0762] Residual solvent content (mass%) = {(MN) / N} × 100

[0763] Furthermore, M in the above formula represents the mass (g) of the sample taken at any time during or after the manufacture of the cast film or film, and N in the above formula represents the mass (g) of the sample after heating it at 115°C for 1 hour.

[0764] <Protrusion Adjustment Process (S2)>

[0765] (Membrane stretching)

[0766] Then, the membrane is transported in the stretching device, and while the membrane is locally heated, it is stretched laterally.

[0767] (Local heating method)

[0768] Infrared (IR) heaters are used as a localized heating method.

[0769] Regarding the position of the heat source of each infrared heater on the membrane, it is positioned at a distance of 75 mm from the membrane surface.

[0770] In addition, the heating width is set to 150mm (when the intensity directly below the infrared heater is set to 1, the heating width becomes 0.2).

[0771] Each heat source part of the infrared heater is set within the range of 180 to 350°C at a rated power of 750W.

[0772] (Infrared heater arrangement and heat source unit spacing)

[0773] Infrared heaters, such as Figure 6B As shown, they are arranged in two columns along the length direction, with the heat source parts of each infrared heater set at a spacing of 30mm.

[0774] (Connecting to heat source section E) A and E B The average angle of inclination θ of a straight line relative to its length direction. E ′)

[0775] To configure each heat source unit E A and E B The average angle of inclination θ between the connecting line and the line forming the length direction. E The infrared heater is set to 5.7°.

[0776] (The heat ratio (B / A) of the heat A in the central part of the infrared (IR) heater to the average heat B at the ends of the infrared (IR) heater) heater)

[0777] The heat ratio (B / A) of the heat A in the central part of the infrared (IR) heater to the average heat B at the end of the infrared (IR) heater is 0.2.

[0778] In addition, at this time, the online delay film thickness measuring device RE-200L2T-Rth+ film thickness (manufactured by Otsuka Electronics Co., Ltd.) is used to measure the film thickness profile in the width direction of the target film. The difference between the film thickness profile and the target film thickness profile is used to calculate the set temperature of each infrared heater on the computer. The set temperature of each heat source is output via PLC KV-8000 (manufactured by KEYENCE Co., Ltd.). The protrusion is adjusted, and the film thickness is automatically and repeatedly adjusted automatically.

[0779] (Maximum height difference (PV) of average film thickness at various width positions)

[0780] Simultaneously with the above operations, the maximum height difference (PV) of the average film thickness at each width position is controlled to make it conform to the value in Table I (film thickness control is performed using the above operations; the measurement method will be described later).

[0781] <Finishing Process (S3)>

[0782] Cut (trim) both ends of the stretched membrane in the width direction.

[0783] (Presence or absence of vibration)

[0784] Furthermore, the membrane should not be vibrated during the repair process.

[0785] (Is knurling present or absent?)

[0786] Then, do not perform knurling on the film.

[0787] <Winding process (S4)>

[0788] Roll up the above-mentioned film.

[0789] The procedure was carried out with an initial tension of 50 N, a taper of 70%, and a corner angle of 25%.

[0790] The procedure was carried out with a membrane roll width of 2000 mm and a roll length of 3900 m.

[0791] The linear speed of the transport membrane was set to 60 m / min.

[0792] The above procedures are used to produce membrane roll No. 1.

[0793] (Confirmation of the surface properties of the film related to the protrusion)

[0794] Immediately before the winding process after finishing, the number and height of the protrusions were measured as film characteristics related to the protrusions, and the continuity of the protrusions was confirmed.

[0795] In addition, the absolute value of the tilt angle of an approximate straight line relative to the length direction of the membrane surface is measured.

[0796] The following describes the method for confirming continuity.

[0797] Methods for confirming continuity

[0798] As a method to confirm the continuity of the protrusion, specifically, the data measured by the online delay film thickness measuring device RE-200L2T-Rth+ film thickness (manufactured by Otsuka Electronics Co., Ltd.) was displayed on a computer in the form of a heat map (horizontal axis: film width position, vertical axis: film length position, depth: film thickness value), thus confirming the continuity of the protrusion.

[0799] exist Figure 14 The image shows an example of a heatmap used for actual verification.

[0800] Furthermore, Figure 14 For equivalent to Figure 4A An example of the actual heat map of the continuity of the convex part is an example of the representation of "straight line" in Table I.

[0801] (Production of membrane rolls No. 2-4)

[0802] In the <convex part preparation process (S2)>, the maximum height difference (PV) of the average film thickness at each width position is controlled to become the value in Table I. Otherwise, film rolls No.2 to No.4 are made in the same way as film roll No.1.

[0803] (The making of membrane roll No. 5)

[0804] Solution casting is used in membrane fabrication.

[0805] In the <film formation process (S1)> and <protrusion preparation process (S2)>, the same operations as for film roll No.1 are performed.

[0806] <Finishing Process (S3)>

[0807] Cut (trim) both ends of the stretched membrane in the width direction.

[0808] (Presence or absence of vibration)

[0809] Furthermore, the membrane should not be vibrated during the repair process.

[0810] (Is knurling present or absent?)

[0811] Then, the membrane is knurled to a height of 1 μm.

[0812] The details are shown below.

[0813] Laser is used to irradiate the film after the <Trimping Process (S3)> to form a knurled section.

[0814] The knurling width at both ends of the membrane is 15mm from the membrane end.

[0815] The linear speed of the transport membrane was set to 60 m / min.

[0816] As a laser device, a carbon dioxide laser device is used, the output of the laser device is set to 20W, the center wavelength of the emitted light is set to 9.4μm, and the range of the emitted light wavelength is set to within ±0.01μm of the center wavelength.

[0817] Regarding the irradiation of the membrane by laser, the parallel beam emitted from the carbon dioxide laser device is reflected by two galvanometer mirrors, and then focused on the surface of the transported membrane by an fθ lens (focal distance 200mm).

[0818] By controlling the angle of the galvanometer's reflector, the light-collecting position can be moved in the direction of the membrane plane, thereby controlling the trajectory of the laser irradiation on the membrane surface.

[0819] Atmospheric Pressure Plasma Treatment Process: Surface Modification Treatment

[0820] Kasuga Electric Machinery AGP-500 was placed on the back side of the knurling section of the optical film and irradiated with 0.5kW.

[0821] The experiment was conducted with a probe emitting atmospheric pressure plasma at a distance of 5 mm from the membrane.

[0822] The atmospheric pressure plasma is positioned on the back side of the film opposite the knurling section, in a way that it can irradiate 110% of the width of the knurling process.

[0823] <Winding process (S4)>

[0824] Roll up the above-mentioned film.

[0825] It was carried out with an initial tension of 50 N, a taper of 70%, and a corner angle of 25%.

[0826] The procedure was carried out with a membrane roll width of 2000 mm and a roll length of 3900 m.

[0827] The linear speed of the transport membrane was set to 60 m / min.

[0828] The above procedures are used to produce membrane roll No. 5.

[0829] (The making of membrane roll No. 6)

[0830] In the preparation of the adhesive in the <film forming process (S1)>, triacetyl cellulose (TAC) is used as the resin composition instead of COP1. In the <trimming process (S3)>, the membrane is knurled to a height of 2μm. Otherwise, membrane roll No.6 is made using the same steps as membrane roll No.5.

[0831] (The making of membrane roll No. 7)

[0832] In the <convex part preparation process (S2)>, the heat ratio (B / A) of the heat A in the central part of the infrared (IR) heater to the average heat B at the end of the infrared (IR) heater is 0.6. Otherwise, the same steps as for membrane roll No.5 are used to make membrane roll No.7.

[0833] (The making of membrane roll No. 8)

[0834] In the <convex part preparation process (S2)>, the heat ratio (B / A) of the heat A in the central part of the infrared (IR) heater to the average heat B at the end of the infrared (IR) heater is 0.1. Otherwise, membrane roll No.8 is made in the same way as membrane roll No.5.

[0835] (The making of membrane roll No. 9)

[0836] In the <convex part preparation process (S2)>, the infrared heater is as follows: Figure 6C As shown, five columns are arranged along the length direction, with the heat source sections of each infrared heater spaced 10mm apart; this allows for connection between the various heat source sections E. A and E B The infrared heater is set such that the average tilt angle between the straight line and the length direction is 2.0°; the heat ratio (B / A) of the heat A in the central part of the infrared (IR) heater and the average heat B at the end of the infrared (IR) heater is 0.1. Otherwise, membrane roll No. 9 is made in the same manner as membrane roll No. 5.

[0837] (The making of membrane roll No. 10)

[0838] In the <convex part preparation process (S2)>, the heat ratio (B / A) of the heat A in the central part of the infrared (IR) heater to the average heat B at the end of the infrared (IR) heater is 0.9. Otherwise, membrane roll No.10 is made in the same way as membrane roll No.5.

[0839] (Production of membrane rolls No. 11-15)

[0840] In the <convex part preparation process (S2)>, the infrared heater is as follows: Figure 6A As shown, they are arranged in one column along the length direction, with the heat source sections of each infrared heater spaced 125mm apart; the configured heat source sections E A and E B The average angle of inclination of the connecting straight line and the straight line formed by the length direction was not calculated because the infrared heaters were arranged in a single column in the length direction; the heat ratio (B / A) of the heat A in the central part of the infrared (IR) heater to the average heat B at the end of the infrared (IR) heater was 0.9; in the (confirmation of the surface characteristics of the membrane related to the protrusion), the absolute value of the angle of inclination of the approximate straight line with respect to the length direction of the membrane surface was set to the value recorded in Table I, and otherwise, membrane rolls No. 11 to 15 were manufactured in the same manner as membrane roll No. 5.

[0841] (The making of membrane roll No. 16)

[0842] In (confirmation of the surface properties of the membrane related to the protrusion), the continuity of the protrusion is adjusted to draw a trajectory of a curve with a curvature that changes at approximately a certain rate of change. Otherwise, membrane roll No. 16 is made in the same manner as membrane roll No. 11.

[0843] Furthermore, by adjusting the continuity of the aforementioned protrusions to draw a trajectory of a curve with curvature that changes at approximately a certain rate of change, the absolute value of the inclination angle relative to the approximate straight line along the length direction of the membrane surface was not calculated.

[0844] (The production of membrane rolls No. 17 and 18)

[0845] Vibration is performed at an amplitude of 100 mm in the <Trimping Process (S3)>; the height of the protrusion is adjusted in (confirmation of the surface characteristics of the membrane related to the protrusion) to make it the value recorded in Table I. Otherwise, membrane rolls No. 17 and 18 are made in the same manner as membrane roll No. 16.

[0846] (The production of membrane rolls No. 19 and 20)

[0847] Vibration is performed at an amplitude of 100 mm in the <Trimping Process (S3)>; the number of protrusions is adjusted in (confirmation of the surface characteristics of the membrane related to the protrusions) to make it the value recorded in Table I. Otherwise, membrane rolls No. 19 and 20 are made in the same manner as membrane roll No. 16.

[0848] (The making of membrane roll No. 21)

[0849] Vibration is performed at an amplitude of 100mm in the <Treading Process (S3)>. Otherwise, membrane roll No. 21 is manufactured in the same manner as membrane roll No. 16.

[0850] (The making of membrane roll No. 22)

[0851] In the <convex part preparation process (S2)>, hot air is used for local heating; in the <trimming process (S3)>, vibration is performed at an amplitude of 100 mm. Otherwise, membrane roll No. 22 is made in the same manner as membrane roll No. 16.

[0852] (The making of membrane roll No. 23)

[0853] The melt casting method is used in the film fabrication process.

[0854] <Membrane Formation Process (S1)>

[0855] (Melted extrusion of resin)

[0856] The resin (resin composition cycloolefin resin COP2) was prepared using the same steps as for film roll No.1. The granulated granules and additives (microparticles (AEROSILR812: manufactured by AEROSIL Co., Ltd. of Japan, primary average particle size: 7nm, apparent specific gravity 50g / L)) were fed to the extruder, melted in the extruder, and extruded into a film from the casting die on the casting drum through a pressure-type quantitative gear pump.

[0857] (Casting and molding of molten resin granules)

[0858] In the above extrusion process, the length of the piping from the pump to the casting die is 60m, and the gear ratio of the gear pump used for liquid delivery is adjusted so that the pump rotation speed is 20rpm.

[0859] By using the hot bolts of the casting die to adjust the gap of the slit for discharging the adhesive, the film thickness deviation immediately after discharge is adjusted to 1.5% relative to the overall cast film, thus controlling the initial discharge film thickness of the cast film.

[0860] After drying the film until the residual solvent content of the cast film on the tape is 5% by mass, a coating is formed on the surface, and then warm air at 45 m / s (40°C) is sprayed to flatten the protrusions.

[0861] The extruded resin is cooled by a cooling drum, thus forming a film.

[0862] <Protrusion preparation process (S2)>

[0863] (Membrane stretching)

[0864] Then, the membrane is transported in the stretching device, and while the membrane is locally heated, it is stretched laterally.

[0865] (Local heating method)

[0866] Infrared (IR) heaters are used as a localized heating method.

[0867] Regarding the position of the heat source of each infrared heater on the membrane, it is positioned at a distance of 75 mm from the membrane surface.

[0868] In addition, the heating width is set to 150mm (the heating width with an intensity of 0.2 when the intensity directly below the infrared heater is set to 1).

[0869] Each heat source part of the infrared heater is set within the range of 180 to 350°C at a rated power of 750W.

[0870] (Infrared heater arrangement and heat source unit spacing)

[0871] Infrared heaters, such as Figure 6A As shown, they are arranged in a single column along the length, with the heat source sections of each infrared heater spaced 125mm apart.

[0872] (Connecting to heat source section E) A and E B The average angle of inclination θ of a straight line relative to its length direction. E ′)

[0873] Configure each heat source section E A and E BThe average angle of inclination of the line connecting the two lines and the line forming the length direction was not calculated because the infrared heaters were arranged in a single column along the length direction.

[0874] (The heat ratio (B / A) of the heat A in the central part of the infrared (IR) heater to the average heat B at the ends of the infrared (IR) heater) heater)

[0875] The heat ratio (B / A) of the heat A in the central part of the infrared (IR) heater to the average heat B at the end of the infrared (IR) heater is 0.9.

[0876] In addition, at this time, the online delay film thickness measuring device RE-200L2T-Rth+ film thickness (manufactured by Otsuka Electronics Co., Ltd.) is used to measure the film thickness profile in the width direction of the target film. The difference between the film thickness profile and the target film thickness profile is used to calculate the set temperature of each infrared heater on the computer. The set temperature of each heat source is output via PLC KV-8000 (manufactured by KEYENCE Co., Ltd.). The protrusion is adjusted, and the film thickness is automatically and repeatedly adjusted automatically.

[0877] (Maximum height difference (PV) of average film thickness at various width positions)

[0878] Simultaneously with the above operations, the maximum height difference (PV) of the average film thickness at each width position is controlled to make it conform to the value in Table I (film thickness control is performed using the above operations; the measurement method will be described later).

[0879] <Finishing Process (S3)>

[0880] Cut (trim) both ends of the stretched membrane in the width direction.

[0881] (Presence or absence of vibration)

[0882] Furthermore, during the adjustment process, the membrane is vibrated with an amplitude of 100mm.

[0883] (Is knurling present or absent?)

[0884] Then, the membrane is knurled to a height of 1 μm.

[0885] Furthermore, the same knurling process is performed as with film roll No. 5.

[0886] <Winding process (S4)>

[0887] Roll up the above-mentioned film.

[0888] The procedure was carried out with an initial tension of 50 N, a taper of 70%, and a corner angle of 25%.

[0889] The procedure was carried out with a membrane roll width of 2000 mm and a roll length of 3900 m.

[0890] The linear speed of the transport membrane was set to 60 m / min.

[0891] The above procedures were used to produce membrane roll No. 23.

[0892] (Confirmation of the surface properties of the film related to the protrusion)

[0893] As described above, immediately before the winding process after finishing, the number and height of the protrusions were measured as film characteristics related to the protrusions, and the continuity of the protrusions was confirmed.

[0894] In addition, the absolute value of the tilt angle of an approximate straight line relative to the length direction of the membrane surface is measured.

[0895] (Production of membrane rolls No. 24-27)

[0896] In the <convex part preparation process (S2)>, the infrared heater is as follows: Figure 6A As shown, they are arranged in one column along the length direction, with the heat source sections of each infrared heater spaced 125mm apart; the configured heat source sections E A and E B The average tilt angle of the connecting straight line and the straight line formed by the length direction was not calculated because the infrared heaters were arranged in a row along the length direction; the heat ratio (B / A) of the heat A in the central part of the infrared (IR) heater to the average heat B at the end of the infrared (IR) heater was 0.9; vibration was performed at an amplitude of 100 mm in the <trimming process (S3); in the (confirmation of the surface characteristics of the membrane related to the protrusions) the number of protrusions, the height of the protrusions, the continuity of the protrusions, the absolute value of the tilt angle of the approximate straight line of the length direction relative to the membrane surface, and the maximum height difference (PV) between the approximate straight line tilt angle of the protrusions and the average membrane thickness at each width position were set to the values ​​recorded in Table I. Otherwise, membrane rolls No. 24 to 27 were manufactured in the same manner as membrane roll No. 5.

[0897] (The making of membrane roll No. 28)

[0898] The (local heating method) in the <convex part preparation process (S2)> was not used; the values ​​of the surface properties of the membrane related to the convex part were controlled as shown in Table I. Otherwise, membrane roll No. 28 was made in the same manner as membrane roll No. 24.

[0899] (Examples and Comparative Examples)

[0900] Using film rolls No. 1 to 23 as examples and film rolls No. 24 to 28 as comparative examples, the following evaluation was conducted.

[0901] The measured values ​​and evaluations related to membrane rolls No. 1 to 28 are summarized in Table I.

[0902] [Table I]

[0903]

[0904] [Various measurements and evaluations]

[0905] The following shows the methods for measuring, calculating, and evaluating the outer diameter and other characteristics of the various membrane rolls mentioned above.

[0906] A. Maximum vertical variation (PV) of average film thickness at various width locations.

[0907] (Determination Method)

[0908] The measurement of the maximum height difference (PV) of the average film thickness at each width position in the direction inclined relative to the width direction of the film, measured in the order of steps 1 to 3 below, was carried out by measuring 30,000 points using an online delayed film thickness measuring device RE-200L2T-Rth+ film thickness (manufactured by Otsuka Electronics Co., Ltd.).

[0909] Furthermore, the timing of the measurement is set to immediately before the winding process at room temperature in all processes of solution casting and melt casting.

[0910] At this time, the lateral movement speed is 100 mm / s.

[0911] Furthermore, the data used in step 3 to calculate the length-average film thickness is based on measurements taken at 30,000 locations.

[0912] Step 1:

[0913] After measuring the film thickness at any position at the end of the membrane, the film thickness is measured at a position 10 mm away in the width direction and 30 mm away in the length direction at each measurement. The width position, length position, and film thickness value are recorded, and this process is repeated until the end of another membrane is reached.

[0914] Step 2:

[0915] After step 1 is completed, perform the same measurements as in step 1 until the total distance of the movement along the length direction reaches 1000m.

[0916] Step 3:

[0917] Based on the large amount of film thickness data obtained from steps 1 and 2 above, the film thickness values ​​at the same width position are averaged to calculate the length-average film thickness value at each width position. From this, the height difference (PV) between the maximum and minimum values ​​is calculated.

[0918] B. Orientation Angle

[0919] (Determination Method)

[0920] Using the online delay film thickness measurement device RE-200L2T-Rth+ film thickness (manufactured by Otsuka Electronics Co., Ltd.), the optical value (orientation angle) of the film was measured at the end of the film in the width direction (for example, from the position 15 mm inside the widest end) and in the length direction of the film with a sampling period of 50 milliseconds.

[0921] Regarding the measurement position (the setting position of the measurement device), it is set in such a way that the film length is 100m from the end of the film (winding position).

[0922] Then, the variation in orientation angle in the length direction is evaluated based on the following evaluation criteria.

[0923] Furthermore, the angle of the hysteresis axis of the molecules in the membrane relative to the membrane length direction (film forming direction, transport direction) is set as the orientation angle θ.

[0924] In addition, the so-called "orientation angle variation" refers to the standard deviation (σ) of the measured orientation angle.

[0925] (Evaluation Criteria)

[0926] ◎: The orientation angle varies within the range of 0 to 0.10° over a length of 3000m.

[0927] ○: The orientation angle variation over a length of 3000m is greater than 0.10° but less than 0.12°.

[0928] ×: The orientation angle variation over a length of 3000m is greater than 0.12°.

[0929] Furthermore, the phrase "the orientation angle variation within a 3000m length direction is within the range of 0 to 0.10°" means that when the orientation angle θ at the width end of the membrane is measured at a period of 50 milliseconds along the length direction of 3000m (at this time, the measurement points of the orientation angle at the width end are arranged in the length direction of the membrane at a spacing corresponding to the 50 millisecond period), the variation range of all data of the orientation angle θ converges within the range of 0 to 0.10°.

[0930] Therefore, the closer the evaluation is to ◎, the narrower the range of the orientation angle θ (the smaller the variation in the value of the orientation angle θ), and the smaller the deviation of the orientation angle in the length direction.

[0931] C. Chain Evaluation

[0932] (Evaluation Method)

[0933] After the membrane rolls obtained using the examples and comparative examples were rolled up, they were left to stand for 15 minutes in an environment of 23°C and 55% humidity. The presence of chain-like deformation on the outermost layer of the membrane roll was then visually confirmed.

[0934] Then, the chain-like deformation is evaluated based on the following evaluation criteria.

[0935] (Evaluation Criteria)

[0936] Good: No deformation confirmed.

[0937] Yes: It is confirmed that there is a slight deformation, but since it is elastic deformation, there is no problem in practical use.

[0938] Defect: Confirmed to have more than one chain-like deformation that is problematic in practical use.

[0939] D. Abrasion assessment

[0940] (Evaluation Method)

[0941] The appearance of abrasions on the membrane rolls obtained in the examples and the comparative examples was visually observed, and evaluated according to the following evaluation criteria.

[0942] It should be noted that sometimes even without any noticeable winding misalignment, slight scratches can be detected.

[0943] This is caused by membrane friction (mutual friction) within the membrane roll, and the scratches in this case are equivalent to "○" in the evaluation below.

[0944] (Evaluation Criteria)

[0945] ◎: Almost no scratches were found on the membrane.

[0946] ○: Slight scratches were found on the film, but there were no problems with the product.

[0947] ×: Numerous scratches were found on the membrane, indicating a problem with the work-in-process.

[0948] (Summarize)

[0949] Based on the above description, the various performance evaluations of the embodiments and comparative examples are compared in Table I, and it can be seen that the embodiments are superior overall.

[0950] Industrial availability

[0951] A method for manufacturing film rolls suitable for wide-width film processing and a protrusion adjustment system for use in the manufacturing of film rolls that can prevent roll-shaped defects and minimize orientation angle variations are provided.

[0952] Explanation of reference numerals in the attached figures

[0953] 1.1a Agitator (Agitator Tank)

[0954] 2 Casting die

[0955] 3. Support body (annular belt, rotating drum)

[0956] Rollers 3a and 3b

[0957] 4. Peeling rollers

[0958] 5 Cast film

[0959] 6. Drying device

[0960] 7. Tensioning devices (stretching devices, tilting devices)

[0961] 8. Cutting section

[0962] 10 Cutting section

[0963] 11. Drying device

[0964] 12 Cutting section

[0965] 13. Winding device

[0966] 14 Extruder

[0967] 15 Casting die head

[0968] 16 Casting drum and support body

[0969] 16a Touch Roller

[0970] 17 Cooling Drum

[0971] 19. Tensioning device (tenting and stretching device)

[0972] 20 Cutting section

[0973] 23 Winding device

[0974] 30 membrane rolls

[0975] 31 membrane

[0976] 32 rolls

[0977] 33 Touch Rollers

[0978] 40 Tensioning device (stretching device)

[0979] 42 Fixtures

[0980] 46 masks

[0981] 48. Ring chain

[0982] 50 drive sprocket

[0983] 52 Driven sprocket

[0984] 54 orbits

[0985] 56 Open Components

[0986] 80 Temperature Distribution Sensor

[0987] 101 Nozzle fixing part

[0988] 102 Nozzle

[0989] 103 Cast Film

[0990] 104 End nozzle

[0991] 105 Central Nozzle

[0992] 106 Fixture Cover

[0993] A portion of the end of a membrane roll

[0994] B. A portion of the knurled, uneven shape.

[0995] C. Paste portion in the width direction

[0996] D. Pasted portion along the length direction

[0997] F membrane

[0998] H A H B Width

[0999] Q Infrared (IR) heater

[1000] h convex height

[1001] E A E B Heat source section

[1002] θ′ is the angle of inclination relative to an approximate straight line along the length direction of the membrane surface.

[1003] θ E Heat source section E A and E B The average angle of inclination of the connecting lines relative to the length direction of the line.

[1004] The spacing between the heat source sections of each infrared heater (P1, P2, P3) is as follows:

Claims

1. A method for manufacturing a film roll by a solution or melt casting method, characterized by, At least have: Membrane formation process The process of adjusting the protrusions in the width direction of the membrane surface, The trimming process at both ends of the membrane, and The winding process of the film after the trimming process. The protrusion adjustment process involves adjusting the number, height, and position of the protrusions. This is achieved by applying localized heating to the membrane, ensuring the number of protrusions is between 1 and 10 per 1m in the width direction, and the height of the protrusions is between 0.05 and 0.50 μm. The position of the protrusions is then adjusted to allow continuous movement along the length direction of the membrane surface. The protrusion is a portion whose film thickness profile in the width direction is thicker than the average film thickness, and which is continuously greater than 50 mm in the width direction. When connecting the positions of the protrusions to each other, draw a roughly straight line or a trajectory with a curve having a curvature that changes at a roughly constant rate of change. When this approximate straight line is used as an approximate straight line obtained by the least squares method, the absolute value of the correlation coefficient of the linear expression representing this approximate straight line is 0.8 or greater, and the approximate straight line has an angle of inclination. The rate of change is roughly a certain percentage within the range of ±10% of the average value.

2. The method of manufacturing a film roll according to claim 1, characterized by, During the trimming process, the membrane is not vibrated in the width direction before trimming the two ends of the membrane.

3. The method of manufacturing a film roll according to claim 1 or 2, characterized in that, In the protrusion adjustment process, the position of the protrusion is adjusted by locally heating the membrane so that it is arranged in a generally straight line along the length direction of the membrane surface, and the absolute value of the tilt angle of the generally straight line with respect to the length direction of the membrane surface is in the range of 0.01 to 0.6°.

4. The method of manufacturing a film roll according to claim 1 or 2, characterized by The local heating is performed using infrared heaters arranged in the width direction and the length direction of the film, the heat source portions of the infrared heaters are arranged at intervals of 10 to 100 mm in the width direction of the film, and the heat source portions are arranged at positions different from the width positions in the length direction of the film, each of the arranged heat source portions E A and E B The average inclination angle θ of the connected straight lines E is in the range of 2 to 45° with respect to the length direction.

5. The method of manufacturing a film roll according to claim 4, characterized by The average value of the heat A in the central part of the infrared heater and the heat B at the end of the infrared heater satisfies the following formula (1). Equation (1): 0.2 < (B / A) < 0.

6.

6. The method of manufacturing a film roll according to claim 1 or 2, characterized by, After the finishing process, the membrane was not knurled.

7. The method for manufacturing a film roll according to claim 1 or 2, characterized in that, The maximum height difference (PV) of the average film thickness at each width position, measured in the order of steps 1 to 3 below, in a direction inclined relative to the width direction of the film, is within the range of 0.02 to 0.40 μm. Step 1: After measuring the film thickness at any position at the end of the membrane, at each measurement, the film thickness is measured at a position moved 10 mm in the width direction and 30 mm in the length direction from the arbitrary position. The width position, length position, and film thickness value are recorded. This process is repeated until the other end of the membrane is reached. Step 2: After step 1 is completed, the same measurements as in step 1 are performed until the total distance of the movement along the length direction reaches 1000m. Step 3: Based on the large amount of film thickness data obtained from steps 1 and 2, the film thickness values ​​at the same width position are averaged to obtain the average film thickness value at each width position, and the height difference (PV) between the largest and smallest values ​​is calculated from them.

8. A protrusion adjustment system for implementing the film roll manufacturing method of claim 1, which is a protrusion adjustment system used in the manufacturing of a film roll having a protrusion adjustment step that adjusts the number, height, and position of protrusions in the width direction of the film surface, characterized in that, The device includes: a film thickness acquisition means for obtaining the film thickness profile of the film during or after the protrusion adjustment process; a determination means for determining whether the number of protrusions in the width direction is within an ideal range of 1 to 10 per 1m and whether the height of the protrusions in the width direction is within an ideal range of 0.05 to 0.50 μm, based on the film thickness profile data; and a means for locally heating the film using an infrared heater in a manner where both the number of protrusions and the height of the protrusions are within an ideal range, provided that either the number of protrusions or the height of the protrusions is outside the ideal range in the determination means.

Citation Information

Patent Citations

  • JP1974061164A

  • Sticking of printing spacer

    JP1988250028A

  • Production of mixed fatty acid ester of cellulose

    JP1998045804A

  • Film winding method and roll as well as protected film

    JP2002255409A

  • Retardation film, polarizing plate and liquid crystal display element using the same

    JP2005227606A