Preparation method of low-oxygen CuCr alloy contact material

By introducing Al elements into the CuCr alloy and utilizing internal oxidation reaction, the oxygen content of the CuCr contact material is reduced, the problem of reducing vacuum degree in the vacuum chamber and discontinuity of powder deposition is solved, and the conductivity and hardness of the material are improved. A more efficient forming process is achieved.

CN117535544BActive Publication Date: 2024-12-06DONGGUAN JINGWEI NEW MATERIALS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202311373166.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-10-23
Publication Date
2024-12-06
Estimated Expiration
2043-10-23

AI Technical Summary

Technical Problem

In the existing CuCr contact material forming process, it is difficult to effectively reduce the oxygen content of the material, resulting in a decrease in the vacuum degree of the vacuum chamber. In addition, the two materials have interference and continuous deposition problems during the double-spraying powder.

Method used

A small amount of Al elements were introduced during the preparation of CuCr alloy. The internal oxidation reaction principle of Al was used to seize oxygen atoms in the CuCr alloy under high temperature conditions to generate a third phase of Al2O3 with a diffuse state distribution. Through cold spraying technology and internal oxidation and timely effect Process to reduce the oxygen content of contact material.

Benefits of technology

It significantly reduces the oxygen content of CuCr contact material, improves its conductivity and hardness, enhances the insulation strength and breaking capacity of the vacuum arc extinguishing chamber, solves the problem of excessive oxygen content of the material, and improves the continuous powder deposition sex.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117535544B_ABST
    Figure CN117535544B_ABST
Patent Text Reader

Abstract

The present invention discloses a method for preparing a low-oxygen CuCr alloy contact material, comprising the following steps: (1) uniformly mixing CuAl alloy powder and Cr powder to obtain a mixed powder; (2) cold spraying the mixed powder to obtain a blank; (3) subjecting the blank to an internal oxidation and aging process. In the preparation process of the CuCr alloy, the present invention introduces a small amount of Al element into the material formula, utilizes the internal oxidation reaction principle of Al, enables the Al element to capture oxygen atoms in the CuCr alloy under high temperature conditions, and generates Al in a dispersed state. 2 O 3 The third phase greatly reduces the oxygen content in the CuCr alloy contact material formed by the cold spraying process, so that the product has good electrical conductivity and higher hardness.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a method for preparing a low-oxygen CuCr alloy contact material. Background Art

[0002] The contact is one of the key components of the switchgear. The main performance and life of the switchgear depend largely on the quality of the contact material. The contact material is usually required to have good conductivity, low contact resistance, high resistance to welding, high resistance to arc erosion and resistance to material transfer. For vacuum contact materials, it is also required to have a small cutoff value, high compressive strength and high breaking capacity. The microstructure of the contact material has an important influence on its macroscopic performance. CuCr alloy is a typical medium and high voltage contact material. It has the characteristics of "pseudo-alloy": Cu and Cr are not miscible with each other. In terms of organization, it is physically combined by two immiscible metal powders. Cu has high thermal conductivity, high electrical conductivity and good plasticity, but pure Cu has low resistance to welding and mechanical strength; Cr has a high melting point, high mechanical strength, and strong air absorption ability. CuCr pseudoalloy has the characteristics of both Cr and Cu metals: good arc erosion resistance, high voltage resistance, large breaking current capacity, excellent current carrying capacity, high voltage resistance, low cutoff current, and its excellent current breaking capacity and arc erosion resistance are unmatched by other contact materials. For copper-chromium contacts, the gas composition in the material (including oxygen content and nitrogen content, mainly oxygen content) is a very important performance indicator (generally required to be less than 500ppm), which directly affects the working state of the vacuum interrupter. When the oxygen content in the contact is too high, under working conditions, oxygen is released from the contact material, which will greatly reduce the vacuum degree of the vacuum interrupter, which is fatal to vacuum devices. At present, the industrial molding processes of CuCr contact materials mainly include: mixed powder sintering method, arc melting method, vacuum casting method and vacuum infiltration method. The performance characteristics of products made by different molding methods are somewhat different. Copper-chromium contacts mainly choose the above appropriate methods to form rough blanks according to customer needs, and then obtain finished products through machining. Among them, the mixed powder sintering, vacuum infiltration and arc melting processes all have high requirements for the oxygen content of the raw materials, and the degassing effect is limited during the manufacturing process. Due to its process characteristics, the vacuum melting method can effectively degas during the melting process, thereby reducing the gas content of the material to a certain extent. In the prior art, there is no better method to deoxidize and remove impurities from the formed copper-chromium alloy.

[0003] In recent years, with the development of vacuum switches towards miniaturization and intelligence and increasingly fierce market competition, the industry has been seeking to develop new production processes: on the one hand, seeking shorter production processes to reduce production costs; on the other hand, seeking new processes and technologies that can improve the comprehensive performance of contact materials. In terms of the manufacturing and molding process of CuCr contacts, a variety of new process explorations have emerged: for example, patent CN202110310961 mentions a technology for preparing CuCr contacts using 3D printing technology; patent 202010316328.X mentions an exploration of producing CuCr contacts using laser cladding technology. Patent 202010575151.5 mentions a process attempt to prepare CuCr contact materials using a dual-nozzle cold spraying device: Cu powder and Cr powder are respectively filled into two storage containers of the cold spraying equipment. During spraying, the two nozzles control the Cu powder and Cr powder separately, and the two metal powders are focused 1mm away from the surface of the substrate; after one layer of spraying is completed, the substrate is placed in a press and the coating surface is compacted by mechanical force; then the coating surface of the substrate is re-sandblasted and roughened, and then the substrate is lowered by 20-50mm to continue spraying the next layer. After each layer of spraying is completed, the coating surface needs to be mechanically compacted and sandblasted until the final required thickness of the coating is reached. However, this process exploration failed to solve the problem of interference between the two materials during dual-nozzle powder spraying and the continuous and effective deposition of the two powders. Summary of the invention

[0004] In view of the defects of the prior art, the inventive concept of the present invention is to introduce a small amount of Al element into the material formula during the preparation process of CuCr alloy, and utilize the internal oxidation reaction principle of Al to enable the Al element to capture oxygen atoms in the CuCr alloy under high temperature conditions to generate a dispersed Al2O3 third phase, thereby significantly reducing the oxygen content in the CuCr alloy contact material formed by the cold spraying process.

[0005] A method for preparing a low-oxygen CuCr alloy contact material comprises the following steps:

[0006] (1) Mixing CuAl alloy powder and Cr powder uniformly;

[0007] (2) Cold spraying;

[0008] (3) Internal oxidation and aging process.

[0009] Preferably, a method for preparing a low-oxygen CuCr alloy contact material comprises the following steps:

[0010] (1) uniformly mixing CuAl alloy powder and Cr powder to obtain mixed powder;

[0011] (2) cold spraying the mixed powder to obtain a blank;

[0012] (3) performing internal oxidation and aging processes on the blank.

[0013] Preferably, in step (1), the Al content in the CuAl alloy powder is 0.1-0.9wt%.

[0014] Preferably, the CuAl alloy powder is prepared by the following method: mixing and smelting metal copper and metal aluminum, and obtaining the CuAl alloy powder by an inert gas atomization method. Further preferably, the CuAl alloy powder is prepared by the following method: smelting metal Cu with a purity of 99.99% and metal Al with a purity of 99.99% according to a designed ratio, and obtaining the CuAl alloy powder by an inert gas atomization method. Further preferably, the CuAl alloy powder with a particle size range of 5-53 μm is screened out.

[0015] Preferably, in step (1), the Cr powder is spherical powder prepared by inert gas atomization, or irregularly shaped high-purity Cr powder produced by other methods, with a purity of >99.99% and an oxygen content of 200-5000ppm; further preferably, the particle size of the Cr powder is in the range of 5-38μm.

[0016] Preferably, in step (1), the final percentage of CuAl alloy powder and Cr powder after mixing is Cu 余 Al (0.1-0.9)wt% Cr (5-55wt%) .

[0017] Preferably, the step (1) is to mix the CuAl alloy powder and the Cr powder in a mixer for 2-10 hours.

[0018] Preferably, the specific process of cold spraying in step (2) is as follows: the working gas is an inert gas, preferably nitrogen, the spraying pressure is 6-9Mpa, the working gas heating temperature is 600-900°C, and the powder feeding efficiency is 200-400g / min. Preferably, the thickness of the sprayed layer is 0.2-10mm, which can be accumulated by multiple spraying. Preferably, in step (3), the internal oxidation reaction is carried out at a temperature of 900-950°C in an oxygen-free environment, and the insulation time is 30-120min. Preferably, the internal oxidation reaction is carried out in a vacuum furnace, and the vacuum degree should be higher than 8×10 -3 Preferably, the furnace temperature is then lowered to 500-700°C for 1-4 hours for aging treatment, and then cooled to room temperature. Finally, a CuCr contact with an oxygen content of less than 200 ppm can be obtained.

[0019] In the preparation process of the CuCr alloy, the present invention introduces a small amount of Al element into the material formula, and utilizes the internal oxidation reaction principle of Al to enable the Al element to capture oxygen atoms in the CuCr alloy under high temperature conditions to generate a third phase of Al2O3 distributed in a dispersed state, so that the oxygen content in the CuCr alloy contact material formed by the cold spraying process is greatly reduced, so that the product has good electrical conductivity and high hardness. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0021] Figure 1 It is a metallurgical-grade bonding interface diagram of the Cu-CuCr coating of the present invention;

[0022] Figure 2 This is the island-like distribution diagram of Cr in the sprayed layer of the present invention;

[0023] Figure 3 It is the effect diagram of the aging process of the present invention. DETAILED DESCRIPTION

[0024] A method for preparing a low-oxygen CuCr alloy contact material comprises the following steps:

[0025] (1) Mix the CuAl alloy powder and Cr powder in a mixer for 2-10 hours until they are evenly mixed to obtain CuAl 0.1-0.9wt% Mixed powder, that is, the Al content in the CuAl alloy powder is 0.1-0.9wt%. The CuAl alloy powder is prepared by the following method: metal copper and metal aluminum are mixed and smelted, and the CuAl alloy powder is obtained by an inert gas atomization method. Further preferably, the CuAl alloy powder is prepared by the following method: metal Cu with a purity of 99.99% and metal Al with a purity of 99.99% are smelted according to the designed ratio, and the CuAl alloy powder is obtained by an inert gas atomization method. Then, the CuAl alloy powder with a particle size range of 5-53μm is screened out. The Cr powder is a spherical powder prepared by an inert gas atomization method, or an irregularly shaped high-purity Cr powder produced by other methods, with a purity of >99.99%, and the oxygen content of the Cr powder is 200-5000ppm; further preferably, the particle size range of the Cr powder is 5-38μm. The final percentage of the CuAl alloy powder after mixing with the Cr powder is Cu 余 Al (0.1-0.9)wt% Cr (5-55wt%), that is, the mass ratio of CuAl alloy powder to Cr powder in the CuAlCr alloy powder is (45-95):(5-55).

[0026] Raw material selection and proportion: In the embodiment, electrolytic Cu plate raw material and 4N pure Al ingot raw material were selected to ensure the purity of the final alloy and avoid the adverse effects of impurity elements on the performance.

[0027] Melting: The electrolytic Cu plate and high-purity Al ingot are mixed and then melted. The purpose of this step is to make the copper and aluminum fully mixed and evenly form a solid solution alloy.

[0028] Inert gas atomization method: CuAl alloy powder is obtained by inert gas atomization. This method forms metal atomized droplets by exposing molten metal to high-pressure inert gas (usually nitrogen or argon), which quickly solidify in flight to form metal powder. This method can produce metal powder with uniform particle size, regular shape and high purity.

[0029] Control of Al content: The Al content in the CuAl alloy powder prepared in this embodiment is controlled at 0.3wt%. The Al content is obtained after equivalent calculation based on the total oxygen content of the raw material powder and the empirical value of oxygen introduced during the cold spraying process.

[0030] In summary, each link is to prepare CuAl alloy powder with uniform composition and particle size distribution that meets the requirements. This powder will be mixed with Cr powder and then undergo cold spraying, internal oxidation, aging and other steps in the subsequent steps to finally obtain low-oxygen CuCr alloy contact material.

[0031] (2) The mixed powder is subjected to cold spraying to obtain a composite blank (i.e. blank); the specific cold spraying process is as follows: the working gas is an inert gas, preferably nitrogen, the spraying pressure is 6-9 MPa, the working gas heating temperature is 600-900°C, and the powder feeding efficiency is 200-400 g / min. Preferably, the spraying thickness is 0.2-10 mm, and usually multiple sprayings are required to obtain the desired coating thickness.

[0032] Cold spraying is a new material surface modification technology. Usually, the powder material is heated to a certain temperature where the material has not yet melted. The plastic powder material is then carried by supersonic gas to make the powder hit the substrate at a very high speed. When the powder flying speed exceeds a certain critical value, it can be deposited on the substrate to form a coating. However, usually only metal powders with good plasticity are suitable for cold spraying.

[0033] CuAl alloy powder and Cr powder are both completely solid and carried by the heated supersonic airflow, and impact on the surface of the metal substrate along the axial direction. The CuAl alloy powder undergoes large plastic deformation and is deposited on the metal substrate. The Cr powder is relatively brittle and hard, and the impact deformation is small. After being accelerated, it is embedded with the copper powder and deposited on the substrate together to obtain a high-density (>98.5%) composite material coating. The interface between the coating and the copper substrate is metallurgical-grade bonded, and Cr is distributed in the coating in an island shape, which meets the microstructural requirements of the CuCr contact material.

[0034] The cold spraying process is the process of preparing CuAl 0.3wt% :Cr composite materials, it realizes the uniform distribution of Al atoms in the CuCr contact material through precise process parameters and equipment, and realizes the high-density forming of CuCr contacts with a forming technology different from the traditional powder metallurgy process, laying the foundation for the next step to obtain low-oxygen CuCr alloy contact materials with excellent performance, stability and reliability.

[0035] (3) The composite embryo plate is subjected to internal oxidation and aging process. The internal oxidation reaction is carried out in a vacuum furnace with a vacuum degree higher than 8×10 -3 Pa, 900-950℃, holding time 30-120min; in this process, since Al element is more active than Cr and Cu, Al atoms in CuAl alloy powder will capture oxygen atoms in the coating as oxygen source for internal oxidation reaction, regardless of whether these oxygen atoms are brought in by raw material powders such as Cu and Cr or introduced in the cold spraying process. The harmful oxygen content in the sprayed layer can be greatly reduced through internal oxidation reaction, and the contact material can be purified. The product of internal oxidation reaction is a tiny third phase of Al2O3, which is dispersed in the CuCr contact material. The presence of dispersed alumina phase can further improve the insulation strength and breaking capacity of the vacuum interrupter. The internal oxidation of the present invention is a key process. By accurately calculating and introducing a small amount of Al element, it just consumes the oxygen atoms in the CuCr material in the internal oxidation reaction, realizes effective purification and oxygen reduction of the contact material, and generates dispersed alumina phase beneficial to the material performance, and finally obtains CuCr contact material with excellent comprehensive performance.

[0036] Then the furnace temperature is lowered to 500-700℃ and kept for 1-4 hours for aging process. The aging process can promote the solid solution and lattice precipitation of the two phases in the CuCr material, further improve the hardness of the contact material, improve the conductivity, and enable the material to obtain better comprehensive performance.

[0037] Then, flowing nitrogen is filled into the vacuum furnace to accelerate the cooling speed of the blank, and the blank can be taken out when it is cooled to below 150°C. Finally, a CuCr contact with an oxygen content of less than 200ppm can be obtained.

[0038] Furthermore, adding metal Mg on the basis of Al in the alloy powder further improves the performance of the alloy.

[0039] Specifically, preferably, in step (1), the CuAl alloy powder is replaced with CuAlMg alloy powder, wherein the Al content is 0.05-0.45wt%, the Mg content is 0.05-0.45wt%, and the balance is Cu. Preferably, the Al content is 0.1-0.3wt%, and the Mg content is 0.1-0.3wt%.

[0040] After internal oxidation reaction, aging process and rapid cooling, a low-oxygen CuCr alloy contact material with excellent performance is finally obtained on a pure Cu substrate. This low-oxygen CuCr alloy contact material obtained by precisely controlling process parameters has excellent application prospects in electrical equipment. Its excellent electrical conductivity and hardness make it widely used in electrical components such as circuit breakers and contactors.

[0041] Embodiment 1:

[0042] A method for preparing a low-oxygen CuCr alloy contact material comprises the following steps:

[0043] (1) Preparation of CuAlCr alloy powder:

[0044] Electrolytic Cu plates with a purity of 99.99% and Al ingots with a purity of 99.99% are made into CuAl 0.3wt% The ingredients are prepared according to the composition ratio (i.e., the Al content in CuAl is controlled to be 0.3wt%) and smelted, and CuAl alloy powder is obtained by inert gas atomization method, and then the alloy powder with a particle size range of 5-53μm is screened out, and the obtained CuAl 0.3wt% The oxygen content of the alloy powder is 350 ppm.

[0045] The CuAl 0.3wt% The alloy powder and the commercially available atomized spherical Cr powder with a particle size range of 5-38μm, an oxygen content of 800ppm, and a purity of >99.9% are CuAl 0.3wt% The weight percentage of Cu:Cr was 75:25, and the mixture was put into a V-type mixer and mixed for 6 hours to make it fully uniform. 余 Al 0.3wt% Cr 25wt% Mix metal powders.

[0046] (2) Cold spraying:

[0047] The mixed metal powder is input into the powder feeding system of the cold spraying equipment for cold spraying process operation. The specific process is: using nitrogen with a pressure of 7.5Mpa as the working gas, the working gas is heated to 750°C, and the gas carrying the mixed metal powder passes through the Laval nozzle to generate a supersonic airflow with a speed of 1000m / s, and the powder feeding efficiency is 300g / min. The mixed metal powder is cold sprayed onto the pure copper substrate to obtain a composite embryo plate, and the spraying thickness is controlled to be 6mm.

[0048] In the cold spraying step of the present invention, the CuAl alloy powder and the Cr raw material powder are first fully and evenly mixed, and then put into the powder feeding system of the cold spraying equipment, and only one nozzle is used to perform high-pressure supersonic cold spraying. During the spraying process, the CuAl alloy powder with better plasticity undergoes a large flow plastic deformation and is deposited on the metal substrate, and the plastic deformation of the Cr powder during spraying is relatively small, and the Cr powder is mainly deposited on the substrate together with the CuAl powder by mechanical biting and inlaying, and is sprayed layer by layer until a CuCr composite material layer of a required thickness is formed.

[0049] Figure 1 It is confirmed that the interface of the Cu-CuCr coating of the present invention has a metallurgical grade bonding effect; Figure 2 It shows that Cr in the Cu-CuCr coating of the present invention is distributed in an island shape.

[0050] (3) Internal oxidation and aging treatment:

[0051] The composite embryo plate is internally oxidized in a vacuum furnace and the vacuum degree is evacuated to 9×10 -3 Mpa, control the internal oxidation temperature at 930°C, and the reaction time for 1 hour.

[0052] The furnace temperature is then lowered to 600°C and kept warm for 1.5 hours for aging. Aging can further increase the hardness of the contact material, improve the electrical conductivity, and enable the material to obtain better overall performance.

[0053] Then fill the vacuum furnace with flowing nitrogen, cool it to below 150°C and take out the blank.

[0054] Figure 3 The effect of the aging process of the present invention is shown, and densely distributed fine chromium spots appear around the Cr particles.

[0055] Finally, the low-oxygen CuCr25 alloy contact material of the present invention is obtained on the pure Cu substrate.

[0056] Embodiment 2:

[0057] The difference from Example 1 is that step (3) includes internal oxidation and aging treatment. The specific step (3) is:

[0058] The composite embryo plate is internally oxidized in a vacuum furnace and the vacuum degree is evacuated to 9×10-3 Mpa, control the internal oxidation temperature at 930℃, and keep warm for 2 hours.

[0059] Then the furnace temperature was lowered to 650°C and kept for 1.5 hours for aging.

[0060] Then, flowing nitrogen is filled into the vacuum furnace to accelerate the cooling rate of the blank, and the blank is taken out after being cooled to below 150° C., and finally the low-oxygen CuCr25 alloy contact material of the present invention is obtained on a pure Cu substrate.

[0061] Embodiment 3:

[0062] The difference from Example 1 is that step (3) includes internal oxidation and aging treatment. The specific step (3) is:

[0063] The composite embryo plate is internally oxidized in a vacuum furnace and the vacuum degree is evacuated to 9×10 -3 Mpa, control the internal oxidation temperature at 930°C, and the reaction time for 2 hours.

[0064] Then the furnace temperature was lowered to 500°C and kept for 3 hours for aging.

[0065] Then, flowing nitrogen is filled into the vacuum furnace to accelerate the cooling rate of the blank, and the blank is taken out after being cooled to below 150° C., and finally the low-oxygen CuCr25 alloy contact material of the present invention is obtained on a pure Cu substrate.

[0066] Embodiment 4:

[0067] The difference from Example 1 is that in step 1, CuAl 0.3wt% Alloy powder and atomized spherical Cr powder (oxygen content 800ppm) according to CuAl 0.3wt% :Cr weight percentage 70:30 ingredients, Cu 余 Al 0.3wt% Cr 30wt% Mix metal powders.

[0068] Subsequently, cold spraying, internal oxidation, aging and other processes were performed according to the same process as in Example 1, and finally the low-oxygen CuCr30 alloy contact material of the present invention was obtained on a pure Cu substrate.

[0069] Embodiment 5:

[0070] The difference from Example 1 is that the chromium powder raw material used in step (1) is irregular chromium powder produced by electrolysis, and its oxygen content is measured to be 1800ppm. After equivalent calculation, the formula of the designed CuAl alloy is CuAl 0.1wt% , Cu 余 Al 0.1wt% Cr 30wt% Mix metal powders.

[0071] Subsequently, cold spraying, internal oxidation, aging and other processes were performed according to the same process as in Example 1, and finally the low-oxygen CuCr30 alloy contact material of the present invention was obtained on a pure Cu substrate.

[0072] Embodiment 6:

[0073] The difference from Example 1 is that the chromium powder raw material used in step (1) is irregular chromium powder produced by electrolysis, and its oxygen content is measured to be 1800ppm. After equivalent calculation, the formula of the designed CuAl alloy is CuAl 0.3wt% , Cu 余 Al 0.3wt% Cr 30wt% Mix metal powders.

[0074] Subsequently, cold spraying, internal oxidation, aging and other processes were performed according to the same process as in Example 1, and finally the low-oxygen CuCr30 alloy contact material of the present invention was obtained on a pure Cu substrate.

[0075] Embodiment 7:

[0076] The difference from Example 1 is that the chromium powder raw material used in step (1) is irregular chromium powder produced by electrolysis, and its oxygen content is measured to be 1800ppm. After equivalent calculation, the formula of the designed CuAl alloy is CuAl 0.9wt% , Cu 余 Al 0.9wt% Cr 30wt% Mix metal powders.

[0077] Subsequently, cold spraying, internal oxidation, aging and other processes were performed according to the same process as in Example 1, and finally the low-oxygen CuCr30 alloy contact material of the present invention was obtained on a pure Cu substrate.

[0078] Embodiment 8:

[0079] The difference from Example 1 is that the chromium powder raw material used in step (1) is irregular chromium powder produced by aluminothermic method, and its oxygen content is measured to be 3800ppm. After equivalent calculation, the formula of the designed CuAl alloy is CuAl 0.3wt% , Cu 余 Al 0.3wt% Cr 30wt% Mix metal powders.

[0080] Subsequently, cold spraying, internal oxidation, aging and other processes were performed according to the same process as in Example 1, and finally the low-oxygen CuCr30 alloy contact material of the present invention was obtained on a pure Cu substrate.

[0081] Embodiment 9:

[0082] The difference from Example 1 is that the chromium powder raw material used in step (1) is irregular chromium powder produced by aluminothermic method, and its oxygen content is measured to be 3800ppm. After equivalent calculation, the formula of the designed CuAl alloy is CuAl 0.9wt% , Cu 余 Al 0.9wt% Cr 30wt% Mix metal powders.

[0083] Subsequently, cold spraying, internal oxidation, aging and other processes were performed according to the same process as in Example 1, and finally the low-oxygen CuCr30 alloy contact material of the present invention was obtained on a pure Cu substrate.

[0084] Embodiment 10:

[0085] The difference from Example 1 is that the final content of CuAlCr alloy powder in step (1) is different. The CuAl alloy powder is still CuAl 0.2wt% The ratio of CuAl powder is 95wt%, the ratio of Cr is 5wt%, and Cu 余 Al 0.2wt% Cr 5wt% Mix metal powders.

[0086] Subsequently, cold spraying, internal oxidation, aging and other processes were performed according to the same process as in Example 1, and finally the low-oxygen CuCr5 alloy contact material of the present invention was obtained on a pure Cu substrate.

[0087] Embodiment 11:

[0088] The difference from Example 1 is that the final content of CuAlCr alloy powder in step (1) is different. The CuAl alloy powder is still CuAl 0.3wt% The ratio of CuAl powder is 50wt%, the ratio of Cr is 50wt%, and Cu 余 Al 0.3wt% Cr 50wt% Mix metal powders.

[0089] Subsequently, cold spraying, internal oxidation, aging and other processes are performed according to the same process as in Example 1, and finally the low-oxygen CuCr50 alloy contact material of the present invention is obtained on a pure Cu substrate.

[0090] Embodiment 12:

[0091] The difference from Example 1 is that the alloy powder is prepared differently in step (1).

[0092] Specifically, the alloy powder preparation in step (1) is as follows:

[0093] Electrolytic Cu plates with a purity of 99.99%, Al ingots with a purity of 99.99%, and magnesium bars with a purity of CuAl 0.15wt% Mg 0.15wt% The composition ratio of the CuMgAl alloy is controlled to be 0.15wt% Mg, 0.15wt% Al, and the balance is Cu) and smelted, and CuAlMg alloy powder is obtained by inert gas atomization method, and then the alloy powder with a particle size range of 5-53μm is screened out, and the obtained CuAl 0.15wt% Mg 0.15wt% The oxygen content of the alloy powder is 350 ppm.

[0094] The CuAl 0.15wt% Mg 0.15wt% The alloy powder and the commercially available atomized spherical Cr powder with a particle size range of 5-38μm, an oxygen content of 800ppm, and a purity of >99.9% are CuAl 0.15wt% Mg 0.15wt% The weight percentage of Cu:Cr was 75:25, and the mixture was put into a V-type mixer and mixed for 6 hours to make it fully uniform. 余 Al 0.15wt% Mg 0.15wt% Cr 25wt% Mix metal powders.

[0095] Subsequently, cold spraying, internal oxidation, aging and other processes were performed according to the same process as in Example 1, and finally the low-oxygen CuCr25 alloy contact material of the present invention was obtained on a pure Cu substrate.

[0096] Comparative Example 1:

[0097] The difference from Example 1 is the internal oxidation and aging treatment in step (3). Specifically, step (3) is as follows: the sample is not subjected to the internal oxidation process, and the composite embryo plate is directly subjected to aging at 600°C for 2 hours in a vacuum furnace, and then the composite embryo plate is cooled to room temperature in the furnace, and finally a CuCr25 alloy contact material for comparison is obtained on a pure Cu substrate.

[0098] Comparative Example 2:

[0099] The difference from Example 1 is that the chromium powder raw material used in step (1) is a commercially available spherical chromium powder produced by an inert gas atomization method, and its oxygen content is measured to be 800 ppm. Commercially available pure copper powder is used instead of CuAl alloy powder for batching, and the oxygen content of the pure copper powder is measured to be 350 ppm. CuCr 25wt% Mix metal powders.

[0100] Subsequently, cold spraying, internal oxidation, aging and other process flows were carried out according to the same process as in Example 1, and finally a CuCr25 alloy contact material for comparison was obtained on a pure Cu substrate.

[0101] Comparative Example 3:

[0102] The difference from Example 1 is that in step (1), irregular shaped chromium powder produced by commercial electrolysis is used, and its oxygen content is measured to be 1800ppm. Pure copper powder is used instead of CuAl alloy powder for mixing, and the oxygen content of pure copper powder is measured to be 350ppm. CuCr 30wt% Mix metal powders.

[0103] Subsequently, cold spraying, internal oxidation, aging and other process flows were carried out according to the same process as in Example 1, and finally a CuCr30 alloy contact material for comparison was obtained on a pure Cu substrate.

[0104] Comparative Example 4:

[0105] The difference from Example 1 is that the chromium powder raw material used in step (1) is irregular chromium powder produced by aluminothermic method, and its oxygen content is 3800ppm. Commercially available atomized pure copper powder is used instead of CuAl alloy powder for batching, and the oxygen content of pure copper powder is 350ppm. CuCr 30wt% Mix metal powders.

[0106] Subsequently, cold spraying, internal oxidation, aging and other process flows were carried out according to the same process as in Example 1, and finally a CuCr30 alloy contact material for comparison was obtained on a pure Cu substrate.

[0107] Comparative Example 5:

[0108] The difference from Example 1 is that the alloy powder is prepared differently in step (1).

[0109] Specifically, the alloy powder preparation in step (1) is as follows:

[0110] Electrolytic Cu plate with 99.99% purity and magnesium strip are made according to CuMg 0.3wt% The ingredients are prepared according to the composition ratio (i.e., the Mg content in CuMg is controlled to be 0.3wt%) and smelted, and CuMg alloy powder is obtained by inert gas atomization method, and then the alloy powder with a particle size range of 5-53μm is screened out, and the obtained CuMg 0.3wt% The oxygen content of the alloy powder is 350 ppm.

[0111] The CuMg 0.3wt% The alloy powder and the commercially available atomized spherical Cr powder with a particle size range of 5-38μm, an oxygen content of 800ppm, and a purity of >99.9% are CuMg 0.3wt% The weight percentage of Cu:Cr was 75:25, and the mixture was put into a V-type mixer and mixed for 6 hours to make it fully uniform. 余 Mg0.3wt% Cr 25wt% Mix metal powders.

[0112] Subsequently, cold spraying, internal oxidation, aging and other processes were carried out according to the same process as in Example 1, and finally a low-oxygen CuCr25 alloy contact material was obtained on a pure Cu substrate.

[0113] Test Example 1:

[0114] Table 1: CuCr alloy contact material performance test results

[0115]

[0116]

[0117] The first set of embodiments:

[0118] The material formulas of Examples 1, 2, 3 and Comparative Example 1 are all CuAl 0.3% Cr 25% , all use chromium powder with an oxygen content of 800ppm as raw material, and the CuAl alloy formula uses 0.3wt%. This group of samples mainly examines the effects of internal oxidation and aging process parameters on the oxygen content, hardness and conductivity of the contact material. The internal oxidation and aging process parameters can be further optimized according to the actual effect. From the test data of the above embodiments, it can be seen that appropriately extending the internal oxidation time can reduce the oxygen content in the contact material and improve the conductivity. Selecting a suitable aging temperature and time is conducive to the interface fusion between CuCr, and the material tends to obtain a higher hardness value. Although the same proportion of Al element is added to the formula of Comparative Example 1, the internal oxidation process is not performed, so the oxygen of the contact material cannot combine with Al to form aluminum oxide. After Al is added, not only the oxygen content cannot be reduced, but the added Al as an impurity element makes the conductivity of the material worse. No aluminum element is added to the formula of Comparative Example 2, and no internal oxidation reaction will occur to reduce the oxygen content in the material, so the oxygen brought in by the raw material and the oxygen brought in by the cold spraying process are retained.

[0119] The second set of embodiments:

[0120] Examples 5, 6, 7 and Comparative Example 3 all use electrolytic chromium powder with an oxygen content of 1800ppm as raw material, and the CuAl alloy formula is selected as 0.1wt%, 0.3wt%, and 0.9wt%. Comparative Example 3 is a formula without Al. This group of samples mainly examines the effect of Al content on the internal oxidation effect on the performance of the contact material. From the test data of the above embodiments, it can be seen that the appropriately added Al element can effectively reduce the oxygen content of the contact material finally obtained, but it is not the case that the more Al is added, the better. When the Al in the powder is consumed in the internal oxidation, the excess Al will have a negative effect on the conductivity of the material as an impurity element. Therefore, although the material has a low oxygen content, the overall performance of the material is not good enough. In the formula of Comparative Example 3, no aluminum element is added, and no internal oxidation reaction will occur to reduce the oxygen content in the material. Therefore, the oxygen introduced in the raw material and the oxygen introduced in the cold spraying process are retained. It can be seen that if the Al element is not introduced, the oxygen content of the electrolytic chromium powder is too high, and direct application to the contact material will result in an unqualified oxygen content in the product.

[0121] The third group of embodiments:

[0122] Examples 8, 9 and Comparative Example 4 all use aluminothermic chromium powder with an oxygen content of 3800ppm as raw material, and the CuAl alloy formula is selected as 0.3wt% and 0.9wt%, among which Comparative Example 4 is a formula without Al. This group of samples mainly examines whether it is possible to use aluminothermic chromium powder with a low price but high oxygen content to produce qualified contact materials by introducing Al elements. It can be seen from the test data of the above embodiments that as long as the equivalent calculation is performed based on the oxygen content data measured by the raw material and the appropriate Al content is introduced, the oxygen content of the contact material can be effectively reduced. No aluminum element is added to the formula of Comparative Example 3. It can be seen that if the Al element is not introduced, the oxygen content of the aluminothermic chromium powder is seriously exceeded and cannot be directly used as a raw material for the contact material.

[0123] The fourth group of embodiments:

[0124] Examples 10 and 11 show two typical contact material formulas. The product performance obtained after adding an appropriate equivalent of Al element is as follows: the conductivity of the contact material with a chromium content of 10% reaches 46Ms / m, i.e. 80% IACS. When the chromium content reaches 50%, the conductivity of the contact material can still reach 32Ms / m, which is much better than the 20-23Ms / m conductivity of CuCr50 material produced by traditional processes.

[0125] The fifth group of embodiments:

[0126] Based on the data in Example 1, Example 12 and Comparative Example 5, we can indeed see that the performance of Example 12 is better. This enhancement may be related to the synergistic effect of Al and Mg in CuCr alloys. Metal additives such as Al and Mg can promote grain refinement. Grain refinement is very beneficial for improving the strength and hardness of the alloy. Moreover, when Al and Mg exist at the same time, more uniform and finer grains may be formed in the alloy, thereby further improving the strength. In the alloy, Al and Mg act as solute atoms, and when they enter the lattice of Cu, a solid solution strengthening effect can be produced. The combined effect of the two may lead to a higher solid solution strengthening effect, thereby improving the strength and hardness of the alloy. During the internal oxidation process, Al and Mg form stable oxide dispersions, which can be strengthened as a second phase in the alloy. During the aging treatment process, these oxide dispersions may undergo some microstructural changes, thereby further improving the strength and hardness of the material.

[0127] The above is only a specific embodiment of the present invention, but the protection scope of the present invention is not limited thereto. Any changes or substitutions that are not conceived through creative work should be included in the protection scope of the present invention. Therefore, the protection scope of the present invention should be based on the protection scope defined in the claims.

Claims

1. A method for preparing a low-oxygen CuCr alloy contact material, It is characterized in that The steps include: (1) uniformly mixing CuAlMg alloy powder and Cr powder to obtain mixed powder; (2) cold spraying the mixed powder to obtain a blank; (3) subjecting the blank to internal oxidation and aging processes; In the step (1), the CuAlMg alloy powder has an Al content of 0.05-0.45wt%, a Mg content of 0.05-0.45wt%, and the balance is Cu.

2. The method for preparing the low-oxygen CuCr alloy contact material according to claim 1, It is characterized in that In the step (1), the oxygen content of the Cr powder is 200-5000 ppm; and the particle size of the Cr powder is in the range of 5-38 μm.

3. The method for preparing the low-oxygen CuCr alloy contact material according to claim 1, It is characterized in that The specific process of cold spraying in step (2) is as follows: the working gas is an inert gas, the spraying pressure is 6-9 MPa, the working gas heating temperature is 600-900° C., and the powder feeding efficiency is 200-400 g / min.

4. The method for preparing the low-oxygen CuCr alloy contact material according to claim 1, It is characterized in that In the step (3), the internal oxidation reaction is carried out at a temperature of 900-950° C. in an anaerobic environment for a holding time of 30-120 min.

5. The method for preparing the low-oxygen CuCr alloy contact material according to claim 4, It is characterized in that The internal oxidation reaction is carried out in a vacuum furnace with a vacuum degree higher than 8×10 -3 Pa.

6. The method for preparing the low-oxygen CuCr alloy contact material according to claim 5, It is characterized in that After the internal oxidation reaction is completed, the furnace temperature is lowered to 500-700°C and kept for 1-4 hours for aging process treatment, and then quickly cooled to room temperature.