Preparation method of PU protective film for permanent support film of flexible electronic devices

Through the preparation method of PU protective film with three-layer structure, the component adjustment and network cross-linking technology of antistatic coatings are used to solve the problem of easy damage and peeling of permanent support films in flexible electronic devices, achieving low adhesion and no residues The effect of the device improves the service life and convenience of replacement.

CN117535019BActive Publication Date: 2024-12-03AZUSA TECH (SHENZHEN) CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202311397619.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-10-26
Publication Date
2024-12-03
Estimated Expiration
2043-10-26

AI Technical Summary

Technical Problem

In flexible electronic devices, the permanent support film is easily damaged and difficult to replace, and the existing PU protective film often has residual problems during peeling, making it difficult to meet the requirements of low adhesion and no residue.

Method used

The preparation method of PU protective film with a three-layer structure includes a dual-resistant substrate, an adhesive layer and a dual-resistant release layer. The low peeling force and release force are achieved through the component adjustment of the antistatic coating, and the use of hexamethylene diisocyanate Cross-linking with 2,2-bis(hydroxymethyl)propionic acid to avoid adhesive residue.

Benefits of technology

The PU protective film with low adhesion and no residue after peeling is achieved, which improves the service life of flexible electronic devices and the convenience of replacement.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117535019B_ABST
    Figure CN117535019B_ABST
Patent Text Reader

Abstract

The present invention discloses a method for preparing a PU protective film for a permanent support film of a flexible electronic device, which specifically comprises the following steps: step 1, preparing a double-resistance substrate; step 2, preparing a double-resistance release film; step 3, spin coating a layer of adhesive on the lower surface of the double-resistance substrate prepared in step 1 to form an adhesive layer, and drying it at 80°C-120°C, and then compounding it with the double-resistance release film prepared in step 2, rolling it up, and ripening it at 40°C-50°C for 40h-60h to obtain a PU protective film. The PU protective film prepared by the present invention has the characteristics of low adhesion of the adhesive layer and no residue after peeling.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of polymer composite materials and relates to a method for preparing a PU protective film used as a permanent support film for flexible electronic devices. Background Art

[0002] PU (polyurethane resin) protective film is widely used in the field of flexible electronic devices, and its main function is to improve the service life of the device. In the field of flexible electronic devices, such as solid-state lighting, new displays, and solar cells, polymer substrates (polyimide films, polyester films) are usually very thin and flexible, and a permanent support film needs to be introduced to improve the stiffness of flexible electronic devices. It should be pointed out that the permanent support film is directly and tightly attached to the substrate, and the permanent support film is not easy to replace. Since the support film on the surface of electronic products is easily scratched and damaged during actual application and transportation, it has a certain service life. Therefore, adding a layer of PU protective film to the surface of the permanent support film can protect the permanent support film in the electronic product. In order to use the PU protective film in flexible electronic devices and facilitate replacement, the PU protective film needs to meet the requirements of light peeling of the release layer, low adhesion of the adhesive layer, and no residue after peeling. Summary of the invention

[0003] The purpose of the present invention is to provide a method for preparing a PU protective film used as a permanent support film for flexible electronic devices. The PU protective film prepared by the method has the characteristics of low adhesion of the bonding layer and no residue after peeling.

[0004] The technical solution adopted by the present invention is a method for preparing a PU protective film for a permanent support film of a flexible electronic device, which specifically comprises the following steps:

[0005] Step 1, preparing a double antibody substrate;

[0006] Step 2, preparing a double-resistance release film;

[0007] Step 3, spin-coat a layer of adhesive on the lower surface of the double-resistance substrate prepared in step 1 to form an adhesive layer, and dry it at 80℃-120℃, then compound it with the double-resistance release film prepared in step 2, roll it up, and mature it at 40℃-50℃ for 40h-60h to obtain a PU protective film.

[0008] The present invention is also characterized in that:

[0009] The specific process of step 1 is: take a PET film with a thickness of 25um-40um, spin-coat a layer of 3um-5um antistatic coating I on the upper surface of the PET, and then spin-coat a layer of 3um-5um antistatic coating II on the lower surface of the PET; finally, dry it at 80℃-120℃ to obtain a double-antistatic substrate.

[0010] The preparation process of antistatic coating I is:

[0011] The following components are weighed respectively by mass percentage: 2wt%-5wt% of hexamethylene diisocyanate, 2wt%-5wt% of 2,2-bis(hydroxymethyl)propionic acid, 10wt%-15wt% of aqueous polyurethane, 2wt%-5wt% of cationic guar gum, 0.002wt%-0.3wt% of wetting agent, and the remaining component is water. The sum of the mass percentages of the above components is 100%. After mixing and stirring the above components, the antistatic coating I is obtained.

[0012] The preparation process of antistatic coating II is:

[0013] The following components are weighed respectively according to mass percentage: 4wt%-10wt% of hexamethylene diisocyanate, 2%-5% of 2,2-bis(hydroxymethyl)propionic acid, 10wt%-15wt% of aqueous polyurethane, 0.002wt%-0.3wt% of wetting agent, and the remaining component is water. The sum of the mass percentages of the above components is 100%. After mixing and stirring the above components, the antistatic coating II is obtained.

[0014] The specific process of step 2 is:

[0015] Take a PET film with a thickness of 5um-10um, spin-coat a layer of 3um-5um antistatic coating III on the upper and lower surfaces of the PET respectively, and then dry it at 80℃-120℃ to obtain a double anti-release film.

[0016] In step 2, the preparation process of antistatic coating III is:

[0017] The following components are weighed respectively by mass percentage: 2wt%-5wt% of cationic guar gum, 10wt%-15wt% of water-based polyurethane, 2wt%-5wt% of acrylic acid, 0.002wt%-0.3wt% of wetting agent, and the remaining component is water. The sum of the mass percentages of the above components is 100%. After mixing and stirring the above components, the antistatic coating III is obtained.

[0018] In step 3, the components of the adhesive include:

[0019] 10% wt-20% wt of polyvinyl alcohol, 10% wt-20% wt of silicon phosphate, 10% wt-20% acrylate, 10% wt-20% wt of dimethyldivinylsilane, 10% wt-20% wt of epoxy acrylate, 10% wt-20% wt of N-dodecyldimethylamine, 5% wt-15% wt of hexamethylene diisocyanate, and 5% wt-15% wt of 2,2-bis(hydroxymethyl)propionic acid, and the sum of the mass percentages of the above components is 100%.

[0020] The beneficial effect of the present invention is that the main structure of the PU protective film is three layers: a double-resistance substrate, an adhesive layer, and a double-resistance release layer. Cationic guar gum is used to adjust the antistatic properties of the upper and lower surfaces of the double-resistance substrate. The peeling force between the double-resistance substrate and the adhesive layer and the release force between the double-resistance release layer and the adhesive layer are adjusted by hexamethylene diisocyanate. While achieving the antistatic requirements, low peeling force and release force are met. Finally, through the network cross-linking polymerization of hexamethylene diisocyanate and 2,2-bis(hydroxymethyl)propionic acid, the adhesive residue after peeling caused by molecular chain displacement is avoided. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1 It is a schematic structural diagram of a PU protective film prepared by the method for preparing a PU protective film as a permanent support film for flexible electronic devices of the present invention;

[0022] Figure 2 It is a comparison diagram of the bonding force between the substrate and the bonding layer in Example 1 of the method for preparing the PU protective film for a permanent support film of a flexible electronic device of the present invention and Comparative Examples 1 to 3.

[0023] In the figure, 1. antistatic layer I, 2. PET film I, 3. antistatic layer II, 4. adhesive layer, 5. antistatic layer III, 6. PET film II, 7. antistatic layer IV. DETAILED DESCRIPTION

[0024] The present invention is described in detail below with reference to the accompanying drawings and specific embodiments.

[0025] The method for preparing the PU protective film for the permanent support film of the flexible electronic device of the present invention specifically comprises the following steps:

[0026] Preparation of double-antistatic substrate: first take a PET film with a thickness of 25um-40um, spin-coat a layer of 3um-5um antistatic coating I on the upper surface of the PET; spin-coat a layer of 3um-5um antistatic coating II on the lower surface of the PET; then dry it at 80℃-120℃ for later use.

[0027] The preparation process of antistatic coating I is as follows: hexamethylene diisocyanate (2wt%-5wt%), 2,2-bis(hydroxymethyl)propionic acid (2wt%-5wt%), water-based polyurethane (10wt%-15wt%), cationic guar gum (2wt%-5wt%), wetting agent (0.002wt%-0.3wt%), and the remaining component is water. The sum of the mass percentages of the above components is 100%. The antistatic coating I is obtained by stirring at 600r / min in a mixer for 20min.

[0028] The preparation process of antistatic coating II is as follows: hexamethylene diisocyanate (4wt%-10wt%), 2,2-bis(hydroxymethyl)propionic acid (2wt%-5wt%), water-based polyurethane (10wt%-15wt%), wetting agent (0.002wt%-0.3wt%), and the remaining components are water. The sum of the mass percentages of the above components is 100%, and the mixture is stirred at 600r / min in a mixer for 20 minutes.

[0029] Preparation of double anti-release film: First, take a PET film with a thickness of 5um-10um, spin-coat a layer of 3um-5um antistatic coating III on the upper and lower surfaces of the PET, and then dry it at 80℃-120℃ for use.

[0030] Preparation of PU protective film: First, a layer of adhesive is spin-coated on the lower surface of the double-resistance substrate to form an adhesive layer. The thickness of the adhesive layer is 3um-6um and is dried at 80℃-120℃. Then, it is compounded with the double-resistance release film, rolled up, and aged at 40℃-50℃ for 40h-60h to obtain the PU protective film.

[0031] The preparation process of antistatic coating III is as follows: cationic guar gum (2wt%-5wt%), water-based polyurethane (10wt%-15wt%), acrylic acid (2wt%-5wt%), wetting agent (0.002wt%-0.3wt%), and the remaining component is water. The sum of the mass percentages of the above components is 100%, and the mixture is stirred at 600r / min for 20 minutes in a mixer.

[0032] The adhesive composition of the adhesive layer: polyvinyl alcohol (10% wt-20% wt), silicon phosphate (10% wt-20wt%), acrylate (10% wt-20wt%), dimethyldivinylsilane (10% wt-20wt%), epoxy acrylate (10% wt-20wt%), N-dodecyldimethylamine (10% wt-20wt%), hexamethylene diisocyanate (5% wt-15wt%), and 2,2-bis(hydroxymethyl)propionic acid (5% wt-15wt%).

[0033] The structure of the PU protective film prepared by the present invention is as follows Figure 1 In the figure, straight line AB is the release surface, the antistatic layer I1, PET film I2, and antistatic layer II3 are combined together to form a double antistatic base, 4 is an adhesive layer, and the antistatic layer III5, PET film II6, and antistatic layer IV7 are combined together to form a double antistatic release film.

[0034] Example 1

[0035] Step 1, take a PET film with a thickness of 25um, spin-coat a layer of 3um antistatic coating I on the upper surface of the PET, and then spin-coat a layer of 3um antistatic coating II on the lower surface of the PET; finally, dry at 80°C to obtain a double-antistatic substrate.

[0036] The preparation process of antistatic coating I is:

[0037] The following components were weighed respectively by mass percentage: 2wt% of hexamethylene diisocyanate, 2wt% of 2,2-bis(hydroxymethyl)propionic acid, 10wt% of aqueous polyurethane, 2wt% of cationic guar gum, 0.002wt% of wetting agent, and 83.998wt% of water, and stirred at 600r / min for 20min in a mixer.

[0038] The preparation process of antistatic coating II is as follows: 4wt% hexamethylene diisocyanate, 4wt% 2,2-bis(hydroxymethyl)propionic acid, 10wt% aqueous polyurethane, 0.002wt% wetting agent, 81.9984wt% water, stirring at 600r / min for 20min in a mixer to obtain antistatic coating II.

[0039] Step 2, take a PET film with a thickness of 5um, spin-coat a layer of 3um antistatic coating III on the upper and lower surfaces of the PET respectively, and then dry it at 80°C to obtain a double anti-release film.

[0040] The preparation process of antistatic coating III is:

[0041] The following components were weighed respectively by mass percentage: 2 wt % of cationic guar gum, 10 wt % of aqueous polyurethane, 2 wt % of acrylic acid, 0.002 wt % of wetting agent, and 85.998 wt % of water, and stirred at 600 r / min for 20 min to obtain an antistatic coating III.

[0042] Step 3, preparation of PU protective film: first, spin coat a layer of adhesive on the lower surface of the double-resistance substrate to form an adhesive layer. The thickness of the adhesive layer is 3um and is dried at 80°C. Then, it is compounded with the double-resistance release film, rolled up, and aged at 40°C for 40 hours to obtain the PU protective film.

[0043] The adhesive components of the adhesive layer are: 10% wt of polyvinyl alcohol, 10% wt of silicon phosphate, 10% wt of acrylate, 10% wt of dimethyldivinylsilane, 20% wt of epoxy acrylate, 20% wt of N-dodecyldimethylamine, 5% wt of hexamethylene diisocyanate, and 15% wt of 2,2-bis(hydroxymethyl)propionic acid.

[0044] Comparative Example 1 (the antistatic coating II on the lower surface of the double-resistance substrate in Example 1 was replaced with antistatic coating III, and the adhesive had the same force as the substrate and the release layer, and the release layer could not be accurately released)

[0045] Preparation of double-antistatic substrate: First, take a PET film with a thickness of 25um, spin-coat a layer of 3um antistatic coating I on the upper surface of the PET; spin-coat a layer of 3um antistatic coating III on the lower surface of the PET; then dry it at 80℃ for later use.

[0046] Preparation of double anti-release film: First, take a PET film with a thickness of 5um, spin-coat a layer of 3um antistatic coating III on the upper and lower surfaces of the PET, and then dry it at 80℃ for use.

[0047] Preparation of PU protective film: First, a layer of adhesive was spin-coated on the lower surface of the double-resistance substrate to form an adhesive layer. The thickness of the adhesive layer was 3um and it was dried at 80°C. Then it was compounded with the double-resistance release film, rolled up, and aged at 40°C for 40 hours to obtain the PU protective film.

[0048] Antistatic coating I: 2wt% of hexamethylene diisocyanate, 2wt% of 2,2-bis(hydroxymethyl)propionic acid, 10wt% of aqueous polyurethane, 2wt% of cationic guar gum, 0.002wt% of wetting agent, and 83.998wt% of water were mixed, and stirred at 600r / min for 20min in a mixer to obtain antistatic coating I.

[0049] Antistatic coating III: 2 wt% of cationic guar gum, 10 wt% of waterborne polyurethane, 2 wt% of acrylic acid, 0.002 wt% of wetting agent and 85.998 wt% of water were mixed and stirred at 600 r / min for 20 min in a mixer to obtain the antistatic coating.

[0050] The adhesive components of the adhesive layer include: 10% wt of polyvinyl alcohol, 10% wt of silicon phosphate, 10% wt of acrylate, 10% wt of dimethyldivinylsilane, 20% wt of epoxy acrylate, 20% wt of N-dodecyldimethylamine, 5% wt of hexamethylene diisocyanate, and 15% wt of 2,2-bis(hydroxymethyl)propionic acid.

[0051] Comparative Example 2 (hexamethylene diisocyanate was removed from the adhesive of Example 1, resulting in adhesive residue)

[0052] Preparation of double-antistatic substrate: First, take a PET film with a thickness of 25um, spin-coat a layer of 3um antistatic coating I on the upper surface of the PET; spin-coat a layer of 3um antistatic coating II on the lower surface of the PET; then dry it at 80℃ for later use.

[0053] Preparation of double anti-release film: First, take a PET film with a thickness of 5um, spin-coat a layer of 3um antistatic coating III on the upper and lower surfaces of the PET, and then dry it at 80℃ for use.

[0054] Preparation of PU protective film: First, a layer of adhesive was spin-coated on the lower surface of the double-resistance substrate. The thickness of the adhesive layer was 3um and it was dried at 80°C. Then it was compounded with the double-resistance release film, rolled up, and aged at 40°C for 40 hours to obtain the PU protective film.

[0055] Antistatic coating I: 2 wt% of hexamethylene diisocyanate, 2 wt% of 2,2-bis(hydroxymethyl)propionic acid, 10 wt% of waterborne polyurethane, 2 wt% of cationic guar gum, 0.002 wt% of wetting agent and 83.998 wt% of water were mixed and stirred at 600 r / min for 20 min in a mixer.

[0056] Antistatic coating II: 4 wt% of hexamethylene diisocyanate, 2 wt% of 2,2-bis(hydroxymethyl)propionic acid, 10 wt% of waterborne polyurethane, 0.002 wt% of wetting agent and 83.998 wt% of water were mixed and stirred at 600 r / min for 20 min in a mixer.

[0057] Antistatic coating III: 2 wt% of cationic guar gum, 10 wt% of waterborne polyurethane, 2 wt% of acrylic acid, 0.002 wt% of wetting agent and 85.998 wt% of water were mixed and stirred at 600 r / min for 20 min in a mixer to obtain the antistatic coating.

[0058] The adhesive composition of the adhesive layer is: polyvinyl alcohol 10.53wt%, silicon phosphate 10.53wt%, acrylate 10.53wt%, dimethyldivinylsilane 10.53wt%, epoxy acrylate 21.05wt%, N-dodecyldimethylamine 21.05wt%, and 2,2-bis(hydroxymethyl)propionic acid 15.78wt%.

[0059] Comparative Example 3 (Compared with Example 1, the upper surface of the double-antistatic substrate is replaced by antistatic coating I with antistatic coating II, and the antistatic effect is insufficient)

[0060] Preparation of double-antistatic substrate: First, take a PET film with a thickness of 25um, and spin-coat a layer of 3um antistatic coating II on the upper and lower surfaces of the PET; then dry it at 80℃ for later use.

[0061] Preparation of double anti-release film: First, take a PET (polyethylene terephthalate) film with a thickness of 5um, spin-coat a layer of 3um antistatic coating III on the upper and lower surfaces of the PET, and then dry it at 80°C for use.

[0062] Preparation of PU protective film: First, a layer of adhesive was spin-coated on the lower surface of the double-resistance substrate. The thickness of the adhesive layer was 3um and it was dried at 80°C. Then it was compounded with the double-resistance release film, rolled up, and aged at 40°C for 40 hours to obtain the PU protective film.

[0063] Antistatic coating II: After mixing 4 wt% of hexamethylene diisocyanate, 2 wt% of 2,2-bis(hydroxymethyl)propionic acid, 10 wt% of waterborne polyurethane, 0.002 wt% of wetting agent and 83.998 wt% of water, stir at 600 r / min for 20 min to obtain the antistatic coating.

[0064] Antistatic coating III: 2 wt% of cationic guar gum, 10 wt% of waterborne polyurethane, 2 wt% of acrylic acid, 0.002 wt% of wetting agent and 85.998 wt% of water were mixed and stirred at 600 r / min for 20 min to obtain antistatic coating III.

[0065] The adhesive composition of the adhesive layer: 10wt% polyvinyl alcohol, 10wt% silicon phosphate, 10wt% acrylate, 10wt% dimethyldivinylsilane, 20wt% epoxy acrylate, 20wt% N-dodecyldimethylamine, 5wt% hexamethylene diisocyanate, and 15wt% 2,2-bis(hydroxymethyl)propionic acid.

[0066] The performance test results of the PU protective films prepared in the above Example 1 and Comparative Examples 1 to 3 are shown in Table 1 below:

[0067] Table 1

[0068]

[0069] It can be seen from Table 1 that in Comparative Example 1, the antistatic coating 3 is used on the lower surface of the substrate and the release layer, so that the forces between the adhesive and the substrate and the release layer are the same, both of which are 0.03N / 50mm. Only when the forces between the adhesive and the substrate and the release layer are greater than the forces between the adhesive and the substrate, the release layer can be effectively peeled off when the PU protective film is used. Since hexamethylene diisocyanate is used as an effective adhesive component, and the difunctional monomer can form a three-dimensional cross-linked structure with the adhesive macromolecule after polymerization. The lack of hexamethylene diisocyanate in Comparative Example 2 reduces the adhesion between the release film and the substrate, as well as the adhesion with PMMA. At the same time, the adhesive macromolecule cannot form a three-dimensional structure, so that the molecular chain is easily displaced when the protective film is peeled off, so that the adhesive remains when peeled off. Cationic guar gum has good antistatic properties. In Comparative Example 3, after removing the cationic guar gum, its antistatic properties are reduced (the resistance is 10 6 Increase to 10 10 )

[0070] Figure 21 is a comparison diagram of the bonding force between the substrate and the bonding layer in Example 1 of the method for preparing the PU protective film for the permanent support film of the flexible electronic device of the present invention and Comparative Examples 1 to 3. Figure 2 It can be seen that the bonding force between the substrate and the adhesive in Example 1, Comparative Examples 2 and 3 is greater than the release peeling force, and the PU protective film can be effectively peeled off when pasted. However, in Comparative Example 2, the bonding force between the substrate and the adhesive is equal to the release peeling force, and there is peeling between the substrate and the adhesive, making the PU protective film unusable.

[0071] Example 2

[0072] Step 1, take a PET film with a thickness of 40um, spin-coat a layer of 5um antistatic coating I on the upper surface of the PET, and then spin-coat a layer of 5um antistatic coating II on the lower surface of the PET; finally, dry at 120°C to obtain a double-antistatic substrate.

[0073] The preparation process of antistatic coating I is:

[0074] The following components were weighed respectively by mass percentage: 5wt% of hexamethylene diisocyanate, 5wt% of 2,2-bis(hydroxymethyl)propionic acid, 15wt% of aqueous polyurethane, 5wt% of cationic guar gum, 0.3wt% of wetting agent, and 69.7wt% of water, and stirred at 600r / min for 20min in a mixer.

[0075] The preparation process of antistatic coating II is as follows: 10wt% hexamethylene diisocyanate, 2wt% 2,2-bis(hydroxymethyl)propionic acid, 15wt% aqueous polyurethane, 0.3wt% wetting agent, 72.7wt% water, stirring at 600r / min for 20min in a mixer to obtain antistatic coating II.

[0076] Step 2, take a PET film with a thickness of 10um, spin-coat a layer of 5um antistatic coating III on the upper and lower surfaces of the PET respectively, and then dry it at 120°C to obtain a double anti-release film.

[0077] The preparation process of antistatic coating III is:

[0078] The following components were weighed respectively by mass percentage: 5 wt % of cationic guar gum, 15 wt % of aqueous polyurethane, 5 wt % of acrylic acid, 0.3 wt % of wetting agent, and 74.7 wt % of water, and stirred at 600 r / min for 20 min to obtain an antistatic coating III.

[0079] Step 3, preparation of PU protective film: first, spin coat a layer of adhesive on the lower surface of the double-resistance substrate to form an adhesive layer. The thickness of the adhesive layer is 6um and is dried at 120°C. Then, it is compounded with the double-resistance release film, rolled up, and aged at 50°C for 60 hours to obtain the PU protective film.

[0080] The adhesive components of the adhesive layer are: polyvinyl alcohol 15% wt, silicon phosphate 15% wt, acrylate 15% wt, dimethyldivinylsilane 15% wt, epoxy acrylate 15% wt, N-dodecyldimethylamine 15% wt, hexamethylene diisocyanate 5% wt, and 2,2-bis(hydroxymethyl)propionic acid 5% wt.

[0081] Example 3

[0082] Step 1, take a PET film with a thickness of 30um, spin-coat a layer of 4um antistatic coating I on the upper surface of the PET, and then spin-coat a layer of 4um antistatic coating II on the lower surface of the PET; finally, dry it at 100°C to obtain a double-antistatic substrate.

[0083] The preparation process of antistatic coating I is:

[0084] The following components were weighed respectively by mass percentage: 3 wt % of hexamethylene diisocyanate, 4 wt % of 2,2-bis(hydroxymethyl)propionic acid, 12 wt % of aqueous polyurethane, 3 wt % of cationic guar gum, 0.1 wt % of wetting agent, and 77.9 wt % of water, and stirred at 600 r / min for 20 min in a mixer.

[0085] The preparation process of antistatic coating II is as follows: 8wt% hexamethylene diisocyanate, 3wt% 2,2-bis(hydroxymethyl)propionic acid, 12wt% aqueous polyurethane, 0.1wt% wetting agent, 76.9wt% water, stirring at 600r / min for 20min in a mixer to obtain antistatic coating II.

[0086] Step 2, take a PET film with a thickness of 8um, spin-coat a layer of 4um antistatic coating III on the upper and lower surfaces of the PET respectively, and then dry it at 100°C to obtain a double anti-release film.

[0087] The preparation process of antistatic coating III is:

[0088] The following components were weighed respectively by mass percentage: 3 wt % of cationic guar gum, 12 wt % of aqueous polyurethane, 3 wt % of acrylic acid, 0.1 wt % of wetting agent, and 81.9 wt % of water, and stirred at 600 r / min for 20 min to obtain an antistatic coating III.

[0089] Step 3, preparation of PU protective film: first, spin coat a layer of adhesive on the lower surface of the double-resistance substrate to form an adhesive layer. The thickness of the adhesive layer is 5um and is dried at 100°C. Then, it is compounded with the double-resistance release film, rolled up, and aged at 45°C for 50 hours to obtain the PU protective film.

[0090] The adhesive components of the adhesive layer are: 20% wt of polyvinyl alcohol, 15% wt of silicon phosphate, 20% wt of acrylate, 10% wt of dimethyldivinylsilane, 10% wt of epoxy acrylate, 10% wt of N-dodecyldimethylamine, 5% wt of hexamethylene diisocyanate, and 10% wt of 2,2-bis(hydroxymethyl)propionic acid.

[0091] Example 4

[0092] Step 1, take a PET film with a thickness of 30um, spin-coat a layer of 4um antistatic coating I on the upper surface of the PET, and then spin-coat a layer of 4um antistatic coating II on the lower surface of the PET; finally, dry it at 100°C to obtain a double-antistatic substrate.

[0093] The preparation process of antistatic coating I is:

[0094] The following components were weighed respectively by mass percentage: 3 wt % of hexamethylene diisocyanate, 4 wt % of 2,2-bis(hydroxymethyl)propionic acid, 12 wt % of aqueous polyurethane, 3 wt % of cationic guar gum, 0.1 wt % of wetting agent, and 77.9 wt % of water, and stirred at 600 r / min for 20 min in a mixer.

[0095] The preparation process of antistatic coating II is as follows: 8wt% hexamethylene diisocyanate, 3wt% 2,2-bis(hydroxymethyl)propionic acid, 12wt% aqueous polyurethane, 0.1wt% wetting agent, 76.9wt% water, stirring at 600r / min for 20min in a mixer to obtain antistatic coating II.

[0096] Step 2, take a PET film with a thickness of 8um, spin-coat a layer of 4um antistatic coating III on the upper and lower surfaces of the PET respectively, and then dry it at 100°C to obtain a double anti-release film.

[0097] The preparation process of antistatic coating III is:

[0098] The following components were weighed respectively by mass percentage: 3 wt % of cationic guar gum, 12 wt % of aqueous polyurethane, 3 wt % of acrylic acid, 0.1 wt % of wetting agent, and 81.9 wt % of water, and stirred at 600 r / min for 20 min to obtain an antistatic coating III.

[0099] Step 3, preparation of PU protective film: first, spin coat a layer of adhesive on the lower surface of the double-resistance substrate to form an adhesive layer. The thickness of the adhesive layer is 5um and is dried at 100°C. Then, it is compounded with the double-resistance release film, rolled up, and aged at 45°C for 50 hours to obtain the PU protective film.

[0100] The adhesive components of the adhesive layer are: 10% wt of polyvinyl alcohol, 20% wt of silicon phosphate, 10% wt of acrylate, 20% wt of dimethyldivinylsilane, 10% wt of epoxy acrylate, 10% wt of N-dodecyldimethylamine, 15% wt of hexamethylene diisocyanate, and 5% wt of 2,2-bis(hydroxymethyl)propionic acid.

[0101] The method for preparing the PU protective film for the permanent support film of flexible electronic devices of the present invention is characterized in that the double-antistatic substrate and the double-antistatic release film structure of the present invention contain four antistatic layers, which can achieve the antistatic effect before and after use. Three different antistatic coatings are designed, and the antistatic properties of the double-antistatic substrate and the double-antistatic release film can be adjusted by components, and the difference in the release force and the peeling force can be adjusted by utilizing the difference in the antistatic coating components.

Claims

1. Preparation method of PU protective film for permanent support film of flexible electronic devices, Features: The specific steps include: Step 1, preparing a double antibody substrate; The specific process of step 1 is: take a PET film with a thickness of 25um-40um, spin-coat a layer of 3um-5um antistatic coating I on the upper surface of the PET, and then spin-coat a layer of 3um-5um antistatic coating II on the lower surface of the PET; finally, dry at 80℃-120℃ to obtain a double anti-static substrate; The preparation process of the antistatic coating I is: The following components are weighed respectively by mass percentage: 2wt%-5wt% of hexamethylene diisocyanate, 2wt%-5wt% of 2,2-bis(hydroxymethyl)propionic acid, 10wt%-15wt% of aqueous polyurethane, 2wt%-5wt% of cationic guar gum, 0.002wt%-0.3wt% of a wetting agent, and the remaining component is water, and the sum of the mass percentages of the above components is 100%. After mixing and stirring the above components, an antistatic coating I is obtained; The preparation process of the antistatic coating II is: The following components are weighed respectively by mass percentage: 4wt%-10wt% of hexamethylene diisocyanate, 2%-5% of 2,2-bis(hydroxymethyl)propionic acid, 10wt%-15wt% of waterborne polyurethane, 0.002wt%-0.3wt% of a wetting agent, and the remaining component is water, and the sum of the mass percentages of the above components is 100%. After mixing and stirring the above components, an antistatic coating II is obtained; Step 2, preparing a double-resistance release film; The specific process of step 2 is: Take a PET film with a thickness of 5um-10um, spin-coat a layer of 3um-5um antistatic coating III on the upper and lower surfaces of the PET, and then dry it at 80℃-120℃ to obtain a double anti-release film; In the step 2, the preparation process of the antistatic coating III is: The following components are weighed respectively by mass percentage: 2wt%-5wt% of cationic guar gum, 10wt%-15wt% of waterborne polyurethane, 2wt%-5wt% of acrylic acid, 0.002wt%-0.3wt% of a wetting agent, and the remaining component is water, and the sum of the mass percentages of the above components is 100%. After mixing and stirring the above components, an antistatic coating III is obtained; Step 3, spin-coating a layer of adhesive on the lower surface of the double-resistance substrate prepared in step 1 to form an adhesive layer, and drying it at 80°C-120°C, and then compounding it with the double-resistance release film prepared in step 2, rolling it up, and ripening it at 40°C-50°C for 40h-60h to obtain a PU protective film; In step 3, the components of the adhesive include: 10%wt-20%wt of polyvinyl alcohol, 10wt%-20wt% of silicon phosphate, 10wt%-20wt% of acrylate, 10wt%-20wt% of dimethyldivinylsilane, 10wt%-20wt% of epoxy acrylate, 10wt%-20wt% of N-dodecyldimethylamine, 5wt%-15wt% of hexamethylene diisocyanate, and 5wt%-15wt% of 2,2-bis(hydroxymethyl)propionic acid, and the sum of the mass percentages of the above components is 100%.