A Nb2O5 photocatalyst rich in oxygen vacancies and its preparation method and application

By calcining Nb2O5 photocatalysts rich in oxygen vacancies under a protective gas atmosphere, the problems of low catalytic activity and complexity of oxygen defect construction in the existing technology are solved, the effect of efficient photocatalytic reduction of CO2 is achieved, the preparation process is simplified and the cost is reduced cost.

CN117563583BActive Publication Date: 2024-10-18NANYANG NORMAL UNIV
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202310242194.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-03-14
Publication Date
2024-10-18
Estimated Expiration
2043-03-14

AI Technical Summary

Technical Problem

The existing Nb2O5 photocatalyst has low catalytic activity and poor product selectivity in the process of converting CO2 into CH4. The oxygen defect construction method has strict equipment requirements, high cost and poor performance.

Method used

A Nb2O5 photocatalyst rich in oxygen vacancies was constructed using a calcination method under a protective gas atmosphere. Niobium pentoxide powder was prepared by a hydrothermal method and calcined at 400-600°C to simplify the oxygen vacancy construction process and improve catalytic performance.

Benefits of technology

It achieves efficient photocatalytic reduction of CO2, improves the visible light utilization rate and product selectivity of the catalyst, simplifies the preparation process, reduces equipment requirements and costs, and has no harmful by-products.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117563583B_ABST
    Figure CN117563583B_ABST
Patent Text Reader

Abstract

The present invention belongs to the technical field of photocatalytic materials, and discloses a Nb2O5 photocatalyst rich in oxygen vacancies, a preparation method and an application thereof. The preparation method comprises the following steps: using a soluble niobium salt as a precursor, adding water and adopting a hydrothermal method to prepare a hydrated niobium pentoxide powder; placing the niobium pentoxide powder under a protective gas and calcining at 400-600°C to obtain a Nb2O5 photocatalyst rich in oxygen vacancies. The present invention calcines amorphous niobium pentoxide rich in oxygen vacancies under a protective gas atmosphere, which has good economic and environmental protection effects on the application of semiconductor materials in the fields of photocatalytic CO2 reduction, and the relative concentration of oxygen vacancies in the prepared niobium pentoxide is significantly increased, which significantly improves the performance of photocatalytic reduction of CO2.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of photocatalytic materials, and in particular relates to a Nb2O5 photocatalyst rich in oxygen vacancies and a preparation method and application thereof. Background Art

[0002] Energy shortage and environmental pollution are urgent problems affecting public health that need to be solved today. Photocatalytic reduction of CO2 to produce CH4 and other hydrocarbons is a promising strategy to solve the problems of global warming and energy crisis. In the CO2 conversion process, catalysts play an important role in controlling the reaction pathway and product selectivity.

[0003] Niobium pentoxide (Nb2O5), a metal oxide, is a common semiconductor material with the advantages of safety, non-toxicity, and good chemical stability. It is widely used in many fields including photocatalysis, gas sensors, traditional acid catalysis, electrochromism, field emission displays, and microelectronics. In the field of photocatalysis, the application of Nb2O5 is currently mainly concentrated in environmental remediation, such as photocatalytic degradation of organic pollutants. There are few reports on the use of Nb2O5 to photocatalytically reduce CO2 to prepare CH4 and other hydrocarbon fuels, with low photocatalytic activity and poor product selectivity. On the one hand, this is determined by its energy band structure: the band gap is wide (Eg~3.4eV), it can only adsorb and utilize visible light, the conduction band position is low, and the photogenerated electron reduction ability is poor; on the other hand, due to the lack of sufficient active sites, it is difficult to adsorb and activate reactive molecules such as CO2 and H2O. In addition, there are also problems such as high recombination rate of photogenerated electrons-holes.

[0004] Introducing defects in semiconductors can not only improve the utilization rate of visible light and promote the separation of photogenerated electrons and holes, but also become active sites for photocatalytic reactions. Introducing oxygen vacancies in oxide semiconductors has been shown to be an effective means to improve photocatalytic activity and regulate product selectivity. However, the current methods for constructing oxygen defects often involve high-temperature treatment in a reducing gas atmosphere such as hydrogen or hydrothermal treatment using a strongly reducing organic-metal reducing agent. These methods have strict requirements on equipment, high preparation costs, and poor catalytic performance. It is of great significance to develop a safe and simple preparation method for Nb2O5 rich in oxygen vacancies to obtain efficient photocatalytic reduction of CO2 to selectively prepare non-toxic CH4 clean fuel. Summary of the invention

[0005] The purpose of the present invention is to provide a Nb2O5 photocatalyst rich in oxygen vacancies and its preparation method and application, in view of the problems of existing oxygen defect construction methods having high equipment requirements and preparation costs and poor catalytic performance, to improve the complex and strict experimental conditions of the current oxygen vacancy construction process and to improve the catalytic performance of its photocatalyst, and to construct Nb2O5 rich in oxygen vacancies by calcination under a protective gas atmosphere for use in the field of photocatalysis.

[0006] In order to achieve the above purpose, the technical solution adopted in this application is:

[0007] A method for preparing a Nb2O5 photocatalyst rich in oxygen vacancies comprises the following steps: using a soluble niobium salt as a precursor, adding water and preparing hydrated niobium pentoxide powder by a hydrothermal method; placing the niobium pentoxide powder under protective gas and calcining it at 400-600°C to obtain a Nb2O5 photocatalyst rich in oxygen vacancies.

[0008] Preferably, the soluble niobium salt is niobium pentachloride or niobium oxalate.

[0009] Preferably, the molar volume ratio of the soluble niobium salt to water is 0.5-2 mmol:30 mL.

[0010] Preferably, the temperature of the hydrothermal reaction is 140-180° C. and the time is 24 hours.

[0011] Preferably, the protective gas is an inert gas or nitrogen.

[0012] Preferably, the calcination heating rate is 1-10°C / min.

[0013] Preferably, the calcination time is 1 to 3 hours.

[0014] In addition, the present invention also provides a Nb2O5 photocatalyst rich in oxygen vacancies prepared by the above preparation method.

[0015] The present invention also provides the use of the above-mentioned Nb2O5 photocatalyst rich in oxygen vacancies in photocatalysis, and the Nb2O5 photocatalyst selectively reduces CO2.

[0016] Compared with the prior art, the present invention has the following beneficial effects:

[0017] (1) The present invention provides a relatively simple, easy-to-operate and effective method for constructing oxygen defects in niobium pentoxide semiconductors. The obtained Nb2O5 photocatalyst has an amorphous structure, a mesoporous morphology of nanoparticle stacking, abundant oxygen vacancies and a wider light absorption range. The presence of oxygen vacancies can not only improve the visible light utilization rate of the catalyst and promote the separation of photogenerated electrons and holes, but also become active sites for photocatalytic reactions, which greatly simplifies the process of constructing oxygen vacancies in semiconductors and greatly improves production efficiency. It also has good economic and environmental benefits and improves the activity of photocatalytic reduction of CO2.

[0018] (2) The photocatalyst prepared by the present invention has a simple preparation process, short time consumption, easy operation, no need for strict equipment, no harmful or toxic by-products, and is environmentally friendly; no high pressure is required during calcination, no reducing gases such as hydrogen or high-cost strong reducing agents are used, the raw materials are abundant and easy to obtain, and the experimental conditions are relatively safe.

[0019] (3) The present invention is the first to obtain oxygen vacancy-rich niobium pentoxide by calcination under a protective gas atmosphere, which has good economic and environmental protection effects on the application of semiconductor materials in the fields of photocatalytic CO2, and the relative concentration of oxygen vacancies in the prepared niobium pentoxide is significantly increased, which significantly improves the performance of photocatalytic reduction of CO2. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] Figure 1 The X-ray diffraction pattern of the Nb2O5 catalyst containing oxygen vacancies constructed for the present invention;

[0021] Figure 2 Transmission electron microscopy image of the Nb2O5 catalyst containing oxygen vacancies constructed by the present invention;

[0022] Figure 3 X-ray photoelectron spectrum of Nb2O5 catalyst containing oxygen vacancies constructed for the present invention;

[0023] Figure 4 X-ray photoelectron spectrum of Nb2O5 catalyst Nb3d containing oxygen vacancies constructed for the present invention;

[0024] Figure 5 The X-ray photoelectron spectrum of the Nb2O5 catalyst O1s containing oxygen vacancies is constructed for the present invention;

[0025] Figure 6 An electron sequential resonance spectrum for comparing the relative concentrations of oxygen vacancies in a Nb2O5 catalyst containing oxygen vacancies constructed for the present invention;

[0026] Figure 7 Raman spectra of Nb2O5 catalysts containing oxygen vacancies constructed for the present invention;

[0027] Figure 8 The UV-visible absorption spectrum of the Nb2O5 catalyst containing oxygen vacancies is constructed for the present invention;

[0028] Fig. 9 A graph showing the relationship between the amount of material produced by photocatalytic reduction of CO2 to produce CH4 over time using a Nb2O5 catalyst containing oxygen vacancies constructed for the present invention;

[0029] Fig.10 A graph showing the relationship between the amount of CO produced by photocatalytic reduction of CO2 by a Nb2O5 catalyst containing oxygen vacancies and the time of the photocatalytic reduction of CO2 by the present invention;

[0030] Fig.11 A selectivity data graph for the photocatalytic reduction of Nb2O5 catalysts containing oxygen vacancies to produce CH4 is constructed for the present invention. DETAILED DESCRIPTION

[0031] The following will combine the data in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0032] It should be noted that the professional terms used in the present invention are only for the purpose of describing specific embodiments and are not intended to limit the scope of protection of the present invention. Unless otherwise specifically stated, the various raw materials, reagents, instruments and equipment used in the following embodiments of the present invention can be purchased from the market or prepared by existing methods.

[0033] Example 1

[0034] A method for preparing a Nb2O5 photocatalyst rich in oxygen vacancies comprises the following steps:

[0035] S1. Weigh 1 mmol of niobium pentachloride (NbCl5), dissolve it in 30 mL of deionized water, stir and ultrasonicate for 15 min to obtain a white uniform liquid; then put the white liquid into a 50 mL high-pressure reactor, put it into an oven, heat it to 160°C and perform hydrothermal reaction for 24 h. After the hydrothermal reaction cools to room temperature, wash it with water and alcohol several times, dry it at 80°C overnight, and grind it to obtain hydrated niobium pentoxide (Nb2O5) powder;

[0036] S2. Place Nb2O5 powder in a porcelain boat, then put it into a tubular furnace, heat it to 400°C at a rate of 5°C / min in an argon atmosphere, and calcine it for 2 hours. After cooling to room temperature, grind it for later use to obtain a Nb2O5 photocatalyst rich in oxygen vacancies. The sample prepared by high-temperature calcination is named NBO-Ar-400.

[0037] Example 2

[0038] A method for preparing a Nb2O5 photocatalyst rich in oxygen vacancies comprises the following steps:

[0039] S1. Weigh 1mmol NbCl5, dissolve it in 30mL deionized water, stir and ultrasonic for 15min to obtain a white uniform liquid; then put the white liquid into a 50mL high-pressure reactor, put it into an oven, heat it to 160℃ and perform hydrothermal reaction for 24h. After the hydrothermal reaction cools to room temperature, wash it with water and alcohol several times, dry it at 80℃ overnight, and grind it to obtain hydrated niobium pentoxide (Nb2O5) powder;

[0040] S2. Place Nb2O5 powder in a porcelain boat, then put it into a tubular furnace, heat it to 600℃ at a rate of 5℃ / min in an argon atmosphere, and calcine it for 2h. After cooling to room temperature, grind it for later use to obtain a Nb2O5 photocatalyst rich in oxygen vacancies. The sample prepared by high-temperature calcination is named NBO-Ar-600.

[0041] Example 3

[0042] A method for preparing a Nb2O5 photocatalyst rich in oxygen vacancies comprises the following steps:

[0043] S1. Weigh 2mmol NbCl5, dissolve it in 30mL deionized water, stir ultrasonically for 15min to obtain a white uniform liquid; then put the white liquid into a 50mL high-pressure reactor, put it into an oven, heat it to 180℃ and perform hydrothermal reaction for 24h. After the hydrothermal reaction cools to room temperature, wash it with water and alcohol several times, dry it at 80℃ overnight, and grind it to obtain hydrated niobium pentoxide (Nb2O5) powder;

[0044] S2. Place Nb2O5 powder in a porcelain boat, then put it into a tubular furnace, heat it to 500°C at a rate of 4°C / min in an argon atmosphere, calcine it for 2 hours, cool it to room temperature, and grind it for later use to obtain a Nb2O5 photocatalyst rich in oxygen vacancies.

[0045] Comparative Example 1

[0046] A method for preparing a Nb2O5 photocatalyst comprises the following steps:

[0047] S1. Weigh 1mmol NbCl5, dissolve it in 30mL deionized water, stir and ultrasonic for 15min to obtain a white uniform liquid; then put the white liquid into a 50mL high-pressure reactor, put it into an oven, heat it to 160℃ and perform hydrothermal reaction for 24h. After the hydrothermal reaction cools to room temperature, wash it with water and alcohol several times, dry it at 80℃ overnight, and grind it to obtain hydrated niobium pentoxide (Nb2O5) powder;

[0048] S2. Place Nb2O5 powder in a porcelain boat, then put it into a tubular furnace, heat it to 400℃ at a rate of 5℃ / min in an air atmosphere, and calcine it for 2h. After cooling to room temperature, grind it for later use to obtain a Nb2O5 photocatalyst rich in oxygen vacancies. The sample prepared by high-temperature calcination is named NBO-Air-400.

[0049] Comparative Example 2

[0050] A method for preparing a Nb2O5 photocatalyst comprises the following steps:

[0051] Weigh 1mmolNbCl5, dissolve it in 30mL deionized water, stir and ultrasonicate for 15min to obtain a white uniform liquid; then put the white liquid into a 50mL high-pressure reactor, put it into an oven, heat it to 160℃ and perform hydrothermal reaction for 24h. After the hydrothermal reaction cools to room temperature, wash it with water and alcohol several times, dry it at 80℃ overnight, and grind it to obtain a hydrated Nb2O5 catalyst, named NBO.

[0052] Figure 1 The X-ray diffraction pattern (XRD) of the Nb2O5 catalyst containing oxygen vacancies is constructed for the present invention. Figure 1 As shown, the untreated Nb2O5 (Comparative Example 2) is amorphous and can be explained as hydrated niobium pentoxide. After calcination at 400°C, it is still amorphous as in Example 1. The inherent disordered structure and thermodynamic metastable state of amorphous materials give them unique electrical and optical properties, which can effectively enhance the light absorption of the material and promote the separation of carriers, which is of great significance for improving the photocatalytic activity of the material.

[0053] Figure 2 The transmission electron microscope (TEM) image of the Nb2O5 catalyst containing oxygen vacancies constructed by the present invention is shown in FIG. Figure 2 As shown, Example 1 NBO-Ar-400, Comparative Example 1 NBO-Air-400 and Comparative Example NBO all present a mesoporous morphology of nanoparticle accumulation. The hydrolysis of niobium pentachloride produces a strongly acidic environment, which has a strong inhibitory effect on the re-nucleation and growth of Nb2O5 during the hydrothermal process, so as to obtain the following Figure 2 The mesoporous morphology of the nanoparticles shown in the figure can remain basically unchanged at a high temperature of 400°C. This mesoporous morphology can provide abundant adsorption sites for CO2, which is beneficial to improving the photocatalytic activity of the catalyst. When the temperature rises to 600°C, the particles of Example 2 NBO-Ar-600 are significantly enlarged, and the mesoporous structure basically disappears, which is not conducive to the adsorption of CO2 and the improvement of photocatalytic activity.

[0054] Figure 3 The X-ray photoelectron spectrum of the Nb2O5 catalyst containing oxygen vacancies is constructed for the present invention. Figure 3As shown, the NBO-Ar-400 catalyst sample of Example 1 contains Nb and O, but no other elements.

[0055] Figure 4 The X-ray photoelectron spectrum of the Nb2O5 catalyst Nb3d containing oxygen vacancies is constructed for the present invention. Figure 4 As shown, the NBO-Ar-400 catalyst sample of Example 1 has Nb 4+ , while in the comparative example 2NBO, there is no Nb 4+ The existence of is due to oxygen vacancies.

[0056] Figure 5 The X-ray photoelectron spectrum of the Nb2O5 catalyst O1s containing oxygen vacancies is constructed for the present invention. Figure 5 As shown, in Example 1 NBO-Ar-400, there is an oxygen peak formed by oxygen vacancies, but in the original sample there is no such peak. The larger OH in the original sample is caused by hydrothermal.

[0057] Figure 6 The electron sequential resonance spectrum of the oxygen vacancy relative concentration comparison of the Nb2O5 catalyst containing oxygen vacancies is constructed for the present invention. Figure 6 As shown, the sample calcined in air, such as Comparative Example 1, has almost no spin resonance peak of oxygen vacancies, while the samples calcined in argon under the same conditions, such as Examples 1 and 2, show spin resonance peaks of oxygen vacancies. The existence of oxygen vacancies constructed in Examples 1 and 2 can not only improve the visible light utilization rate of the catalyst and promote the separation of photogenerated electrons and holes, but also become active sites for photocatalytic reactions. The abundant oxygen vacancies in Examples 1 and 2 are an important factor that makes their photocatalytic activity higher than that of the NBO catalyst in Comparative Example 1.

[0058] Figure 7 The Raman spectrum of the Nb2O5 catalyst containing oxygen vacancies is constructed for the present invention. Figure 7 As shown, the Raman spectrum of Sample Example 1 calcined at 400° C. under argon was found to have a red shift, which once again proved the existence of oxygen vacancies in its structure.

[0059] Figure 8 The UV-visible absorption spectrum of the Nb2O5 catalyst containing oxygen vacancies is constructed for the present invention. Figure 8 As shown, after calcination under argon, Example 1 and Example 2 have a certain red shift, and the absorption wavelength moves toward infrared light. The wider light absorption range can provide more photogenerated electrons for the catalyst to participate in the photocatalytic reaction, which is another factor that the photocatalytic activity of Example 1 and Example 2 is higher than that of the NBO catalyst in Comparative Example 1.

[0060] The Nb2O5 catalysts prepared in Example 1-2 and Comparative Example 1-2 were subjected to photocatalytic research, and the photocatalytic CO2 test process was as follows:

[0061] 5mL deionized water (providing the water vapor required for reducing carbon dioxide) is added to the reactor, and 50mg sample is evenly spread on the glass plate in the glass reactor. Before illumination, the reactor is filled with Ar gas, and 1mL high-purity CO2 gas is injected into the reactor. Subsequently, a 300W xenon lamp is used to irradiate from the top of the reactor to react. Then, 1mL gas is extracted from the reactor every 30min and injected into a gas chromatograph (Zhejiang Fu Li, GC9790II). The amount of the substance of the reduction product CH4 and CO is determined respectively using the external standard method, and the selectivity of the catalyst photocatalytic reduction production CH4 is calculated by comparison.

[0062] Fig. 9 A graph showing the relationship between the amount of CH4 produced by photocatalytic reduction of CO2 per unit mass of Nb2O5 catalyst containing oxygen vacancies and the time of the photocatalytic reduction of CO2 per unit mass of Nb2O5 catalyst is constructed for the present invention. Fig. 9 As shown, Example 1 NBO-Ar-400 exhibits the best photocatalytic activity.

[0063] Fig.10 The present invention constructs a graph showing the relationship between the amount of CO produced by photocatalytic reduction of CO2 per unit mass of Nb2O5 catalyst containing oxygen vacancies and the time. Fig.10 As shown, Example 1 NBO-Ar-400 exhibits the best photocatalytic activity.

[0064] Fig.11 The selectivity data diagram of CH4 production by photocatalytic reduction of Nb2O5 catalyst containing oxygen vacancies is constructed for the present invention (calculated based on the amount of CH4 and CO produced per unit catalyst per unit time). Fig.11 As shown, Example 1 NBO-Ar-400 exhibits the highest selectivity for photocatalytic reduction of CO2 to produce CH4, reaching 87.3%.

[0065] Based on the above data, NBO-Ar-400 in Example 1 exhibits the highest photocatalytic reduction activity for CO2 and product CH4 selectivity, which is due to its unique amorphous structure, mesoporous morphology of nanoparticle stacking, abundant oxygen vacancies, and wider light absorption range.

[0066] It should be noted that when the present invention involves a numerical range, it should be understood that the two endpoints of each numerical range and any value between the two endpoints can be selected. Since the steps and methods used are the same as those in the embodiments, in order to avoid redundancy, the present invention describes a preferred embodiment. Although the preferred embodiments of the present invention have been described, those skilled in the art may make additional changes and modifications to these embodiments once they know the basic creative concept. Therefore, the attached claims are intended to be interpreted as including the preferred embodiments and all changes and modifications that fall within the scope of the present invention.

[0067] Obviously, those skilled in the art can make various changes and modifications to the present invention without departing from the spirit and scope of the present invention. Thus, if these modifications and variations of the present invention fall within the scope of the claims of the present invention and their equivalents, the present invention is also intended to include these modifications and variations.

Claims

1. A method for preparing a Nb2O5 photocatalyst rich in oxygen vacancies, characterized in that: The following steps are involved: A soluble niobium salt is used as a precursor, and water is added to prepare hydrated niobium pentoxide powder by a hydrothermal method; the niobium pentoxide powder is placed under a protective gas and calcined at 400-600°C to obtain a Nb2O5 photocatalyst rich in oxygen vacancies; The protective gas is an inert gas or nitrogen.

2. The method for preparing the oxygen vacancy-rich Nb2O5 photocatalyst according to claim 1, characterized in that: The soluble niobium salt is niobium pentachloride or niobium oxalate.

3. The method for preparing the Nb2O5 photocatalyst rich in oxygen vacancies according to claim 1, characterized in that: The molar volume ratio of the soluble niobium salt to water is 0.5-2 mmol:30 mL.

4. The method for preparing the Nb2O5 photocatalyst rich in oxygen vacancies according to claim 1, characterized in that: The temperature of the hydrothermal reaction is 140-180°C and the time is 24 h.

5. The method for preparing the Nb2O5 photocatalyst rich in oxygen vacancies according to claim 1, characterized in that: The calcination heating rate is 1-10 °C / min.

6. The method for preparing the Nb2O5 photocatalyst rich in oxygen vacancies according to claim 1, characterized in that: The calcination time is 1 to 3 h.

7. A Nb2O5 photocatalyst rich in oxygen vacancies prepared by the preparation method according to any one of claims 1 to 6.

8. The use of the Nb2O5 photocatalyst rich in oxygen vacancies according to claim 7 in photocatalysis, characterized in that: The Nb2O5 photocatalyst selectively reduces CO2.

Citation Information

Patent Citations

  • Black titanium dioxide light nano material rich in oxygen vacancy defects as well as preparation method and application thereof