A method for preparing porcelain tiles at ultra-low temperature using rare earth tailings and its products

Through the multi-composite flux system of rare earth tailings, potash feldspar, albite, boronite and other raw materials, the porcelain bricks are sintered at low temperature, which solves the problems of high firing temperature of ceramic bricks and low utilization rate of rare earth tailings, and achieves Highly efficient, energy-saving and environmentally friendly production results.

CN117567136BActive Publication Date: 2024-10-29JINGDEZHEN CERAMIC UNIV
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202311590356.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-11-27
Publication Date
2024-10-29
Estimated Expiration
2043-11-27

AI Technical Summary

Technical Problem

Ceramic bricks are fired at high temperatures, consume a lot of energy, and have low utilization rates of rare earth tailings, resulting in huge production costs and environmental pressure. Moreover, the cooling effect of existing technologies is not obvious, which can easily lead to product deformation and cracking.

Method used

Rare earth tailings, potassium feldspar, albite, boronite and other raw materials are used to form a multi-component composite flux system. Through ball milling, drying, granulation and dry pressing molding processes, porcelain bricks are sintered at low temperature, and the sintering temperature is reduced to 1000~1060 ℃, improve the utilization rate of rare earth tailings and form a glass phase to enhance mechanical properties.

Benefits of technology

It significantly reduces the firing temperature, increases the flexural strength and density of porcelain bricks, broadens the sintering temperature range, achieves efficient utilization of rare earth tailings, reduces energy consumption and environmental pollution, and meets the performance requirements of national standards.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117567136B_ABST
    Figure CN117567136B_ABST
Patent Text Reader

Abstract

The invention discloses a method for preparing a porcelain tile by using rare earth tailings at ultra-low temperature and a product thereof. The raw materials of the porcelain tile blank are composed of 7.5-7.7wt% of black mud, 13.5-14.1wt% of Jinxi sodium sand, 4.6-4.9wt% of albite, 1.9-2.1wt% of potassium feldspar, 64.7-66.5wt% of rare earth tailings and 5.0-7.5wt% of colemanite. A multi-component composite flux system "K2O-Na2O-CaO-MgO-B2O3" formed by using rare earth tailings, potassium feldspar, albite and colemanite as composite fluxes significantly reduces the sintering temperature and broadens the sintering temperature range. In addition, the introduction amount of the rare earth tailings of the invention is greatly increased (>60%), which not only realizes the resource-efficient utilization of the rare earth tailings and reduces the environmental pressure caused by the large amount of waste of the rare earth tailings, but also greatly reduces the firing temperature, which is beneficial to saving energy and reducing environmental pollution, and has important significance for the sustainable development of building ceramic production.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of building ceramic materials, and in particular to a method for preparing porcelain tiles at ultra-low temperature by utilizing rare earth tailings and products thereof. Background Art

[0002] The firing temperature of ceramic tiles is generally between 1150 and 1220°C, which not only consumes a lot of energy, but also produces a lot of waste gas. The production cost and environmental pressure are huge, which restricts the sustainable development of the industry. At present, the existing ceramic tiles mostly use potassium feldspar as the main flux raw material, and introduce CaO to form a composite flux by adding wollastonite, dolomite, etc. to reduce the firing temperature, but the cooling effect is not obvious, generally 1100-1185°C, and it is easy to cause problems such as product deformation and cracking. For example, on the basis of the binary "K2O-Na2O" flux, the introduction of wollastonite and other multi-component composite fluxes to replace part of the potassium feldspar can reduce the firing temperature, but the cooling effect is not obvious; for example, the firing temperature of ceramic tiles prepared by "K2O-Na2O-CaO-MgO" composed of potassium feldspar, sodium feldspar, dolomite and other fluxes is still relatively high, and compared with the national standard requirements (35MPa), the flexural strength is not significantly improved.

[0003] Therefore, how to use rare earth tailings to turn waste into treasure and apply them to building ceramics has become one of the research hotspots. However, the utilization rate of rare earth tailings is only 10-25% at present. This is because when rare earth tailings are used in large quantities, not only the firing temperature is increased, but also the strength of the green body after firing is not high. Therefore, while improving the utilization rate of rare earth tailings, significantly reducing the firing temperature and improving product quality has very important economic and social benefits. Summary of the invention

[0004] The purpose of the present invention is to overcome the shortcomings of the prior art and provide a method for preparing porcelain tiles using rare earth tailings at ultra-low temperature, so as to solve the problems of high firing temperature, high energy consumption and low utilization rate of rare earth tailings in the current porcelain tiles. Another purpose of the present invention is to provide a product obtained by the above preparation method.

[0005] The purpose of the present invention is achieved through the following technical solutions:

[0006] The invention provides a method for preparing porcelain tiles at ultra-low temperature by using rare earth tailings. The raw materials of the porcelain tile blank are composed of 7.5-7.7wt% of black mud, 13.5-14.1wt% of Jinxi sodium sand, 4.6-4.9wt% of albite, 1.9-2.1wt% of potassium feldspar, 64.7-66.5wt% of rare earth tailings and 5.0-7.5wt% of colemanite. The preparation method comprises the following steps:

[0007] (1) mixing the raw materials according to a ratio, and then ball milling to obtain a slurry;

[0008] (2) sieving and drying the slurry, and then granulating the slurry to obtain a powder;

[0009] (3) the powder is sieved, aged, and dry-pressed to obtain a green body;

[0010] (4) The green body enters into a firing device, is heated to 1000-1060° C. at a rate of 3-5° C. / min, is kept at that temperature for 10-20 min, and is naturally cooled to obtain a ceramic tile body.

[0011] In the above scheme, the chemical composition of the rare earth tailings described in the present invention is SiO247.28-47.50wt%, Al2O319.36-20.53wt%, Fe2O31.78-1.95wt%, TiO20.10-0.25wt%, CaO 20.94-21.35wt%, MgO 0.32-0.54wt%, K2O 4.13-4.30wt%, Na2O 0.78-0.96wt%, SrO0.01-0.10wt%, IL3.52-3.72wt%.

[0012] Furthermore, in the step (1) of the present invention, the ball milling is carried out at a ratio of ball: material: water = 1.9-2.1: 1: 0.6-0.8, and the ball milling time is 10-12 minutes. In the step (2), the drying temperature is 90-120° C., and the drying time is 3-6 hours. In the step (3), the pressure of dry pressing is 10-15 MPa, and the holding time is 10-20 seconds.

[0013] The product prepared by the preparation method of the present invention comprises the following chemical compositions: SiO2 50.8-52.1wt%, Al2O3 19.5-19.94wt%, CaO 17.3-18.1wt%, MgO 0.4-0.5wt%, K2O 4.0-4.3wt%, Na2O 1.5-1.7wt%, Fe2O3 1.6-1.8wt%, TiO2 0.1-0.3wt%, B2O3 2.3-3.6wt%, SrO 0.01-0.02wt%.

[0014] The present invention has the following beneficial effects:

[0015] (1) The present invention utilizes rare earth tailings rich in CaO and MgO to replace the commonly used raw materials such as wollastonite and dolomite, and by adding raw materials such as colemanite, a multi-component composite flux system "K2O-Na2O-CaO-MgO-B2O3" with rare earth tailings, potassium feldspar, sodium feldspar and colemanite as composite fluxes is formed. Compared with the prior art that uses wollastonite and dolomite to form a multi-component composite flux system, the present invention has a more obvious low-temperature sintering effect (sintering temperature is 1000-1060°C) and significantly broadens the sintering temperature range.

[0016] (2) The CaO in the rare earth tailings of the present invention is more conducive to forming a low eutectic point glass phase at low temperature. The introduction of rare earth tailings with a high Al2O3 content (>60%) increases its high-temperature liquid phase viscosity, which helps to densify the green body and reduce voids, thereby giving the green body better mechanical properties and sintering properties. The prepared porcelain tile green body has a water absorption rate of 0.03-0.23%, a flexural strength of 72.50-75.45 MPa, a sintering shrinkage rate of 9.8-11.5%, and a volume density of 2.3547-2.3958 g / cm 3 .

[0017] (3) The amount of rare earth tailings introduced by the present invention is greatly increased (>60%), which not only realizes the resource-efficient utilization of rare earth tailings, solves the problems of low rare earth tailings consumption at present, reduces the environmental pressure caused by the large amount of waste of rare earth tailings, but also greatly reduces the firing temperature, which is conducive to saving energy and reducing environmental pollution, has very important economic and social benefits, and is of great significance to the sustainable development of building ceramics production. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] The present invention will be further described in detail below with reference to the embodiments and accompanying drawings:

[0019] Figure 1 is the XRD diffraction pattern of the porcelain tile body prepared in the embodiment of the present invention;

[0020] Figure 2 The following are surface SEM photos of the porcelain tile bodies prepared in the examples of the present invention at different magnifications (a: 500 times; b: 2000 times). DETAILED DESCRIPTION

[0021] The present invention discloses a method for preparing porcelain tiles by ultra-low temperature using rare earth tailings. The raw materials of the porcelain tile blank are composed of 7.5-7.7wt% black mud, 13.5-14.1wt% Jinxi sodium sand, 4.6-4.9wt% albite, 1.9-2.1wt% potassium feldspar, 64.7-66.5wt% rare earth tailings, and 5.0-7.5wt% colemanite. The rare earth tailings are rare earth tailings from Shangrao, Jiangxi Province. The chemical composition of each raw material is shown in Table 1.

[0022] Table 1 Experimental raw materials and their chemical composition (wt%)

[0023]

[0024] Embodiment 1:

[0025] This embodiment provides a method for preparing porcelain tiles at ultra-low temperature using rare earth tailings. The raw materials of the porcelain tile blank are composed of 7.5wt% black mud, 13.7wt% Jinxi sodium sand, 4.6wt% albite, 2.0wt% potassium feldspar, 64.7wt% rare earth tailings, and 7.5wt% colemanite. The preparation method has the following steps:

[0026] (1) After mixing the above raw materials according to the ratio, ball milling was performed at a ratio of ball: material: water = 2: 1: 0.6 for 12 min to obtain a slurry;

[0027] (2) the slurry is passed through a 100-mesh sieve with a residue of ≤3%, and then dried at 110° C. for 4 h, and granulated to obtain a powder;

[0028] (3) The powder is sieved through a 40-mesh sieve, aged, and dry-pressed at 15 MPa for 10 seconds to obtain a green body;

[0029] (4) The green body is put into the firing equipment, heated to 1000°C at a rate of 3°C / min, kept at that temperature for 20min, and cooled naturally to obtain a ceramic tile body.

[0030] Embodiment 2:

[0031] This embodiment provides a method for preparing porcelain tiles at ultra-low temperature using rare earth tailings. The raw materials of the porcelain tile blank are composed of 7.7wt% black mud, 14.0wt% Jinxi sodium sand, 4.7wt% albite, 2.1wt% potassium feldspar, 66.5wt% rare earth tailings, and 5.0wt% colemanite. The preparation method has the following steps:

[0032] (1) After mixing the above raw materials according to the ratio, ball milling was performed at a ratio of ball: material: water = 2: 1: 0.8 for 11 min to obtain a slurry;

[0033] (2) passing the slurry through a 100-mesh sieve with a residue of ≤3%, and then drying at 120° C. for 3 h, and granulating to obtain a powder;

[0034] (3) The powder is sieved through a 40-mesh sieve, aged, and dry-pressed at 13 MPa for 20 seconds to obtain a green body;

[0035] (4) The green body is placed in a firing device, heated to 1060°C at a rate of 4°C / min, kept at that temperature for 10 minutes, and cooled naturally to obtain a ceramic tile body.

[0036] Embodiment three:

[0037] This embodiment provides a method for preparing porcelain tiles at ultra-low temperature using rare earth tailings. The raw materials of the porcelain tile blank are composed of 7.5wt% black mud, 13.7wt% Jinxi sodium sand, 4.6wt% albite, 2.0wt% potassium feldspar, 64.7wt% rare earth tailings, and 7.5wt% colemanite. The preparation method has the following steps:

[0038] (1) After mixing the above raw materials according to the ratio, ball milling was performed at a ratio of ball: material: water = 2: 1: 0.7 for 12 min to obtain a slurry;

[0039] (2) passing the slurry through a 100-mesh sieve with a residue of ≤3%, and then drying at 100° C. for 5 h, and granulating to obtain a powder;

[0040] (3) The powder is sieved through a 40-mesh sieve, aged, and dry-pressed at 15 MPa for 15 seconds to obtain a green body;

[0041] (4) The green body is put into the firing equipment, heated to 1020°C at a rate of 3°C / min, kept at that temperature for 15 minutes, and cooled naturally to obtain a ceramic tile body.

[0042] Embodiment 4:

[0043] This embodiment provides a method for preparing porcelain tiles at ultra-low temperature using rare earth tailings. The raw materials of the porcelain tile blank are composed of 7.6wt% black mud, 13.5wt% Jinxi sodium sand, 4.9wt% albite, 1.9wt% potassium feldspar, 65.4wt% rare earth tailings, and 6.7wt% colemanite. The preparation method has the following steps:

[0044] (1) After mixing the above raw materials according to the ratio, ball milling was performed at a ratio of ball: material: water = 1.9: 1: 0.8 for 10 min to obtain a slurry;

[0045] (2) the slurry is passed through a 100-mesh sieve with a residue of ≤3%, and then dried at 90° C. for 6 h, and granulated to obtain a powder;

[0046] (3) The powder is sieved through a 40-mesh sieve, aged, and dry-pressed at 10 MPa for 10 seconds to obtain a green body;

[0047] (4) The green body is placed in a firing device, heated to 1040°C at a rate of 5°C / min, kept at that temperature for 12 minutes, and cooled naturally to obtain a ceramic tile body.

[0048] The chemical composition of the ceramic tile body prepared in the embodiment of the present invention is shown in Table 2; the performance test was carried out according to the national standard GB-T4100-2015, and the test results are shown in Table 3.

[0049] Table 2 Chemical composition of the porcelain tile body prepared in the embodiment of the present invention (wt%)

[0050]

[0051] Table 3 Performance test results of porcelain tile bodies prepared in the embodiments of the present invention

[0052]

[0053] The results in Table 3 show that the sintering performance of the porcelain tile body is good, the water absorption rate is less than 0.3%, and the flexural strength is greater than 70MPa, which meets the national standard requirements.

[0054] from Figure 1 It can be seen that the main crystal phase of the porcelain tile body is feldspar, indicating that its firing temperature is low. Figure 2 It can be seen that the formation of glass phase by feldspar at high temperature helps to densify the body and reduce voids, thus giving the porcelain tile body better mechanical strength and sintering properties.

Claims

1. A method for preparing porcelain tiles using rare earth tailings at ultra-low temperature, characterized in that: The raw material composition of the porcelain tile body is black mud 7.5-7.7wt%, Jinxi sodium sand 13.5-14.1wt%, sodium feldspar 4.6-4.9wt%, potassium feldspar 1.9-2.1wt%, rare earth tailings 64.7-66.5wt%, and colemanite 5.0-7.5wt%; the chemical composition of the rare earth tailings is SiO2 47.28-47.50wt%, Al2O3 19.36-20.53wt%, Fe2O3 1.78-1.95wt%, TiO2 0.10-0.25wt%, CaO 20.94-21.35wt%, MgO 0.32-0.54wt%, K2O 4.13-4.30wt%, Na2O 0.78-0.96wt%, SrO 0.01~0.10wt%, IL3.52~3.72wt%; the preparation method comprises the following steps: (1) mixing the raw materials according to the ratio, and then ball milling them at a ratio of ball: material: water = 1.9-2.1: 1: 0.6-0.8 for 10-12 minutes to obtain a slurry; (2) sieving the slurry, drying it at 90 to 120° C. for 3 to 6 hours, and granulating it to obtain a powder; (3) The powder is sieved, aged, and dry pressed to obtain a green body, wherein the dry pressing pressure is 10 to 15 MPa and the holding time is 10 to 20 seconds; (4) The green body enters the firing equipment, is heated to 1000-1060°C at a rate of 3-5°C / min, is kept at this temperature for 10-20min, and is naturally cooled to obtain a ceramic tile body. The ceramic tile body has a water absorption rate of 0.03-0.23%, a flexural strength of 72.50-75.45MPa, a firing shrinkage rate of 9.8-11.5%, and a bulk density of 2.3547-2.3958g / cm 3 .

2. The product obtained by the preparation method according to claim 1.

3. The product according to claim 2, characterized in that: The chemical composition of the porcelain tile body is SiO2 50.8-52.1wt%, Al2O3 19.5-19.94wt%, CaO 17.3-18.1wt%, MgO 0.4-0.5wt%, K2O 4.0-4.3wt%, Na2O 1.5-1.7wt%, Fe2O3 1.6-1.8wt%, TiO2 0.1-0.3wt%, B2O3 2.3-3.6wt%, and SrO 0.01-0.02wt%.

Citation Information

Patent Citations

  • Ceramic brick produced by using rare earth tailings and production method thereof

    CN102515695A