Pulp composition, paper-plastic product and paper-plastic manufacturing process

By adjusting the pulp composition formulation and process flow, and introducing various additives, the problem of difficult demolding of pulp molded products in the hot pressing section was solved, and efficient demolding and high-strength pulp molded product production were achieved.

CN117468264BActive Publication Date: 2024-11-22KUNSHAN YUJIN GREEN PACKAGING CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202311510527.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-11-14
Publication Date
2024-11-22
Estimated Expiration
2043-11-14

AI Technical Summary

Technical Problem

Pulp molded products are difficult to demold in the hot pressing stage, resulting in product deformation, poor surface appearance and low production efficiency. Existing demolding methods cannot be effective in the long run.

Method used

By adjusting the pulp composition formulation, reducing the proportion of bamboo pulp and sugarcane pulp, introducing wood pulp, and adding resin control agents, wet strength agents, bactericides, water-based stearic acid and/or water-based stearate release agents, dry strength agents, and internal sizing agents, the pulp ratio and process flow are optimized to ensure the synergistic effect of each additive.

Benefits of technology

This technology enables easy demolding of pulp molded products in the hot pressing stage, improving production efficiency and yield, reducing the incidence of demolding defects, and significantly enhancing product strength and surface smoothness.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117468264B_ABST
    Figure CN117468264B_ABST
Patent Text Reader

Abstract

The present invention relates to the field of paper plastics, and in particular to a pulp composition, a paper plastic product and a paper plastic manufacturing process. The pulp composition comprises fiber pulp and a plurality of additives. The paper plastic product is prepared by using the pulp composition through S1-S7. The paper plastic manufacturing process provided by the present invention is simple, the product demoulding performance in a hot pressing section is excellent, and the physical indexes of the finally obtained paper plastic product are excellent. Each additive is added separately, and other additives are added after mixing for a certain period of time. Due to the different viscosities and surface charges of various additives and the different functions played by them, the additives are added in the order of addition described in the present invention, so that each additive can play a better effect. Through the coordination of a plurality of additives, the characteristics and functions of each additive are fully utilized to achieve the superposition of effects, so that the product demoulding performance in the hot pressing section of the paper plastic manufacturing process is excellent, and the obtained paper plastic product has excellent strength.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of pulp molding, and in particular to a pulp composition, a paper-molding product and a paper-molding manufacturing process. Background Art

[0002] Pulp molding products are made of waste paper, bamboo pulp, sugarcane pulp, and wood pulp fibers. They are made into wet embryos through pulping, pulping, pulping, vacuum filtration, and hot pressing to form finished products. No adhesive is required in the production process of pulp molding products. They are formed only by the interaction between the fibers themselves and the structure of the mold itself. The paper molding process can manufacture paper molding products with various shapes and complex structures and high dimensional accuracy requirements. The obtained paper molding products are environmentally friendly and biodegradable.

[0003] However, in the production process of pulp molded products, there is a problem of difficulty in demolding in the hot pressing stage; the product is easy to stick to the mold during the demolding process, resulting in deformation and poor surface appearance of the demolded product, which will also affect the production efficiency. Employees are required to clean the mold surface from time to time, which increases the workload and reduces production efficiency and product quality.

[0004] In the existing paper plastic manufacturing process, demoulding is assisted by spraying a demoulding agent on the mold surface or polishing the mold surface when poor mold sticking occurs. If demoulding is assisted by spraying a demoulding agent on the mold surface, since most demoulding agents are oily products, they are easy to adhere to the product surface, and there will be imprints on the appearance of the product, resulting in a decrease in the yield of the finished product. At the same time, the demoulding agent needs to be sprayed on the mold surface every 6-8 hours, which cannot guarantee a lasting demoulding effect and cannot be prevented in advance. If the method of polishing the mold surface to assist demoulding is used when poor mold sticking occurs, the polishing of the mold surface with a surface temperature of 150°C or higher takes a long time, and the edges and corners of the mold cannot be effectively cleaned, which can easily cause burns to the operators.

[0005] The above two methods of assisting demoulding cannot form a lasting demoulding effect. They are mainly follow-up measures when abnormalities occur during the production process and products are detected to have poor appearance, and they cannot achieve early prevention and control.

[0006] Therefore, this field still needs a paper-plastic manufacturing process that can fundamentally solve the problem of difficult demoulding of pulp molded products in the hot pressing stage. Summary of the invention

[0007] The purpose of the present invention is to provide a pulp composition, a paper-plastic product and a paper-plastic manufacturing process, by adjusting the formula of the pulp composition in the paper-plastic manufacturing process, optimizing the pulp ratio, using wood pulp to replace part of the bamboo pulp and sugarcane pulp, reducing the ratio of bamboo pulp and sugarcane pulp, and then reducing the ratio of adhesives, while introducing a resin control agent, a wet strength agent, a bactericide, an aqueous stearic acid and / or an aqueous stearate release agent, a dry strength agent and an in-pulp sizing agent as auxiliary agents, preventing the occurrence of poor mucosal aging in the front stage of molding, and fundamentally solving the problem of difficult demolding in the hot pressing stage.

[0008] In order to solve the above technical problems, the present invention provides a pulp composition, comprising:

[0009] Fiber pulp, the fiber pulp includes wood pulp pulp, bamboo pulp pulp, sugarcane pulp pulp;

[0010] A wide range of additives including resin control agents, wet strength agents, biocides, aqueous stearic acid and / or aqueous stearate release agents, dry strength agents and internal sizing agents.

[0011] By adjusting the formula of the pulp composition in the paper plastic manufacturing process, introducing wood pulp, optimizing the pulp ratio, and reducing the proportion of bamboo pulp and sugarcane pulp, the proportion of stickies in the manufacturing process is reduced, and the influence of stickies on the paper plastic manufacturing process is reduced; at the same time, a variety of auxiliary agents such as resin control agent, wet strength agent, bactericide, aqueous stearic acid and / or aqueous stearate release agent, dry strength agent and pulp sizing agent are introduced to cooperate with each other and work synergistically, which can not only improve the physical strength index of the product, but also fundamentally make the product easy to demold in the hot pressing section, reduce the production difficulty of the process, simplify the production process, improve the production efficiency of the process, and at the same time improve the product yield.

[0012] Furthermore, the plurality of additives, calculated by weight percentage of the fiber slurry, include:

[0013] 0.1-0.5% of resin control agent;

[0014] 2-4% wet strength agent;

[0015] 0.1-0.3% fungicide;

[0016] 1-4% aqueous stearic acid and / or aqueous stearate release agent;

[0017] 0.3-0.8% dry strength agent; and

[0018] 2-5% internal sizing agent.

[0019] The use of this ratio of multiple additives allows the effects of each additive to be better exerted, so that the final product has excellent physical indicators and excellent demoulding properties.

[0020] Furthermore, the mass percentage of wood pulp in the fiber pulp is 40%.

[0021] When the mass of wood pulp accounts for 40% of the total fiber pulp mass, the pulp ratio is optimal, which can not only ensure the high hardness of the final molded product, but also reduce the occurrence of poor demoulding problems.

[0022] Furthermore, the resin control agent is a non-ionic resin control agent;

[0023] The bactericide is a small molecule compound bactericide;

[0024] The dry strength agent is a cationic dry strength agent;

[0025] The wet strength agent is a cationic wet strength agent;

[0026] The internal sizing agent is a cationic internal sizing agent.

[0027] By combining and selecting a variety of additives and utilizing the characteristics and functions of each additive, the additives can interact well with each other in the paper plastic manufacturing process. Through the superposition of the effects of various additives, the product has the characteristics of excellent demoulding and high strength.

[0028] Furthermore, in the fiber pulp in the pulp composition, the mass ratio of each pulp is sugarcane pulp: bamboo pulp: wood pulp = 1:2:2;

[0029] Various additives; including

[0030] Calculated by mass percentage of fiber slurry:

[0031] 0.18% of resin control agent;

[0032] 3.2% wet strength agent;

[0033] 0.22% fungicide;

[0034] 2.6% aqueous stearic acid and / or aqueous stearate release agent;

[0035] 0.5% dry strength agent; and

[0036] 3.5% internal sizing agent.

[0037] The pulp composition adopts this ratio, and the paper plastic product (density: 0.71g / cm 3 , thickness: 0.93mm) has a tensile strength of 23.7N / mm and a bursting strength of 16.2Kgf / cm 2 , interlayer bonding strength is 342J / m 2The proportion of mold sticking defects per shift of a single machine is only 0.2% and there is no need to polish the mold surface. Compared with paper-plastic products of similar density manufactured by paper-plastic manufacturing processes using pulp compositions with other proportions, it has high strength and excellent demoulding performance.

[0038] In order to further solve the above technical problems, the present invention also provides a paper plastic manufacturing process, comprising the following steps:

[0039] S1. performing a first pulping step on a wood pulp slurry to obtain a first solution; wherein, in the first pulping step, adding an aqueous stearic acid and / or an aqueous stearate release agent;

[0040] S2. The bamboo pulp is subjected to a second pulping process to obtain a second solution; the sugarcane pulp is subjected to a second pulping process to obtain a third solution; wherein a resin control agent and a fungicide are sequentially added in the second pulping process;

[0041] S3. The first solution and the second solution are mixed and the dry strength agent is added and then refined to obtain a fourth solution;

[0042] S4. Adding a wet strength agent to the fourth solution to obtain a fifth solution;

[0043] S5. mixing the third solution with the fifth solution to obtain a sixth solution;

[0044] S6. Adding an internal sizing agent to the sixth solution to obtain a pulp composition;

[0045] S7. Complete a paper-plastic manufacturing process based on the pulp composition to obtain a paper-plastic product.

[0046] The paper-plastic manufacturing process provided by the present invention is simple, the product demoulding performance in the hot pressing section is excellent, and the physical indicators of the finally obtained paper-plastic product are excellent; each auxiliary agent is added separately, mixed for a certain period of time, and then other auxiliary agents are added; due to the different viscosities and surface charges of various auxiliary agents and the different functions they play, the auxiliary agents are added in the order of addition described in the present invention, so that each auxiliary agent can play a better effect; through the coordination of multiple auxiliary agents, the characteristics and functions of each auxiliary agent are fully utilized, and the superposition of effects is achieved, so that the product demoulding performance in the hot pressing section of the paper-plastic manufacturing process is excellent, and the obtained paper-plastic product has excellent strength.

[0047] Preferably, in the first pulping step, white water and aqueous stearic acid and / or aqueous stearate release agent diluted 20-40 times with clean water are added in sequence, stirred for 5 minutes, and then the wood pulp is dispersed after mixing evenly.

[0048] Furthermore, in the second pulping process, white water and a resin control agent diluted 20-40 times with clean water are first added in sequence and stirred for 5 minutes; after being evenly mixed, a fungicide diluted 20-40 times with clean water is added and stirred for 5 minutes, and after being evenly mixed, the bamboo pulp and sugarcane pulp are dispersed.

[0049] Furthermore, the dry strength agent needs to be diluted 50-80 times with clean water before addition; the wet strength agent needs to be diluted 10-20 times with clean water before addition; and the sizing agent in the slurry needs to be diluted 30-50 times with clean water before addition.

[0050] In order to further solve the above technical problems, the present invention also provides a paper-plastic product, which is obtained based on the above pulp composition or prepared according to the above paper-plastic process.

[0051] The paper-plastic product obtained by the invention has excellent physical indicators and has better strength than paper-plastic products with the same density and thickness. BRIEF DESCRIPTION OF THE DRAWINGS

[0052] The present invention will be further described below in conjunction with the accompanying drawings and embodiments:

[0053] Figure 1 A process flow chart of a paper-plastic manufacturing process of the present invention;

[0054] Figure 2 The present invention is a process flow chart of a paper plastic manufacturing process. DETAILED DESCRIPTION

[0055] The content of the present invention is further described in detail below in conjunction with specific embodiments, examples of which are shown in the accompanying drawings, wherein the same or similar reference numerals throughout represent the same or similar elements or elements with the same or similar functions. The embodiments described below with reference to the accompanying drawings are exemplary and are intended to be used to explain the present invention, and should not be construed as limiting the present invention.

[0056] The present invention first provides a pulp composition, comprising:

[0057] Fiber pulp, the fiber pulp includes wood pulp pulp, bamboo pulp pulp, sugarcane pulp pulp;

[0058] A wide range of additives including resin control agents, wet strength agents, biocides, aqueous stearic acid and / or aqueous stearate release agents, dry strength agents and internal sizing agents.

[0059] By adjusting the paper-plastic formula, replacing part of bamboo pulp and sugarcane pulp with wood pulp, and introducing different additives, we can prevent the occurrence of mold sticking in the early stage of molding, and prevent and reduce the probability of occurrence in advance. The continuity of production and the utilization rate of equipment are improved. By adjusting the pulping process and using functional additives, the adhesion of the product to the mold surface is reduced, the separation efficiency of the product and the mold surface is increased, and the product yield is improved. When the product strength index is improved to a certain extent, it has excellent demoulding performance, which can improve production efficiency and product yield, and reduce the pre-operation intensity of employees.

[0060] Secondly, the present invention also provides a paper-molding manufacturing process, such as Figure 2 As shown, the following steps are included:

[0061] S1. performing a first pulping step on a wood pulp slurry to obtain a first solution; wherein, in the first pulping step, adding an aqueous stearic acid and / or an aqueous stearate release agent;

[0062] S2. The bamboo pulp is subjected to a second pulping process to obtain a second solution; the sugarcane pulp is subjected to a second pulping process to obtain a third solution; wherein a resin control agent and a fungicide are sequentially added in the second pulping process;

[0063] S3. The first solution and the second solution are mixed and the dry strength agent is added and then refined to obtain a fourth solution;

[0064] S4. Adding a wet strength agent to the fourth solution to obtain a fifth solution;

[0065] S5. mixing the third solution with the fifth solution to obtain a sixth solution;

[0066] S6. Adding an internal sizing agent to the sixth solution to obtain a pulp composition;

[0067] S7. Complete a paper-plastic manufacturing process based on the pulp composition to obtain a paper-plastic product.

[0068] The paper-plastic manufacturing process provided by the present invention is simple in process, the product demoulding performance in the hot pressing section is excellent, and the physical indexes of the finally obtained paper-plastic product are excellent; each auxiliary agent is added separately, mixed for a certain period of time, and then other auxiliary agents are added; due to the different viscosities and surface charges of various auxiliary agents and the different functions they play, the auxiliary agents are added in the adding sequence of the present invention, so that each auxiliary agent can play a better effect; through the coordination of multiple auxiliary agents, the characteristics and functions of each auxiliary agent are fully utilized, the superposition and synergistic effect of the effects are achieved, so that the product demoulding performance in the hot pressing section of the paper-plastic manufacturing process is excellent, and the obtained paper-plastic product has excellent strength.

[0069] It should be noted that the first pulping step in the present invention is a wood pulp disintegration step, and the second pulping step is a bamboo pulp or sugarcane pulp disintegration step.

[0070] like Figure 1 As shown, the paper-plastic manufacturing process of the present invention comprises the following specific steps:

[0071] S1. Pulping process of wood pulp: first add white water to the pulping machine, then add water-based stearic acid and / or water-based stearate release agent diluted 20-40 times with clean water, stir for 5 minutes, add wood pulp board to pulp after mixing evenly, and obtain the first solution, and place the first solution in the pulping storage tank I; the surface of the water-based stearic acid is negatively charged, and the surface of the wood pulp fiber is negatively charged, and the two repel each other so that the first solution becomes a uniform whole;

[0072] S2. Bamboo pulp dispersing process and sugarcane pulp dispersing process: first add white water to the dispersing machine, then add a non-ionic resin control agent diluted 20-40 times with clean water, and stir for 5 minutes; then add a small molecule compound fungicide diluted 20-40 times with clean water, stir for 5 minutes, mix well, add a bamboo pulp board to disperse, and obtain a second solution, and place the second solution in a storage tank II after dispersing;

[0073] First add white water to the pulp dispersing machine, then add non-ionic resin control agent diluted 20-40 times with clean water, and stir for 5 minutes; then add small molecular compound fungicide diluted 20-40 times with clean water, stir for 5 minutes, mix well, add sugarcane pulp board to dispersing, and obtain the third solution, and place the third solution in storage tank III after dispersing;

[0074] The resin control agent is non-ionic, and the fungicide is a small molecule compound, which is directly dissolved in white water. The surface of bamboo pulp and sugarcane pulp fibers is negatively charged, and the second and third solutions are negatively charged as a whole;

[0075] S3. The first solution and the second solution are mixed evenly and placed in a pre-refining storage barrel, a cationic dry strength agent diluted 50-80 times with clean water is added, stirred for 5 minutes, and then refined after mixing to obtain a fourth solution, which is placed in a post-refining storage barrel; the surfaces of wood pulp fibers and bamboo pulp fibers are negatively charged, the surface of aqueous stearic acid is negatively charged, and the dry strength agent is strongly positively charged, which serves as a bridge to connect the fibers and the aqueous stearic acid, and the three are connected as a whole through the attraction of positive and negative charges;

[0076] S4. Add a cationic wet strength agent diluted 10-20 times with water to the fourth solution placed in the storage barrel after refining, stir for 5 minutes, and mix evenly to obtain a fifth solution; the surfaces of wood pulp fibers and bamboo pulp fibers are negatively charged, and after refining treatment, more free anionic groups are exposed, and the wet strength agent is positively charged and adsorbed on the fiber surface by charge adsorption;

[0077] S5. The third solution and the fifth solution are evenly mixed and placed in a mixing barrel to obtain a sixth solution;

[0078] S6. Add a cationic internal sizing agent diluted 30-50 times with clean water to the sixth solution, stir for 5 minutes, and mix evenly to obtain a pulp composition; after the dry strength agent, refining, and wet strength agent are applied in the early stage, the fiber surface has a part of positive charge, and some anionic additives have been adsorbed on the fiber surface, and after mixing, they become a whole; then add the internal sizing agent with positive charge to further act as a bridge, and act as an adsorption bridge for the anionic aqueous stearic acid and stearate release agent present in the system, so that all anionic additives and cationic additives can be adsorbed on the fiber surface;

[0079] S7. Dilute the pulp composition, form a wet embryo through vacuum filtration, and then perform hot pressing in a molding machine to form a paper-plastic product. The fibers and the anions and cations adsorbed on the fiber surface are heated to form a network structure that is spatially staggered. At the same time, the aqueous stearic acid and / or stearate used as a demoulding aid melts at high temperature, and as the water evaporates, part of it migrates to the surface of the product, and after cooling, a uniform and dense wax film is formed.

[0080] It should be noted that the wood pulp board, sugarcane pulp board and bamboo pulp board used in the present invention are papermaking fiber boards that can be purchased on the market.

[0081] In the actual production process, the production batch is generally large. In order to ensure product quality and production continuity, it is necessary to continuously perform operations such as slurry dispersion, grinding, mixing, and molding. Therefore, after each step, corresponding containers (such as storage barrels, mixing barrels) are used for mixing or temporary storage to facilitate the continuous implementation of each process; in the process from the mixed liquid to the molding machine, it is necessary to dilute it and transfer it through the corresponding containers after dilution; using containers for mixing, storage, and transfer are all common technical means and cannot be used as a limitation to the technical solution of the present invention.

[0082] 1. As an excellent papermaking raw material, wood pulp has a lower resin content than bamboo pulp and sugarcane pulp, especially sugarcane pulp. Although sugarcane pulp has the characteristics of high hardness of molded products, due to the high content of impurity cells and untreated monosaccharides in the material, some of them will migrate from the pulp to the surface of the product and mold during the heating process, and adhere to the mold, resulting in the occurrence of poor demoulding problems over time.

[0083] 2. The wet strength agent is adsorbed on the fiber surface and, after heating, forms a spatial network structure between the fibers, which restrains the movement of the fibers and also prevents the migration of fine fibers and internal impurity cells to the product surface, reducing the contact between adhesives and impurity cells and the mold, and reducing the probability of mold sticking.

[0084] 3. Aqueous stearic acid and / or aqueous stearate is a spherical particle suspension solution with a particle size of 20-30μm. During the formation of the wet embryo, the aqueous stearic acid or aqueous stearate fills the gaps between the fibers. During the heating and dehydration of the wet embryo, the particles melt and migrate to the surface of the product along with the water vapor. After the product is cooled, it condenses again inside and on the surface of the product to form a layer of stearic acid coating, which is a wax film. This not only improves the smoothness of the product surface, but also blocks the migration of fibers, miscellaneous cells and adhesives to the surface, reduces the contact between adhesives and molds, and reduces the probability of mold sticking.

[0085] 4. Resin control agent is mainly used to deal with stickies in pulp. It retains stickies and fine fibers in the pulp through surface adsorption and complexation. During vacuum pressing and hot pressing drying, impurity cells, stickies and sugars remain in the white water and are sucked away by the vacuum system. They do not stay on the surface of the product, which reduces the contact between stickies and molds and reduces the chance of mold sticking.

[0086] 5. Fungicides are mainly used to reduce the generation of rotten pulp during the production process. As a harmful substance in the production system, rotten pulp will adhere to the surface of the pipe during the production process and become white or brown viscous. Over time, it will fall into the production system and enter the molding system with the slurry. In the slurry absorption process, it enters the wet embryo of the product, stays on the surface of the product during the drying process, and adheres to the surface of the mold, causing the occurrence of mold sticking. The introduction of fungicides can purify the production system, prevent the generation of rotten pulp, and reduce the occurrence of mold sticking.

[0087] In the embodiments of the present invention, the resin control agent adopts pc-301 of Zhongshan Wei Le Chemical Co., Ltd. or 001 of Anshan Youze Tiansheng Environmental Protection Technology Co., Ltd.; the aqueous stearic acid and stearate release agent adopts ye3661 aqueous stearic acid emulsion or yf6633 aqueous zinc stearate emulsion of Luoyang Yefang New Material Technology Co., Ltd.; the wet strength agent adopts JH-1201 of Qingzhou Jinhao New Materials Co., Ltd. or AH-01 of Fengtai Environmental Protection Technology (Shandong) Co., Ltd.; the dry strength agent adopts XQ-70 enhancer from Taishan Xinquan Papermaking Additive Factory or PCG-G20 dry strength agent from Suzhou Paikem New Energy Technology Co., Ltd.; the bactericide adopts JH-8909B of Qingzhou Jinhao New Materials Co., Ltd. or D0025 of Shanghai Dejian Chemical Co., Ltd.; the internal sizing agent adopts JH-AKD200 of Qingzhou Jinhao New Materials Co., Ltd. or DH110 product of Qingzhou Dehai Fine Chemical Co., Ltd. By combining several additives, utilizing the characteristics and functions of each additive, and through the superposition effect, excellent demoulding and high strength effects can be achieved.

[0088] The “parts” in the embodiments of the present invention are parts by mass.

[0089] Example 1

[0090] S1. Pulping process of wood pulp: first add white water to the pulping machine, then add 1.5 parts of aqueous stearic acid and / or aqueous stearate release agent diluted 30 times with clean water, stir for 5 minutes, and after mixing evenly, add 40 parts of wood pulp board to pulp to obtain a first solution, and place the first solution in the post-slurry storage tank I;

[0091] S2. Bamboo pulp dispersing process and sugarcane pulp dispersing process: first add white water to the dispersing machine, then add 0.1 parts of non-ionic resin control agent diluted 30 times with clean water, stir for 5 minutes; then add 0.1 parts of small molecule compound fungicide diluted 30 times with clean water, stir for 5 minutes, mix well, add 40 parts of bamboo pulp board to dispersing, and obtain a second solution, and place the second solution in storage tank II after dispersing;

[0092] First add white water to the pulp dispersing machine, then add 0.1 part of non-ionic resin control agent diluted 30 times with clean water, and stir for 5 minutes; then add 0.1 part of small molecule compound fungicide diluted 30 times with clean water, stir for 5 minutes, mix well, add 20 parts of sugarcane pulp board to dissipate, and obtain the third solution, and place the third solution in the storage tank III after dissipation;

[0093] S3. The first solution and the second solution are mixed and placed in a storage barrel before refining, 0.3 parts of a cationic dry strength agent diluted 60 times with water are added, stirred for 5 minutes, mixed and then refining is performed to obtain a fourth solution, and the fourth solution is placed in a storage barrel after refining;

[0094] S4. Add 3 parts of a cationic wet strength agent diluted 15 times with water to the fourth solution placed in the storage barrel after refining, stir for 5 minutes, and mix to obtain a fifth solution;

[0095] S5. The third solution and the fifth solution are evenly mixed and placed in a mixing barrel to obtain a sixth solution;

[0096] S6. Add 4 parts of a cationic sizing agent diluted 40 times with water to the sixth solution, stir for 5 minutes, and mix well to obtain a pulp composition;

[0097] S7. dilute the pulp composition, form a wet embryo through vacuum filtration, and then perform heat pressing and shaping in a molding machine to form a paper-plastic product.

[0098] The paper-plastic product obtained in this example (density: 0.68 g / cm 3 , thickness: 0.93mm) has a tensile strength of 19.1N / mm and a bursting strength of 12.5Kgf / cm 2 , interlayer bonding strength is 321J / m 2 The proportion of mold defects per machine shift is 2.3%, and the polishing time for mold defects per machine shift is 35 minutes.

[0099] Example 2

[0100] S1. Pulping process of wood pulp: first add white water to the pulping machine, then add 2 parts of aqueous stearic acid and / or aqueous stearate release agent diluted 30 times with clean water, stir for 5 minutes, and after mixing evenly, add 40 parts of wood pulp board to pulp to obtain a first solution, and place the first solution in the storage tank I after pulping;

[0101] S2. Bamboo pulp dispersing process and sugarcane pulp dispersing process: first add white water to the dispersing machine, then add 0.3 parts of non-ionic resin control agent diluted 30 times with clean water, stir for 5 minutes; then add 0.3 parts of small molecule compound fungicide diluted 30 times with clean water, stir for 5 minutes, mix well, add 40 parts of bamboo pulp board to dispersing, and obtain a second solution, and place the second solution in storage tank II after dispersing;

[0102] First add white water to the pulp dispersing machine, then add 0.3 parts of non-ionic resin control agent diluted 30 times with clean water, and stir for 5 minutes; then add 0.3 parts of small molecule compound fungicide diluted 30 times with clean water, stir for 5 minutes, mix well, add 20 parts of sugarcane pulp board to disperse the pulp, and obtain the third solution, and place the third solution in the storage tank III after the pulp is dispersed;

[0103] S3. The first solution and the second solution are mixed and placed in a storage barrel before refining, 0.5 parts of a cationic dry strength agent diluted 60 times with water are added, stirred for 5 minutes, mixed and then refining is performed to obtain a fourth solution, and the fourth solution is placed in a storage barrel after refining;

[0104] S4. Add 3 parts of a cationic wet strength agent diluted 15 times with water to the fourth solution placed in the storage barrel after refining, stir for 5 minutes, and mix to obtain a fifth solution;

[0105] S5. The third solution and the fifth solution are evenly mixed and placed in a mixing barrel to obtain a sixth solution;

[0106] S6. Add 2 parts of a cationic sizing agent diluted 40 times with water to the sixth solution, stir for 5 minutes, and mix well to obtain a pulp composition;

[0107] S7. dilute the pulp composition, form a wet embryo through vacuum filtration, and then perform heat pressing and shaping in a molding machine to form a paper-plastic product.

[0108] The paper-plastic product obtained in this example (density: 0.73 g / cm 3 , thickness: 0.90mm) has a tensile strength of 20.5N / mm and a burst strength of 13.7Kgf / cm 2 , interlayer bonding strength is 333J / m 2 The proportion of mold defects for a single machine per shift is 1.5%, and the polishing time for mold defects for a single machine per shift is 20 minutes.

[0109] Example 3

[0110] S1. Pulp dispersing process: first add white water to the dispersing machine, then add 2.5 parts of aqueous stearic acid and / or aqueous stearate release agent diluted 30 times with clean water, stir for 5 minutes, and after mixing evenly, add 40 parts of wood pulp board to dispersing to obtain a first solution, and place the first solution in the storage tank I after dispersing;

[0111] S2. Bamboo pulp dispersing process and sugarcane pulp dispersing process: first add white water to the dispersing machine, then add 0.4 parts of non-ionic resin control agent diluted 30 times with clean water, stir for 5 minutes; then add 0.25 parts of small molecule compound fungicide diluted 30 times with clean water, stir for 5 minutes, mix well, add 40 parts of bamboo pulp board to dispersing, and obtain a second solution, and place the second solution in storage tank II after dispersing;

[0112] First add white water to the pulp dispersing machine, then add 0.4 parts of non-ionic resin control agent diluted 30 times with clean water, and stir for 5 minutes; then add 0.25 parts of small molecule compound fungicide diluted 30 times with clean water, stir for 5 minutes, mix well, add 20 parts of sugarcane pulp board to disperse the pulp, and obtain the third solution, and place the third solution in the storage tank III after the pulp is dispersed;

[0113] S3. The first solution and the second solution are mixed and placed in a storage barrel before refining, 0.7 parts of a cationic dry strength agent diluted 60 times with water are added, stirred for 5 minutes, mixed and then refining is performed to obtain a fourth solution, and the fourth solution is placed in a storage barrel after refining;

[0114] S4. Add 2 parts of a cationic wet strength agent diluted 15 times with water to the fourth solution placed in the storage barrel after refining, stir for 5 minutes, and mix to obtain a fifth solution;

[0115] S5. The third solution and the fifth solution are evenly mixed and placed in a mixing barrel to obtain a sixth solution;

[0116] S6. Add 3 parts of a cationic internal sizing agent diluted 40 times with water to the sixth solution, stir for 5 minutes, and mix well to obtain a pulp composition;

[0117] S7. dilute the pulp composition, form a wet embryo through vacuum filtration, and then perform heat pressing and shaping in a molding machine to form a paper-plastic product.

[0118] The paper-plastic product obtained in this example (density: 0.70 g / cm 3 , thickness: 0.89mm) has a tensile strength of 21.2N / mm and a bursting strength of 14.2Kgf / cm 2 , interlayer bonding strength is 306J / m 2 The proportion of mold sticking defects per machine shift is 0.9%, and the polishing time for mold sticking defects per machine shift is 8 minutes.

[0119] Example 4

[0120] S1. Pulping process of wood pulp: first add white water to the pulping machine, then add 3 parts of aqueous stearic acid and / or aqueous stearate release agent diluted 30 times with clean water, stir for 5 minutes, and after mixing evenly, add 40 parts of wood pulp board to pulp to obtain a first solution, and place the first solution in the storage tank I after pulping;

[0121] S2. Bamboo pulp dispersing process and sugarcane pulp dispersing process: first add white water to the dispersing machine, then add 0.2 parts of non-ionic resin control agent diluted 30 times with clean water, stir for 5 minutes; then add 0.2 parts of small molecule compound fungicide diluted 30 times with clean water, stir for 5 minutes, mix well, add 40 parts of bamboo pulp board to dispersing, and obtain a second solution, and place the second solution in storage tank II after dispersing;

[0122] First add white water to the pulp dispersing machine, then add 0.2 parts of non-ionic resin control agent diluted 30 times with clean water, and stir for 5 minutes; then add 0.2 parts of small molecule compound fungicide diluted 30 times with clean water, stir for 5 minutes, mix well, add 20 parts of sugarcane pulp board to dissipate, and obtain the third solution, and place the third solution in the storage tank III after dissipation;

[0123] S3. The first solution and the second solution are mixed and placed in a storage barrel before refining, 0.8 parts of a cationic dry strength agent diluted 60 times with water is added, stirred for 5 minutes, mixed and then refining is performed to obtain a fourth solution, and the fourth solution is placed in a storage barrel after refining;

[0124] S4. Add 4 parts of a cationic wet strength agent diluted 15 times with water to the fourth solution placed in the storage barrel after refining, stir for 5 minutes, and mix to obtain a fifth solution;

[0125] S5. The third solution and the fifth solution are evenly mixed and placed in a mixing barrel to obtain a sixth solution;

[0126] S6. Add 3 parts of a cationic internal sizing agent diluted 40 times with water to the sixth solution, stir for 5 minutes, and mix well to obtain a pulp composition;

[0127] S7. dilute the pulp composition, form a wet embryo through vacuum filtration, and then perform heat pressing and shaping in a molding machine to form a paper-plastic product.

[0128] The paper-plastic product obtained in this example (density: 0.69 g / cm 3 , thickness: 0.91mm) has a tensile strength of 23.9N / mm and a bursting strength of 15.1Kgf / cm 2 , interlayer bonding strength is 333J / m 2 The proportion of mold sticking defects per machine shift is 0.7%, and the polishing time for mold sticking defects per machine shift is 5 minutes.

[0129] Example 5

[0130] S1. Pulping process of wood pulp: first add white water to the pulping machine, then add 4 parts of aqueous stearic acid and / or aqueous stearate release agent diluted 30 times with clean water, stir for 5 minutes, and after mixing evenly, add 40 parts of wood pulp board to pulp to obtain a first solution, and place the first solution in the storage tank I after pulping;

[0131] S2. Bamboo pulp dispersing process and sugarcane pulp dispersing process: first add white water to the dispersing machine, then add 0.5 parts of non-ionic resin control agent diluted 30 times with clean water, stir for 5 minutes; then add 0.15 parts of small molecule compound fungicide diluted 30 times with clean water, stir for 5 minutes, mix well, add 40 parts of bamboo pulp board to disperse, obtain a second solution, and place the second solution in the storage tank II after dispersing;

[0132] First add white water to the pulp dispersing machine, then add 0.5 parts of non-ionic resin control agent diluted 30 times with clean water, and stir for 5 minutes; then add 0.15 parts of small molecule compound fungicide diluted 30 times with clean water, stir for 5 minutes, mix well, add 20 parts of sugarcane pulp board to disperse, and obtain the third solution, and place the third solution in the storage tank III after dispersing;

[0133] S3. The first solution and the second solution were mixed and placed in a storage barrel before refining, 0.6 parts of a cationic dry strength agent diluted 60 times with water was added, stirred for 5 minutes, mixed and then refining was performed to obtain a fourth solution, and the fourth solution was placed in a storage barrel after refining;

[0134] S4. Add 3 parts of a cationic wet strength agent diluted 15 times with water to the fourth solution placed in the storage barrel after refining, stir for 5 minutes, and mix to obtain a fifth solution;

[0135] S5. The third solution and the fifth solution are evenly mixed and placed in a mixing barrel to obtain a sixth solution;

[0136] S6. Add 2 parts of a cationic sizing agent diluted 40 times with water to the sixth solution, stir for 5 minutes, and mix well to obtain a pulp composition;

[0137] S7. dilute the pulp composition, form a wet embryo through vacuum filtration, and then perform heat pressing and shaping in a molding machine to form a paper-plastic product.

[0138] The paper-plastic product obtained in this example (density: 0.71 g / cm 3 , thickness: 0.90mm) has a tensile strength of 24.3N / mm and a bursting strength of 12.9Kgf / cm 2 , interlayer bonding strength is 306J / m 2 The proportion of mold sticking defects per machine shift is 1.1%, and the polishing time for mold sticking defects per machine shift is 11 minutes.

[0139] Example 6

[0140] S1. Pulping process of wood pulp: first add white water to the pulping machine, then add 2.6 parts of aqueous stearic acid and / or aqueous stearate release agent diluted 30 times with clean water, stir for 5 minutes, and after mixing evenly, add 40 parts of wood pulp board to pulp to obtain a first solution, and place the first solution in the storage tank I after pulping;

[0141] S2. Bamboo pulp dispersing process and sugarcane pulp dispersing process: first add white water to the dispersing machine, then add 0.18 parts of non-ionic resin control agent diluted 30 times with clean water, stir for 5 minutes; then add 0.22 parts of small molecule compound fungicide diluted 30 times with clean water, stir for 5 minutes, mix well, add 40 parts of bamboo pulp board to disperse, obtain a second solution, and place the second solution in the storage tank II after dispersing;

[0142] First add white water to the pulp dispersing machine, then add 0.18 parts of non-ionic resin control agent diluted 30 times with clean water, and stir for 5 minutes; then add 0.22 parts of small molecule compound fungicide diluted 30 times with clean water, stir for 5 minutes, mix well, add 20 parts of sugarcane pulp board to disperse, and obtain the third solution, and place the third solution in the storage tank III after dispersing;

[0143] S3. The first solution and the second solution are mixed and placed in a storage barrel before refining, 0.5 parts of a cationic dry strength agent diluted 60 times with water are added, stirred for 5 minutes, mixed and then refining is performed to obtain a fourth solution, and the fourth solution is placed in a storage barrel after refining;

[0144] S4. Add 3.2 parts of a cationic wet strength agent diluted 15 times with water to the fourth solution placed in the storage barrel after refining, stir for 5 minutes, and mix to obtain a fifth solution;

[0145] S5. The third solution and the fifth solution are evenly mixed and placed in a mixing barrel to obtain a sixth solution;

[0146] S6. Add 3.5 parts of a cationic sizing agent diluted 40 times with water to the sixth solution, stir for 5 minutes, and mix well to obtain a pulp composition;

[0147] S7. dilute the pulp composition, form a wet embryo through vacuum filtration, and then perform heat pressing and shaping in a molding machine to form a paper-plastic product.

[0148] The paper-plastic product obtained in this example (density: 0.71 g / cm 3 , thickness: 0.93mm) has a tensile strength of 23.7N / mm and a bursting strength of 16.2Kgf / cm 2, interlayer bonding strength is 342J / m 2 The sticking defect rate of a single machine per shift is 0.2%, and there is no need to polish the mold surface.

[0149] Comparative Example 1

[0150] 1. Bamboo pulp dispersing process and sugarcane pulp dispersing process: first add white water to the dispersing machine, then add 65 parts of bamboo pulp board to dispersing bamboo pulp, and place the obtained solution I in the storage tank I after dispersing;

[0151] Firstly add white water to the pulping machine, then add 35 parts of sugarcane pulp board to pulp the sugarcane pulp, and place the obtained solution II in the storage tank II after pulping;

[0152] 2. Refining solution I to obtain solution III, and placing solution III in a refining storage barrel;

[0153] 3. Mix solution III and solution II evenly and place them in a mixing barrel to obtain solution IV; add 4 parts of a cationic internal sizing agent diluted 40 times with clean water to solution IV, stir for 5 minutes, and mix evenly to obtain a pulp composition;

[0154] 4. Dilute the pulp composition, form a wet embryo through vacuum filtration, and then perform heat pressing and shaping in a molding machine to form a paper-plastic product.

[0155] The paper-plastic product obtained in this example (density: 0.71 g / cm 3 , thickness: 0.90mm) has a tensile strength of 13.1N / mm and a bursting strength of 8.5Kgf / cm 2 , interlayer bonding strength is 269J / m 2 The proportion of mold defects per shift for a single machine is 5.8%, and the polishing time for mold defects per shift for a single machine is 110 minutes.

[0156] Comparative Example 2

[0157] 1. Pulping process: first add white water to the pulping machine, then add 40 parts of wood pulp board to pulp, and place the obtained solution I in the pulping storage tank I;

[0158] Bamboo pulp dispersing process and sugarcane pulp dispersing process: first add white water to the dispersing machine, then add 40 parts of bamboo pulp board to dispersing bamboo pulp, and obtain solution II and place it in storage tank II after dispersing;

[0159] Firstly add white water to the pulp dispersing machine, then add 20 parts of sugarcane pulp board to dissipate the sugarcane pulp, and obtain solution III and place it in the storage tank III after dispersing;

[0160] 2. Mix solution I and solution II and perform refining treatment to obtain solution IV, and place solution IV in a refining storage barrel;

[0161] 3. Mix solution III and solution IV evenly and place them in a mixing barrel to obtain solution V; add 4 parts of an internal sizing agent diluted 40 times with clean water to solution V, stir for 5 minutes, and mix evenly to obtain a pulp composition;

[0162] 4. Dilute the pulp composition, form a wet embryo through vacuum filtration, and then perform heat pressing and shaping in a molding machine to form a paper-plastic product.

[0163] The paper-plastic product obtained in this example (density: 0.72 g / cm 3 , thickness: 0.89mm) has a tensile strength of 14.2N / mm and a bursting strength of 9.1Kgf / cm 2 , interlayer bonding strength is 293J / m 2 The proportion of mold sticking defects per machine shift is 3.9%, and the polishing time of mold sticking defects per machine shift is 59 minutes.

[0164] Comparative Example 3

[0165] 1. Pulping process: first add white water to the pulping machine, then add 40 parts of wood pulp board to pulp, and place the obtained solution I in the pulping storage tank I;

[0166] Bamboo pulp dispersing process and sugarcane pulp dispersing process: first add white water to the dispersing machine, then add 65 parts of bamboo pulp board to dispersing bamboo pulp, and obtain solution II and place it in storage tank II after dispersing;

[0167] Firstly add white water to the pulping machine, then add 35 parts of sugarcane pulp board to pulp the sugarcane pulp, and obtain solution III and place it in the storage tank III after pulping;

[0168] 2. Mix solution I and solution II and perform refining treatment to obtain solution IV, and place solution IV in a refining storage barrel; add 2 parts of a cationic wet strength agent diluted 15 times with clean water to solution IV in the refining storage barrel, stir for 5 minutes, and mix well to obtain solution V;

[0169] 3. Mix solution III and solution V evenly and place them in a mixing barrel to obtain solution VI; add 2 parts of a cationic internal sizing agent diluted 40 times with clean water to solution VI, stir for 5 minutes, and mix evenly to obtain a pulp composition;

[0170] 4. Dilute the pulp composition, form a wet embryo through vacuum filtration, and then perform heat pressing and shaping in a molding machine to form a paper-plastic product.

[0171] The paper-plastic product obtained in this example (density: 0.71 g / cm 3 , thickness: 0.92mm) has a tensile strength of 17.3N / mm and a bursting strength of 10.4Kgf / cm 2, interlayer bonding strength is 305J / m 2 The proportion of mold defects per shift for a single machine is 4.2%, and the polishing time for mold defects per shift for a single machine is 72 minutes.

[0172] By analyzing the paper-plastic products with similar density and thickness obtained in Examples 1-6 and Comparative Examples 1-3, it can be seen that, compared with Comparative Examples 1-3, the paper-plastic products prepared by the paper-plastic process of the present invention using the pulp composition of the present invention have a greatly reduced proportion of defective mucosa per shift of a single machine, a greatly shortened polishing time of defective mucosa per shift of a single machine, and excellent demolding performance in the hot pressing section; the paper-plastic products prepared by the paper-plastic process of the present invention using the pulp composition of the present invention have excellent performance in various physical indicators, and the physical indicators of the paper-plastic products obtained in Example 6 have the best performance, that is, the pulp composition ratio in Example 6 of the present invention is the best ratio.

[0173] It should be noted that the resin control agent in the present invention includes but is not limited to the resin control agent product used in the embodiments of the present invention, and any common non-ionic resin control agent on the market can be used; the bactericide in the present invention includes but is not limited to the bactericide product used in the embodiments of the present invention, and any common small molecule compound bactericide on the market can be used; the aqueous stearic acid and / or aqueous stearate release agent in the present invention includes but is not limited to the aqueous stearic acid and / or aqueous stearate release agent product used in the embodiments of the present invention, and any common aqueous stearic acid and / or aqueous stearate release agent on the market can be used; the dry strength agent in the present invention includes but is not limited to the dry strength agent product used in the embodiments of the present invention, and any common cationic dry strength agent on the market can be used; the wet strength agent in the present invention includes but is not limited to the wet strength agent product used in the embodiments of the present invention, and any common cationic wet strength agent on the market can be used; the in-slurry sizing agent in the present invention includes but is not limited to the in-slurry sizing agent product used in the embodiments of the present invention, and any common cationic in-slurry sizing agent on the market can be used.

[0174] It should be noted that the various additives used in this application are not simply superimposed on performance. Due to the different viscosities and surface charges of various additives, as well as the different functions they play, each additive needs to be added separately, mixed evenly, and then the next additive is added. The order of adding the additives cannot be adjusted. If the order of addition is adjusted, the various additives in the entire system will not be able to be efficiently combined or efficiently deposited on the fiber surface, resulting in the weakening of the effects of some additives, and they will be lost with the white water and will not work.

[0175] It should be further explained that the fiber slurry in the embodiment of the present invention is initially in a dry pulp board state, and the "mass ratio, mass part" in the present invention all correspond to the dry weight of each fiber slurry.

[0176] The above embodiments are only for illustrating the technical concept and features of the present invention, and their purpose is to enable people familiar with this technology to understand the content of the present invention and implement it accordingly, and they cannot be used to limit the scope of protection of the present invention. For those skilled in the art, it is obvious that the present invention is not limited to the details of the above exemplary embodiments, and the present invention can be implemented in other specific forms without departing from the spirit or basic features of the present invention. Therefore, no matter from which point of view, the embodiments should be regarded as exemplary and non-restrictive. The scope of the present invention is limited by the attached claims rather than the above description, and it is intended to include all changes within the meaning and scope of the equivalent elements of the claims in the present invention.

Claims

1. A paper plastic manufacturing process, characterized in that: The pulp composition used includes fiber pulp and multiple additives; The fiber pulp includes wood pulp, bamboo pulp and sugarcane pulp; the mass percentage of wood pulp in the fiber pulp is 40%; the mass ratio of each pulp in the fiber pulp in the pulp composition is sugarcane pulp: bamboo pulp: wood pulp = 1:2:2; The multiple auxiliary agents include resin control agents, wet strength agents, fungicides, aqueous stearic acid and / or aqueous stearate release agents, dry strength agents and internal sizing agents; The various additives, calculated by weight percentage of the fiber slurry, include: 0.1-0.5% of resin control agent; 2-4% wet strength agent; 0.1-0.3% fungicide; 1-4% aqueous stearic acid and / or aqueous stearate release agent; 0.3-0.8% dry strength agent; and 2-5% internal sizing agent; The resin control agent is a non-ionic resin control agent; The bactericide is a small molecule compound bactericide; The dry strength agent is a cationic dry strength agent; The wet strength agent is a cationic wet strength agent; The internal sizing agent is a cationic internal sizing agent; The manufacturing process includes the following steps: S1. performing a first pulping step on a wood pulp slurry to obtain a first solution; wherein, in the first pulping step, adding an aqueous stearic acid and / or an aqueous stearate release agent; S2. The bamboo pulp is subjected to a second pulping process to obtain a second solution; the sugarcane pulp is subjected to a second pulping process to obtain a third solution; wherein a resin control agent and a fungicide are sequentially added in the second pulping process; S3. The first solution and the second solution are mixed and the dry strength agent is added and then refined to obtain a fourth solution; S4. Adding a wet strength agent to the fourth solution to obtain a fifth solution; S5. mixing the third solution with the fifth solution to obtain a sixth solution; S6. Adding an internal sizing agent to the sixth solution to obtain a pulp composition; S7. Based on the pulp composition, a wet embryo is formed by vacuum filtration, and then hot pressing and shaping is performed in a molding machine to form a paper-plastic product.

2. The paper-plastic manufacturing process according to claim 1, characterized in that: Various additives include Calculated by mass percentage of fiber slurry: 0.18% of resin control agent; 3.2% wet strength agent; 0.22% fungicide; 2.6% aqueous stearic acid and / or aqueous stearate release agent; 0.5% dry strength agent; and 3.5% internal sizing agent.

3. The paper-plastic manufacturing process according to claim 1, characterized in that: In the first pulping process, white water and aqueous stearic acid and / or aqueous stearate release agent diluted 20-40 times with clean water are added in sequence, stirred for 5 minutes, and then the wood pulp is dispersed after mixing evenly.

4. The paper-plastic manufacturing process according to claim 1, characterized in that: In the second pulping process, white water and a resin control agent diluted 20-40 times with clean water are first added in sequence and stirred for 5 minutes; after being evenly mixed, a fungicide diluted 20-40 times with clean water is added and stirred for 5 minutes, and after being evenly mixed, bamboo pulp and sugarcane pulp are dispersed.

5. The paper-plastic manufacturing process according to claim 1, characterized in that: The dry strength agent is diluted 50-80 times with clean water before adding; the wet strength agent is diluted 10-20 times with clean water before adding; the sizing agent in the slurry is diluted 30-50 times with clean water before adding.

6. A paper-plastic product, wherein the paper-plastic product is prepared according to the paper-plastic manufacturing process according to any one of claims 1 to 5.