A coating liquid for proton exchange membrane and its preparation method and application

By adding H+ compounds to the proton exchange membrane coating solution, the viscosity is reduced and the resin self-assembly is promoted, and the problems of long heat treatment time and poor filling performance in the prior art are solved, thereby achieving efficient preparation of proton exchange membranes and excellent protons Conductive performance.

CN117543039BActive Publication Date: 2024-11-05BEIJING QINGCHI TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202210924011.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-08-02
Publication Date
2024-11-05
Estimated Expiration
2042-08-02

AI Technical Summary

Technical Problem

The existing proton exchange membranes have a long time and low efficiency during the heat treatment process, which affects production efficiency. The high solid content perfluorosulfonic acid resin dispersion has poor filling performance in porous polytetrafluoroethylene film, resulting in poor film-forming proton conduction performance. good.

Method used

H+-containing compounds (such as protic acid) are mixed with perfluorosulfonic acid resin and solvent to form a low-viscosity coating liquid. H+ in the coating liquid promotes the self-assembly of the resin, and a smooth proton conduction channel can be constructed in a short period of heat treatment.

Benefits of technology

The viscosity of the coating liquid in the reinforcement layer is significantly reduced, the filling performance is improved, the heat treatment time is shortened, and the proton conductivity and conduction performance of the proton exchange membrane are improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117543039B_ABST
    Figure CN117543039B_ABST
Patent Text Reader

Abstract

The present invention discloses a coating liquid for proton exchange membrane and a preparation method and application thereof, wherein the coating liquid comprises a perfluorosulfonic acid resin and a solvent, and further comprises H introduced by a non-perfluorosulfonic acid resin. + In the present invention, a small amount of H is added to the coating liquid for proton exchange membrane. + , which can significantly reduce the viscosity of the coating liquid and improve the filling performance of the coating liquid in the porous polytetrafluoroethylene membrane. In addition, H + The addition of can promote the self-assembly of perfluorosulfonic acid resin in the solution. The self-assembled "clusters" only need a short period of heat treatment after membrane formation to construct a smooth proton conduction pathway, so that the proton exchange membrane has excellent proton conduction performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of proton exchange membrane fuel cells, and in particular to a coating liquid for a proton exchange membrane, a preparation method thereof, and an application in a proton exchange membrane. Background Art

[0002] Fuel cells are a clean energy technology that can alleviate energy and environmental problems. Proton exchange membrane fuel cells are an important type of fuel cell, in which the proton exchange membrane is its key component, which plays the role of transferring protons, blocking cathode and anode raw materials, and blocking electrons. Proton exchange membranes are homogeneous membranes and composite membranes. Homogeneous membranes are composed entirely of ion exchange resins, and composite membranes are composed of ion exchange resins and reinforcement layers. Homogeneous membranes have poor mechanical properties. Thinner homogeneous membranes cannot meet the requirements of fuel cells for their mechanical properties, and thicker homogeneous membranes cannot meet the requirements for increasing the volume power density of fuel cells. Based on the above reasons, homogeneous membranes are gradually eliminated. Because they contain reinforcement layers, thinner composite proton exchange membranes (8-15μm) can meet the requirements of fuel cells for the mechanical properties of proton exchange membranes, and can meet the requirements of fuel cells for increasing power density, and are widely used in the field of fuel cells.

[0003] The composite proton exchange membrane includes a resin layer and a reinforcement layer. The reinforcement layer is a porous film. The resin is fully filled in the porous film. The resin layer wraps the reinforcement layer on both sides of the reinforcement layer. The preparation process of the composite proton exchange membrane is generally as follows: a layer of coating liquid is applied on the substrate to form a liquid film, a porous reinforcement layer is composited on the liquid film, and then a layer of coating liquid is applied on the porous reinforcement layer to form a liquid film; the coating liquid infiltrates into the reinforcement layer, and after drying, a continuous phase is formed in the reinforcement layer, and the coating liquid on both sides of the reinforcement layer forms a continuous phase (homogeneous membrane). The reinforcement layer is generally a porous polytetrafluoroethylene film, which is a porous membrane formed by stretching a polytetrafluoroethylene membrane.

[0004] The proton conductivity of the proton exchange membrane is one of its important properties. The higher the proton conductivity, the stronger its proton conduction performance, and the better the electrical performance after being assembled into a battery. At present, the proton exchange membrane is often heat-treated to rearrange its molecules and build a smooth proton transmission channel. Conventional proton exchange membrane heat treatment has high temperature and long time, which seriously affects the production efficiency of the proton exchange membrane. Summary of the invention

[0005] In order to improve the above technical problems, the present invention provides a coating liquid for proton exchange membrane and its preparation method and application. The coating liquid for proton exchange membrane of the present invention is used, and the coating liquid is coated on a reinforcing layer (such as a porous polytetrafluoroethylene membrane). Since the contact angle between the coating liquid and the reinforcing layer is small and the coating liquid has a low viscosity, it is beneficial for the coating liquid to flow in the pores of the reinforcing layer, fully fill the pores of the reinforcing layer, and form a continuous perfluorosulfonic acid resin phase in the pores of the reinforcing layer. The continuous perfluorosulfonic acid resin phase provides a channel for proton conduction. In addition, the proton exchange membrane prepared by the coating liquid of the present invention can make the arrangement of the resin molecules in the proton exchange membrane form a smooth proton transmission channel after a short period of heat treatment.

[0006] The technical solution of the present invention is as follows:

[0007] A coating liquid for a proton exchange membrane, the coating liquid comprising a perfluorosulfonic acid resin and a solvent, the coating liquid further comprising H introduced by a non-perfluorosulfonic acid resin + .

[0008] According to the present invention, the H + H + In the form of a compound, for example, + The compound is selected from protonic acid; specifically, the protonic acid can be selected from at least one of formic acid, acetic acid, citric acid, nitric acid, hydrochloric acid, sulfuric acid, phosphoric acid, benzoic acid, malic acid, etc.

[0009] According to the present invention, the H-containing + The compound is introduced in the form of a solution, the concentration of the solution is 0.1-2 mol / L, preferably 0.5-1 mol / L, for example 0.5 mol / L, 0.6 mol / L, 0.7 mol / L, 0.8 mol / L, 0.9 mol / L or 1 mol / L. Specifically, the solvent in the solution can be at least one of methanol, ethanol, ethylene glycol, acetone, isopropanol, n-propanol, water, N,N-dimethylformamide, N,N-dimethylacetamide, dimethyl sulfoxide, etc.

[0010] According to the present invention, the perfluorosulfonic acid resin may be a perfluorosulfonic acid resin dispersion, and its solid content may be 5-30wt%, exemplarily 5wt%, 10wt%, 15wt%, 20wt%, 25wt%, 30wt%.

[0011] According to the present invention, the dispersant in the perfluorosulfonic acid resin dispersion can be at least one of ethanol, ethylene glycol, acetone, isopropanol, n-propanol, water, N,N-dimethylformamide, N,N-dimethylacetamide, dimethyl sulfoxide, etc.

[0012] According to the present invention, in the coating solution, the perfluorosulfonic acid resin dispersion and the H-containing+ The mass ratio of the compound solution is (1-12):1, preferably (5-10):1.

[0013] According to the present invention, the solvent in the coating solution for proton exchange membrane is an alcohol solvent, a ketone solvent, an amide solvent, a sulfoxide solvent, water or a mixed solvent thereof. Specifically, the solvent can be at least one of methanol, ethanol, ethylene glycol, isopropanol, n-propanol, water, acetone, N,N-dimethylformamide, N,N-dimethylacetamide, dimethyl sulfoxide, etc.

[0014] According to the present invention, the viscosity of the coating liquid at 25° C. is 30-100 mPas, preferably 30-50 mPas.

[0015] The present invention also provides a method for preparing the above-mentioned coating liquid for proton exchange membrane, the method comprising: + The compound, perfluorosulfonic acid resin and solvent are mixed to obtain the coating liquid for proton exchange membrane.

[0016] According to the present invention, the H-containing + The compound is introduced in the form of a solution, i.e. + The compound is dissolved in a solvent to obtain a compound containing H + A solution of a compound.

[0017] Specifically, the H-containing + The concentration of the solution of the compound is 0.1-2 mol / L, preferably 0.5-1 mol / L, for example, 0.5 mol / L, 0.6 mol / L, 0.7 mol / L, 0.8 mol / L, 0.9 mol / L or 1 mol / L.

[0018] Specifically, dissolving the H + The solvent of the compound may be an alcohol solvent, a ketone solvent, an amide solvent, a sulfoxide solvent, water or a mixed solvent thereof. Specifically, the solvent may be at least one of methanol, ethanol, ethylene glycol, acetone, isopropanol, n-propanol, water, N,N-dimethylformamide, N,N-dimethylacetamide, dimethyl sulfoxide, and the like.

[0019] According to the present invention, the perfluorosulfonic acid resin is introduced in the form of a perfluorosulfonic acid resin dispersion.

[0020] According to the present invention, the solid content of the perfluorosulfonic acid resin dispersion is 5-30wt%, exemplarily 5wt%, 10wt%, 15wt%, 20wt%, 25wt%, 30wt%. The perfluorosulfonic acid resin dispersion is, for example, Nafion D2020CS.

[0021] According to the present invention, the method specifically comprises: mixing a perfluorosulfonic acid resin dispersion, a H-containing + The solution of the compound is mixed with a solvent to obtain the coating solution for the proton exchange membrane.

[0022] According to the present invention, the perfluorosulfonic acid resin dispersion and the H-containing + The mass ratio of the solution of the compound is (1-12):1, preferably (5-10):1.

[0023] According to the present invention, the solvent is an alcohol solvent, a ketone solvent, an amide solvent, a sulfoxide solvent, water or a mixed solvent thereof. Specifically, the solvent can be at least one of methanol, ethanol, ethylene glycol, acetone, isopropanol, n-propanol, water, N,N-dimethylformamide, N,N-dimethylacetamide, dimethyl sulfoxide, etc.

[0024] The present invention also provides a proton exchange membrane, which comprises a coating layer prepared by the coating liquid for proton exchange membrane.

[0025] According to the present invention, the proton exchange membrane comprises the above-mentioned coating layer and reinforcement layer in sequence.

[0026] According to the present invention, the reinforcement layer further includes the coating layer mentioned above, that is, the proton exchange membrane includes the coating layer, the reinforcement layer and the coating layer mentioned above in sequence.

[0027] According to the present invention, the reinforcement layer is a polytetrafluoroethylene membrane; preferably a porous polytetrafluoroethylene membrane.

[0028] The present invention also provides a method for preparing the above-mentioned proton exchange membrane, the method comprising the following steps:

[0029] (1) coating a layer of the proton exchange membrane coating liquid on a base membrane to form a first liquid film; and drying the liquid film to obtain the proton exchange membrane.

[0030] According to the present invention, the method specifically comprises the following steps:

[0031] (1a) coating a layer of the proton exchange membrane coating liquid on a base membrane to form a first liquid membrane;

[0032] (2) spreading the reinforcement layer on the first liquid film;

[0033] (3) Drying to obtain the proton exchange membrane.

[0034] According to the present invention, the method specifically comprises the following steps:

[0035] (1a) coating a layer of the proton exchange membrane coating liquid on a base membrane to form a first liquid membrane;

[0036] (2) spreading the reinforcement layer on the first liquid film;

[0037] (3a) coating another layer of the proton exchange membrane coating liquid on the reinforcement layer to form a second liquid membrane;

[0038] (4) Drying the wet membrane prepared in step (3a) to obtain the proton exchange membrane.

[0039] According to the present invention, the drying process in step (4) is: first drying at 60-110° C. for 5-60 min; then annealing at 120-180° C. for 1-60 min, preferably, the annealing time is 1-10 min.

[0040] According to the present invention, the reinforcement layer is a polytetrafluoroethylene membrane, preferably a porous polytetrafluoroethylene membrane.

[0041] Beneficial Effects of the Invention

[0042] In the production process of proton exchange membranes, in order to ensure a high coating speed and coating quality, a perfluorosulfonic acid resin dispersion with a high solid content is usually selected. The viscosity of the perfluorosulfonic acid resin dispersion with a high solid content is high. When producing a proton exchange membrane containing a reinforcement layer, the perfluorosulfonic acid resin dispersion is not easy to infiltrate into the pores of the porous polytetrafluoroethylene membrane, resulting in poor proton conductivity of the membrane.

[0043] In the conventional proton exchange membrane production process, the proton exchange membrane needs to be heat treated for a long time to achieve ideal performance. Under the condition that the length of the heat treatment section of the production line is certain, the longer the heat treatment time required, the lower the production efficiency.

[0044] The coating liquid for proton exchange membrane provided by the present invention comprises a small amount of H + The compound can significantly reduce the viscosity of the coating liquid and improve the filling performance of the coating liquid in the porous polytetrafluoroethylene membrane (i.e., the reinforcement layer). + The addition of can promote the self-assembly of perfluorosulfonic acid resin in the solution. The self-assembled "clusters" only need a short time (1-20 minutes) of heat treatment after membrane formation to construct a smooth proton conduction pathway, so that the proton exchange membrane has excellent proton conduction performance. BRIEF DESCRIPTION OF THE DRAWINGS

[0045] Figure 1 This is a cross-sectional SEM image of the proton exchange membrane prepared in Example 5.

[0046] Figure 2 This is a cross-sectional SEM image of the proton exchange membrane prepared in Comparative Example 2. DETAILED DESCRIPTION

[0047] The technical scheme of the present invention will be further described in detail below in conjunction with specific embodiments. It should be understood that the following embodiments are only exemplary descriptions and explanations of the present invention and should not be construed as limiting the scope of protection of the present invention. All technologies implemented based on the above content of the present invention are included in the scope that the present invention is intended to protect.

[0048] Unless otherwise specified, the raw materials and reagents used in the following examples are commercially available or can be prepared by known methods.

[0049] Nafion D2020CS resin dispersion is a perfluorosulfonic acid resin dispersion purchased from Chemours, with a solid content of 20wt%-22wt%, a n-propanol content of 42wt%-46wt%, a water content of 32wt%-36wt%, and an ethanol content of 0.5wt%.

[0050] Comparative Example 1

[0051] 180 g of Nafion D2020CS resin dispersion with a solid content of 20 wt% was weighed, and 20 g of isopropanol was added thereto; mechanical stirring was performed for 30 min, and ultrasonic treatment was performed for 30 min to obtain a coating liquid for coating a proton exchange membrane with a solid content of 18 wt%. The viscosity of the coating liquid at 25° C. was tested with a viscometer, and the results are shown in Table 1.

[0052] Example 1

[0053] Weigh 180 g of Nafion D2020CS resin dispersion with a solid content of 20 wt%, add 20 g of isopropanol solution with a benzoic acid concentration of 1.0 mol / L, stir mechanically for 30 min, and ultrasonically treat for 30 min to obtain a coating solution for coating a proton exchange membrane with a solid content of 18 wt%. The viscosity of the coating solution at 25°C was tested with a viscometer, and the results are shown in Table 1.

[0054] Example 2

[0055] 180 g of Nafion D2020CS resin dispersion with a solid content of 20 wt% was weighed, and 20 g of isopropanol solution with a malic acid concentration of 0.5 mol / L was added thereto; mechanical stirring was performed for 30 min, and ultrasonic treatment was performed for 30 min to obtain a coating solution for coating a proton exchange membrane with a solid content of 18 wt%. The viscosity of the coating solution at 25° C. was tested with a viscometer, and the results are shown in Table 1.

[0056] Example 3

[0057] Weigh 180 g of Nafion D2020CS resin dispersion with a solid content of 20 wt%, add 24 g of isopropanol solution with a hydrochloric acid concentration of 1.0 mol / L, stir mechanically for 30 min, and ultrasonically treat for 30 min to obtain a coating solution for coating a proton exchange membrane with a solid content of 15 wt%. The viscosity of the coating solution at 25°C is tested with a viscometer, and the results are shown in Table 1.

[0058] Example 4

[0059] Weigh 180 g of Nafion D2020CS resin dispersion with a solid content of 20 wt%, add 24 g of isopropanol solution with a sulfuric acid concentration of 0.5 mol / L, stir mechanically for 30 min, and ultrasonically treat for 30 min to obtain a coating solution for coating a proton exchange membrane with a solid content of 15 wt%. The viscosity of the coating solution at 25°C is tested with a viscometer, and the results are shown in Table 1.

[0060] Comparative Example 2

[0061] The coating liquid described in Comparative Example 1 was applied on a base film (polyimide film) to form a 60 μm liquid film; a 8 μm thick porous polytetrafluoroethylene film was composited thereon; the coating liquid described in Comparative Example 1 was then applied on the porous polytetrafluoroethylene film to form a 60 μm thick liquid film; the formed wet film was sent to a forced air drying oven and dried at 90° C. for 10 min to obtain a dry film; the dry film was sent to a forced air drying oven and heat treated at 140° C. for 10 min to obtain a finished mass exchange membrane.

[0062] Example 5

[0063] The film-making process is the same as that of Comparative Example 2, except that the coating liquid used is the coating liquid prepared in Example 1, and the thickness of the single-layer liquid film is 60 μm.

[0064] Example 6

[0065] The film-making process is the same as that of Comparative Example 2, except that the coating liquid used is the coating liquid prepared in Example 2, and the thickness of the single-layer liquid film is 60 μm.

[0066] Example 7

[0067] The film-making process is the same as that of Comparative Example 2, except that the coating liquid used is the coating liquid prepared in Example 3; the thickness of the single-layer liquid film is 72 μm.

[0068] Example 8

[0069] The film-making process is the same as that of Comparative Example 2, except that the coating liquid used is the coating liquid prepared in Example 4; the thickness of the single-layer liquid film is 72 μm.

[0070] Test Case

[0071] The viscosity of the coating liquids in Comparative Example 1 and Examples 1-4 was tested, and the test results are shown in Table 1 below.

[0072] Table 1 Viscosity of coating solutions prepared in Comparative Example 1 and Examples 1-4

[0073] Coating liquid Viscosity at 25℃(mPas) Comparative Example 1 55.2 Example 1 41.1 Example 2 39.2 Example 3 35.2 Example 4 35.9

[0074] As shown in Table 1, under the same solid content condition, the viscosity of the coating liquid prepared in Examples 1-4 is significantly lower than that of the coating liquid prepared in Comparative Example 1. + The addition of promotes the self-assembly of perfluorosulfonic acid resin, separates the hydrophilic phase and non-hydrophilic phase of perfluorosulfonic acid molecules, reduces the interaction between molecular chains, and significantly reduces the viscosity of the coating liquid.

[0075] The proton exchange membranes prepared in Examples 5-8 and Comparative Example 2 of 10 cm×10 cm were taken respectively, placed in 500 mL of deionized water, and washed in a water bath at 80° C. for 48 h, during which the water was changed every 12 h; the proton exchange membranes were then placed in 500 mL of 1 mol / L sulfuric acid solution, and placed in a water bath at 80° C. for 48 h, during which the sulfuric acid solution was changed every 12 h to ensure that impurity ions were removed; the proton exchange membranes were placed in a 100° C. oven for drying for 12 h, and placed in a constant temperature and humidity chamber at 25° C. and 50% RH, and then taken out for proton conductivity detection.

[0076] Proton conductivity was detected using a four-electrode method at 85°C, 50% RH, a disturbance voltage of 100 mV, and a frequency of 1-10 5 Hz, the size of the proton exchange membrane used for detection is 1 cm×4.5 cm, and the proton conductivity data of the obtained proton exchange membrane are shown in Table 2.

[0077] Table 2 Proton conductivity of proton exchange membranes prepared in Comparative Example 2 and Examples 5-8

[0078] Proton Exchange Membrane Proton conductivity at 85℃50%RH mS / cm Comparative Example 2 20.1 Example 5 31.5 Example 6 32.3 Example 7 30.3 Example 8 34.6

[0079] As can be seen from Table 2, the coating solution of the present invention contains H + The addition of H-containing compounds promoted the self-assembly behavior of perfluorosulfonic acid molecules. During the film formation process, the perfluorosulfonic acid molecules were arranged regularly, constructing a high-quality proton transmission channel. After film formation, its proton conductivity was much better than that without adding H-containing compounds. + For example, the proton conductivity of the proton exchange membranes of Examples 5 and 6 is about 1.5 times that of Comparative Example 2. And for coating solutions with different solid contents, the content of H + The addition of compounds can play a role in improving the proton conductivity of the proton exchange membrane.

[0080] Figure 1This is a cross-sectional SEM image of the proton exchange membrane prepared in Example 5.

[0081] Figure 2 This is a cross-sectional SEM image of the proton exchange membrane prepared in Comparative Example 2.

[0082] like Figure 1 He Ru Figure 2 As described above, the reduction in the viscosity of the coating liquid makes it easier for the coating liquid to penetrate into the reinforcing layer, so that the perfluorosulfonic acid resin is filled more densely in the porous polytetrafluoroethylene (such as Figure 1 shown); without adding H + The proton exchange membrane prepared by the coating solution of the compound (Comparative Example 2) is not fully filled with the porous polytetrafluoroethylene membrane. Figure 2 shown.

[0083] The above is an exemplary description of the embodiments of the present invention. However, the protection scope of the present invention is not limited to the above embodiments. Any modification, equivalent substitution, improvement, etc. made by those skilled in the art within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A coating liquid for a proton exchange membrane, characterized in that: The coating solution includes a perfluorosulfonic acid resin and a solvent, and the coating solution also includes H + ; The H + H + The compound containing H + The compound is selected from at least one of formic acid, acetic acid, citric acid, nitric acid, hydrochloric acid, sulfuric acid, phosphoric acid, benzoic acid and malic acid; The H-containing + The compound is introduced in the form of a solution, the concentration of the solution is 0.1-2 mol / L; The perfluorosulfonic acid resin is a perfluorosulfonic acid resin dispersion, and its solid content is 5-30wt%; In the coating solution, the perfluorosulfonic acid resin dispersion and the H-containing + The mass ratio of the compound solution is (1~12):1; The coating liquid has a viscosity of 30-100 mPas at 25°C.

2. The coating liquid for proton exchange membrane according to claim 1, characterized in that: Dissolve the H + The solvent of the compound is selected from alcohol solvents, ketone solvents, amide solvents, sulfoxide solvents, water or mixed solvents thereof.

3. The coating liquid for proton exchange membrane according to claim 2, characterized in that: The solvent is at least one of methanol, ethanol, ethylene glycol, acetone, isopropanol, n-propanol, water, N,N-dimethylformamide, N,N-dimethylacetamide and dimethyl sulfoxide.

4. The coating liquid for proton exchange membrane according to claim 1, characterized in that: The solvent in the coating liquid for proton exchange membrane is an alcohol solvent, a ketone solvent, an amide solvent, a sulfoxide solvent, water or a mixed solvent thereof.

5. The coating liquid for proton exchange membrane according to claim 4, characterized in that: The solvent in the coating liquid for proton exchange membrane is at least one of methanol, ethanol, ethylene glycol, acetone, isopropanol, n-propanol, water, N,N-dimethylformamide, N,N-dimethylacetamide and dimethyl sulfoxide.

6. A proton exchange membrane, characterized in that: The proton exchange membrane comprises a coating layer prepared by the coating solution for proton exchange membrane according to any one of claims 1 to 5.

7. The proton exchange membrane according to claim 6, characterized in that The proton exchange membrane comprises the above-mentioned coating layer and reinforcement layer in sequence.

8. The proton exchange membrane according to claim 7, characterized in that: The reinforcing layer further comprises the above-mentioned coating layer outside the reinforcing layer, that is, the proton exchange membrane comprises the above-mentioned coating layer, the reinforcing layer and the above-mentioned coating layer in sequence.

9. The method for preparing a proton exchange membrane according to any one of claims 6 to 8, characterized in that: The method comprises: (1) coating a layer of the coating liquid for proton exchange membrane according to any one of claims 1 to 5 on a base membrane to form a first liquid film; and drying to obtain the proton exchange membrane.

10. The preparation method according to claim 9, characterized in that: The method specifically comprises the following steps: (1a) coating a layer of the coating liquid for proton exchange membrane according to any one of claims 1 to 5 on a base membrane to form a first liquid membrane; (2) spreading the reinforcement layer on the first liquid film; (3) Drying to obtain the proton exchange membrane.

11. The preparation method according to claim 9, characterized in that: The method specifically comprises the following steps: (1a) coating a layer of the coating liquid for proton exchange membrane according to any one of claims 1 to 5 on a base membrane to form a first liquid membrane; (2) spreading the reinforcement layer on the first liquid film; (3a) coating a layer of the coating liquid for proton exchange membrane according to any one of claims 1 to 5 on the reinforcement layer to form a second liquid membrane; (4) Drying the wet membrane prepared in step (3a) to obtain the proton exchange membrane.