Positive electrode lithium supplement material and preparation method thereof, positive electrode sheet and secondary battery
By combining the first lithium-rich material and the coating material in the lithium-ion battery cathode material, and filling the cavity of the coating material with the second lithium-rich material, the problem of active lithium loss during the first charge and discharge process of the lithium-ion battery is solved. problem, improves lithium replenishment capacity and interface stability, and improves the overall performance of the battery.
Patent Information
- Application Number
- CN202311672998.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-12-05
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2043-12-05
AI Technical Summary
During the first charge and discharge process of lithium-ion batteries, a solid electrolyte interface film is formed on the surface of the negative electrode, resulting in irreversible loss of active lithium, thereby reducing the energy density and limiting the wide application of lithium-ion batteries.
By combining the first lithium-rich material and the coating material in the cathode material, and filling the cavity of the coating material with the second lithium-rich material, the advantages of both are used to increase the lithium replenishment capacity, and the coating material improves the lithium replenishment capacity. Air stability and conductivity, protecting the second lithium-rich material to reduce its direct contact with the electrolyte and improving interface stability.
It effectively improves the lithium replenishing capacity and interface stability of the positive electrode lithium replenishing material, reduces the gas production and residual alkali value, and improves the overall electrochemical performance.
Smart Images

Figure CN117577848B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of secondary batteries, and in particular to a positive electrode lithium supplement material and a preparation method thereof, a positive electrode plate and a secondary battery. Background Art
[0002] The intermittent and periodic nature of renewable energy sources seriously hinders their widespread application. An effective measure to solve this problem is to convert them into chemical energy and store them. Among various energy storage systems, electrochemical energy storage is favored by people because of its high energy conversion efficiency and less space constraints. Among various electrochemical energy storage devices, secondary batteries, especially lithium-ion batteries (LIBs), have attracted widespread attention due to their high energy density and power density. However, since LIBs will form a solid electrolyte interface film on the negative electrode surface during the first charge and discharge process, causing irreversible loss of active lithium, which in turn leads to a decrease in the capacity of the electrode material and a decrease in energy density, the widespread application of LIBs is seriously limited.
[0003] By adding lithium supplement materials to the positive electrode materials, the loss of active lithium during the first charge of LIBs can be compensated, effectively improving the energy density of LIBs. However, the capacity of conventional ternary lithium-rich materials is low; and although binary lithium-rich materials have higher capacity, their surface residual alkali is high, so the surface and interface structure is unstable, making it difficult to use them in positive electrode lithium supplement materials. Summary of the invention
[0004] The purpose of the present invention is to provide a positive electrode lithium supplement material and a preparation method thereof, a positive electrode plate and a secondary battery, so as to solve the problems of low energy density and poor interface stability of the positive electrode lithium supplement material.
[0005] To achieve the purpose of the present invention, the present invention provides the following technical solutions:
[0006] In a first aspect, the present invention provides a positive electrode lithium replenishing material, which includes a first lithium-rich material, a coating material and a second lithium-rich material, wherein the coating material is combined with the outer layer of the first lithium-rich material, and the coating material has a cavity; the second lithium-rich material is accommodated in the cavity, and the second lithium-rich material is different from the first lithium-rich material.
[0007] The present invention combines a coating material having a cavity on the outer layer of a first lithium-rich material, and fills the cavity of the coating material with a second lithium-rich material, thereby utilizing the combination of the first lithium-rich material and the second lithium-rich material, thereby combining the advantages of the two lithium-rich materials and increasing the lithium replenishment capacity of the positive electrode lithium replenishment material; and the coating material combined with the outer layer of the first lithium-rich material can also improve the air stability and conductivity of the first lithium-rich material; in addition, the second lithium-rich material filled in the cavity is protected by the coating material, which can reduce the direct contact between the second lithium-rich material and the electrolyte, thereby improving the interface stability of the second lithium-rich material.
[0008] In one embodiment, the coating material includes at least two metal oxides, and the cavity is formed between two adjacent metal oxides.
[0009] In one embodiment, the metal oxide has a porous structure. By setting the metal oxide to have a porous structure, on the one hand, more accommodation space can be provided for accommodating the second lithium-rich material, and on the other hand, the metal oxide with a porous structure can also manually accommodate the gas generated by the first lithium-rich material.
[0010] In one embodiment, the metal oxide includes a first metal oxide and a second metal oxide, the second metal oxide is coated on the outer layer of the first metal oxide, and the cavity is formed between the first metal oxide and the second metal oxide. By arranging the second metal oxide to coat the first metal oxide, and forming the cavity between the first metal oxide and the second metal oxide, that is, the cavity is located inside the coating material, thereby ensuring effective protection of the second lithium-rich material, and the periphery of the second lithium-rich material can increase the rate of lithium ion insertion and extraction by contacting with the metal oxide.
[0011] In one embodiment, the second metal oxide has a pore, and the cavity is connected to the outside through the pore. By providing the pores on the coating material, the gas generated on the surface of the first lithium-rich material can be adsorbed by the pores by utilizing the small hole effect formed by the pores, and the adsorbed gas can be contained in the cavity in the coating material, thereby achieving the purpose of reducing the gas generation of the positive electrode lithium supplement material.
[0012] In one embodiment, part of the second lithium-rich material is filled in the pores. By filling the pores with the second lithium-rich material, it is possible to reduce the entry of external water vapor into the cavity through the pores, thereby improving the stability of the second lithium-rich material in the cavity.
[0013] In one embodiment, the number of the cavities is multiple, and the multiple cavities are interconnected, or the multiple cavities are independent of each other. By setting the number of cavities in the coating material to be multiple, and the multiple interconnected or independent cavities can increase the volume inside the coating material, thereby increasing the carrying capacity of the coating material for the second lithium-rich material, which is beneficial to increasing the lithium replenishment capacity of the positive electrode lithium replenishment material.
[0014] In one embodiment, the outer surface of the first lithium-rich material is coated with a coating layer, and the coating layer includes the coating material. By forming the coating layer on the outer surface of the first lithium-rich material, the first lithium-rich material can be fully coated, which can reduce the intrusion of water vapor in the external environment and improve the stability of the first lithium-rich material in the air; on the other hand, the metal oxide in the coating layer can improve the conductivity of the positive electrode lithium-supplementing material and improve the electrical conductivity.
[0015] In one embodiment, the coating layer has a thickness ranging from 500 nm to 5 μm.
[0016] In one embodiment, the coating material further includes a carbon material, and the carbon material is filled in the core of the coating material.
[0017] In one embodiment, the chemical formula of the first lithium-rich material includes Li a1 M b1 O c1 , wherein M is at least one element selected from Fe, Ni, Mn, Cu, Zn, Co, Cr, Zr, Sb, Ti, V, Mo, and Sn, 1≤a1≤8, 0<b1, 0<c1<7.
[0018] In one embodiment, the chemical formula of the second lithium-rich material includes Li a2 A b2 , wherein A is one or more elements selected from S, P, I, Br, F, O, B, and Se, 1≤a2≤5, and 0<b2. In one embodiment, the mass ratio of the first lithium-rich material, the second lithium-rich material, and the coating material is 100:(1-10):(2-20).
[0019] In one embodiment, the volume ratio of the second lithium-rich material to the volume of the cavity is (0-1):1.
[0020] In one embodiment, the wall thickness of the coating material is 50 nm to 200 nm.
[0021] In one embodiment, the volume ratio of the first metal oxide to the second metal oxide is (2.5-6):1. In one embodiment, the specific surface area of the positive electrode lithium supplement material is 0.5 m 2 / g~60m2 / g.
[0022] In a second aspect, the present invention also provides a method for preparing a positive electrode lithium-replenishing material, comprising: mixing and sintering a first lithium-rich material and a precursor of a coating material so that the coating material is bonded to the outer surface of the first lithium-rich material and the coating material has a cavity; mixing and sintering a second lithium-rich material and the first lithium-rich material bonded with the coating material so that the second lithium-rich material is accommodated in the cavity, thereby obtaining the positive electrode lithium-replenishing material.
[0023] In a third aspect, the present invention further provides a positive electrode plate, comprising a current collector and an active material layer disposed on the current collector, wherein the active material layer comprises a positive electrode material and the positive electrode lithium replenishing material described in any one of the embodiments of the first aspect, or the active material layer comprises a positive electrode material and a positive electrode lithium replenishing material obtained by the preparation method of the positive electrode lithium replenishing material described in any one of the embodiments of the second aspect.
[0024] In a fourth aspect, the present invention further provides a secondary battery, comprising the positive electrode plate described in the third aspect, or the battery comprises the positive electrode lithium replenishing material described in any one of the embodiments of the first aspect, or the battery comprises the positive electrode lithium replenishing material obtained by the preparation method of the positive electrode lithium replenishing material described in any one of the embodiments of the second aspect. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0026] Figure 1 is a schematic cross-sectional view of a positive electrode lithium supplement material according to an embodiment;
[0027] Figure 2 is a partially enlarged schematic cross-sectional view of a positive electrode lithium supplement material according to an embodiment;
[0028] Figure 3 is a schematic cross-sectional view of a coating material and a second lithium-rich material according to an embodiment;
[0029] Figure 4 is a cross-sectional schematic diagram of a coating material and a second lithium-rich material according to another embodiment;
[0030] Figure 5 is a cross-sectional schematic diagram of a coating material and a second lithium-rich material according to another embodiment;
[0031] Figure 6 is a cross-sectional schematic diagram of a coating material and a second lithium-rich material according to another embodiment;
[0032] Figure 7 is a cross-sectional schematic diagram of a positive electrode lithium supplement material according to another embodiment;
[0033] Figure 8 The present invention is a flow chart of a method for preparing a positive electrode lithium supplement material according to an embodiment of the present invention. DETAILED DESCRIPTION
[0034] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0035] It should be noted that when a component is said to be "fixed to" another component, it can be directly on the other component or there can be a central component. When a component is said to be "connected to" another component, it can be directly connected to the other component or there can be a central component at the same time.
[0036] Unless otherwise defined, all technical and scientific terms used in the present invention have the same meaning as those commonly understood by those skilled in the art to which the present invention belongs. The terms used in the specification of the present invention are only for the purpose of describing specific embodiments and are not intended to limit the present invention. The term "and / or" used in the present invention includes any and all combinations of one or more of the related listed items.
[0037] Some embodiments of the present invention are described in detail below in conjunction with the accompanying drawings. In the absence of conflict, the following embodiments and features in the embodiments can be combined with each other.
[0038] The present invention provides a positive electrode lithium supplement material, please refer to Figure 1 and Figure 2 The positive electrode lithium supplement material includes a first lithium-rich material 10, a coating material 30 and a second lithium-rich material 20, wherein the coating material 30 is combined with the outer layer of the first lithium-rich material 10, and the coating material 30 has a cavity 31; the second lithium-rich material 20 is accommodated in the cavity 31, and the second lithium-rich material 20 is different from the first lithium-rich material 10.
[0039] Specifically, the first lithium-rich material 10 and the second lithium-rich material 20 can both be in granular form. The lithium-rich material (including the first lithium-rich material 10 and the second lithium-rich material 20) is a lithium source nucleus for lithium supplementation. The positive electrode lithium supplementation material is added to the electrode so that during the first cycle of charging, the lithium-rich material acts as a "sacrificial agent" to release all the lithium ions contained in it at one time as much as possible to supplement the irreversible lithium ions consumed by the negative electrode to form the SEI film, thereby maintaining the abundance of lithium ions in the battery system and improving the first efficiency and overall electrochemical performance of the battery.
[0040] In the embodiment of the present invention, the first lithium-rich material is one of a ternary lithium-rich material and a binary lithium-rich material, and the second lithium-rich material is the other of the ternary lithium-rich material and the binary lithium-rich material. The binary lithium-rich material has a higher lithium replenishing capacity, and the ternary lithium-rich material has a lower residual alkalinity value. The positive electrode lithium replenishing material in the present invention includes both ternary lithium-rich material and binary lithium-rich material. The lithium replenishing capacity of the positive electrode lithium replenishing material can be increased, the residual alkalinity value and gas production of the positive electrode lithium replenishing material can be reduced, and the stability of the positive electrode composite lithium replenishing material can be increased, so that the comprehensive performance of the positive electrode lithium replenishing material is more excellent.
[0041] Optionally, the first lithium-rich material 10 may be a ternary lithium-rich material, that is, including lithium element (Li), transition metal element (non-Li) and non-metal element (O), and the first lithium-rich material 10 may be a primary particle or a secondary particle formed by a plurality of primary particles. The chemical formula of the first lithium-rich material 10 includes Li a1 M b1 O c1 , wherein M is at least one element selected from Fe, Ni, Mn, Cu, Zn, Co, Cr, Zr, Sb, Ti, V, Mo, and Sn, 1≤a1≤8, 0<b1, 0<c1<7. In a specific embodiment, the first lithium-rich material 10 may be Li5FeO4, Li6MnO4, Li6CoO4, Li6ZnO4, Li2NiO2, Li2CuO2, Li2CoO2, Li2MnO2, Li2Ni 0.5 Mn 1.5 O4、Li2Ni d Cu (1-d) One or more of O2 (0<d<1) etc.
[0042] Optionally, the second lithium-rich material 20 may be a binary lithium-rich material, that is, including lithium (Li) and non-metallic elements (S or P, etc.). The chemical formula of the second lithium-rich material 20 includes Li a2 A b2, wherein A is one or more elements selected from S, P, I, Br, F, O, B, and Se, 1≤a2≤5, and 0<b2. In a specific embodiment, the first lithium-rich material 10 may be one or more selected from lithium sulfide (Li2S), lithium phosphide (Li3P), lithium iodide (LiI), and lithium bromide (LiBr).
[0043] Compared with other positive electrode lithium replenishment materials, the positive electrode lithium replenishment materials made of binary lithium-rich materials have a weaker binding force between lithium ions and anions, smaller polarization of binary lithium-rich materials, and a lower voltage platform required for charging, which can effectively reduce the activation barrier of binary lithium-rich materials, thereby significantly improving the efficiency of lithium ion deintercalation, so that the positive electrode lithium replenishment materials can have a higher lithium replenishment specific capacity. In addition, binary lithium-rich materials do not produce oxygen during the lithium replenishment process, which can reduce the risk of flatulence in lithium batteries.
[0044] Of course, in other embodiments, the first lithium-rich material 10 may be a binary lithium-rich material, and the second lithium-rich material 20 may be a ternary lithium-rich material, and the specific material types are not limited.
[0045] In one embodiment, a coating material 30 having a cavity 31 is combined with the outer surface of the first lithium-rich material 10, and the second lithium-rich material 20 is contained in the cavity 31. Specifically, the coating material 30 can be a hollow granular structure. For example, as shown in the figure, the marked part is the first lithium-rich material 10, the coating material 30 is connected to the outer surface of the first lithium-rich material 10, the cavity 31 is provided inside the coating material 30, and the second lithium-rich material 20 is also granular and contained in the cavity 31.
[0046] It can be understood that the coating material 30 is sleeved on the outer periphery of the second lithium-rich material 20 , so that the coating material 30 encapsulates and protects the second lithium-rich material 20 .
[0047] Optionally, the volume of the second lithium-rich material 20 may be equal to the volume of the cavity 31, that is, the entire outer surface of the second lithium-rich material 20 and the entire inner surface of the coating material 30 are connected, and the coating material 30 is coated on the outer surface of the second lithium-rich material 20. It can be understood that under this structure, the entire space of the cavity 31 is filled with the second lithium-rich material 20, and there is no gap or a very small gap between the second lithium-rich material 20 and the coating material 30.
[0048] Optional, please refer to Figure 2 , the volume of the second lithium-rich material 20 can also be smaller than the volume of the cavity 31, that is, part of the outer surface of the second lithium-rich material 20 is connected to part of the inner surface of the coating material 30. It can be understood that under this structure, part of the space of the cavity 31 is filled with the second lithium-rich material 20, and there is also a part of unfilled space between the coating material 30 and the second lithium-rich material 20.
[0049] It can be understood that, compared with the second lithium-rich material 20 , the coating material 30 can be an encapsulation layer of the second lithium-rich material 20 , that is, a layer coating the outer surface of the second lithium-rich material 20 to isolate it from external water vapor.
[0050] Optionally, the contour shape of the cavity 31 is not particularly limited and may be spherical or irregular.
[0051] Optionally, the particles of the coating material 30 may be independently distributed on the outer surface of the first lithium-rich material 10, that is, the particles of the coating material 30 are a discontinuous phase. Alternatively, the particles of the coating material 30 may be densely distributed on the outer surface of the first lithium-rich material 10, that is, the particles of the coating material 30 are a continuous phase.
[0052] The present invention combines a coating material 30 having a cavity 31 on the outer layer of a first lithium-rich material 10, and fills the second lithium-rich material 20 in the cavity 31 of the coating material 30, thereby utilizing the combination of the first lithium-rich material 10 and the second lithium-rich material 20, thereby combining the advantages of the two lithium-rich materials and increasing the lithium replenishment capacity of the positive electrode lithium replenishment material; and the coating material 30 combined on the outer layer of the first lithium-rich material 10 can also improve the air stability and conductivity of the first lithium-rich material 10; in addition, the second lithium-rich material 20 filled in the cavity 31 is protected by the coating material 30, which can reduce the direct contact between the second lithium-rich material 20 and the electrolyte, thereby improving the interface stability of the second lithium-rich material 20.
[0053] In one embodiment, if Figures 2 to 4 As shown, the coating material 30 includes at least two metal oxides (shown as 30A and 30B in the figure), and a cavity is formed between the two adjacent metal oxides. The two metal oxides can be a coating structure or a core-shell structure, that is, one metal oxide is coated on the outside of another metal oxide, and the cavity is formed between the shell and the core; or, the two metal oxides can also be a side-by-side connected structure, and the cavity is formed between the two.
[0054] In one embodiment, the precursor of the coating material 30 can be a MOFs material (a crystalline porous material with a periodic network structure formed by self-assembly of transition metal ions and organic ligands), and after preparing an LDHs material (layered double hydroxide) on the outer surface of the MOFs material, it is sintered at a high temperature to form a metal oxide. Therefore, the metal element of the metal oxide in the coating material 30 can be the metal element in the MOFs material and the LDHs material.
[0055] Optionally, the transition metal ions of the precursor of the coating material 30 (hereinafter referred to as MOFs) include but are not limited to Mg 2+ , Ca 2+、Ni 2+ 、Co 2+ 、Zn 2+ , Cu 2+ 、Al 3+ , Fe 3+ Cr 3+ , Mn 3+ 、In 3+ etc.; organic ligands include but are not limited to imidazole esters, terephthalic acid, etc.
[0056] Optionally, the transition metal ions of the precursor of the coating material 30 (hereinafter referred to as LDHs) include but are not limited to Mg 2+ , Ca 2+ 、Ni 2+ 、Co 2+ 、Zn 2+ , Cu 2+ 、Al 3+ , Fe 3+ Cr 3+ , Mn 3+ 、In 3+ Etc. Therefore, MOFs and LDHs can use the same metal ion material, so that the metal oxides in the obtained coating material 30 are of the same or different types.
[0057] Optionally, in this embodiment, the coating material 30 having the cavity 31 can be formed by: firstly mixing the first lithium-rich material 10 and the metal precursor and organic ligand of MOFs together to obtain the first lithium-rich material 10 with MOFs bound to the outer layer. Then, a salt solution having metal ions different from those of MOFs (hereinafter referred to as L solution) is mixed with the first lithium-rich material 10, and after the L solution reacts with MOFs, LDHs (having transition metal ions of MOFs and transition metal ions in the L solution) are formed on the MOFs, so that the first lithium-rich material 10 with LDHs@MOFs bound to the outer layer is obtained. Then, the first lithium-rich material 10 is sintered, MOFs forms a metal oxide, LDHs forms another (or multiple) metal oxides, and due to the different shrinkage volumes of LDHs and MOFs when heated, a cavity 31 is formed between the two metal oxides.
[0058] It is understandable that a metal oxide formed by MOFs has the same metal element as MOFs; another (or more) metal oxide formed by LDHs has the same metal element as LDHs. Based on the formation process of the coating material 30 having a cavity 31 provided above, the transition metal ions in LDHs@MOFs can react at high temperature to form metal oxides. Moreover, since the coordination metals in LDHs and MOFs can be diverse, the type of metal oxide formed is not specifically limited.
[0059] For example, MOFs have metal ions Co, the L solution is a nickel salt solution, and the formed LDHs have metal ions Co and Ni, so the coating material includes an oxide containing Co formed by MOFs, and an oxide containing Co and Ni formed by LDHs.
[0060] Optionally, the metal oxide in the coating material 30 has a spinel structure.
[0061] In one embodiment, the metal oxide has a porous structure. Specifically, each metal oxide in the above embodiments may have a porous structure, and the pore structure may be located inside or outside the metal oxide.
[0062] Optionally, each metal oxide has a porous structure; or, the connection between the two metal oxides also has holes, that is, a cavity 31 or a hole is formed at the connection between one metal oxide and another metal oxide. It can be understood that since MOFs can be porous structures, after MOFs are converted into metal oxides, part of the porous structure can be retained inside the metal oxide. Alternatively, the porous structure is formed by the organic ligands in MOFs after thermal cracking.
[0063] By setting the metal oxide to a porous structure, on the one hand, more accommodation space can be provided for accommodating the second lithium-rich material 20 , and on the other hand, the metal oxide with a porous structure can also manually accommodate the gas generated by the first lithium-rich material 10 .
[0064] In one implementation, please refer to Figures 2 to 4 The metal oxide includes a first metal oxide 30A and a second metal oxide 30B. The second metal oxide 30B is coated on the outer layer of the first metal oxide 30A. A cavity is formed between the first metal oxide 30A and the second metal oxide 30B.
[0065] Specifically, based on the metal raw materials of LDHs@MOFs, the coating material 30 can be made of LDHs and MOFs with different metal elements. For example, LDHs include Ni and Co, and MOFs include Co, so the formed metal oxides can be NiCo2O4 and Co3O4. Therefore, the first metal oxide 30A can be Co3O4, and the second metal oxide 30B can be NiCo2O4.
[0066] Optionally, based on the above embodiment, after the L solution is added to the first lithium-rich material 10, LDHs will be coated on the outer surface of MOFs. Since the MOFs and the LDHs bound to the outer surface have different shrinkage volumes when heated, MOFs form a first metal oxide 30A located inside, and LDHs form a second metal oxide 30B located on the outer layer. A cavity is formed between the first metal oxide 30A and the second metal oxide 30B.
[0067] Optional, please refer to Figure 4 The first metal oxide 30A, the second metal oxide 30B, and the cavity 31 (the second lithium-rich material 20) may be in an egg yolk-shell structure, wherein the second metal oxide 30B may be considered as an egg shell, the cavity 31 (the second lithium-rich material 20) may be considered as an egg white, and the first metal oxide 30A may be considered as an egg yolk.
[0068] Optionally, the volume of the cavity 31 may be greater than the volume of the second lithium-rich material 20, that is, the cavity 31 is not completely filled with the second lithium-rich material 20. By setting the volume of the cavity 31 to be greater than the volume of the second lithium-rich material 20, it is helpful to reduce the gas production of the positive electrode lithium supplement material. The first lithium-rich material 10 is a ternary lithium-rich material, so it has a higher gas production rate. The oxygen ions in the first lithium-rich material 10 can enter the cavity 31 through the coating material 30. The cavity 31 provides space for the oxygen ions to combine with each other to form oxygen, and the generated oxygen is contained in the cavity 31 and is difficult to escape, so the positive electrode lithium supplement material generates less gas after discharge.
[0069] By arranging the second metal oxide 30B to cover the first metal oxide 30A, and forming a cavity between the first metal oxide 30A and the second metal oxide 30B, that is, the cavity 31 is located inside the coating material 30, thereby ensuring effective protection of the second lithium-rich material 20, and the periphery of the second lithium-rich material 20 can increase the lithium ion deintercalation rate by contacting with the metal oxide.
[0070] In one embodiment, the metal elements in some metal oxides are also doped into the first lithium-rich material 10. Specifically, since secondary sintering is required in the process of preparing the positive electrode lithium supplement material, the second lithium-rich material 20 is sintered into the cavity 31. As a result, the metal elements M1 and M2 in the coating material 30 can enter the first lithium-rich material 10, thereby forming doping. The advantage of forming doping is that the metal elements M1 and M2 are mostly transition metal elements, which can exist stably in the first lithium-rich material 10, thereby improving the conductivity of lithium ions in the first lithium-rich material 10.
[0071] In one embodiment, the coating material 30 further includes a carbon material, and the carbon material is filled in the core of the coating material 30. Specifically, the carbon material can be mixed with the first metal oxide 30A, and together form the coating material 30 and enclose the cavity 31 mentioned above. The position of the carbon material in the coating material 30 is not specifically limited. It can be understood that the precursor MOFs of the coating material 30 has a C element, so after sintering, the C element is retained in the final coating material 30.
[0072] By providing a carbon material in the coating material 30 , the conductivity of the entire coating material 30 can be improved, so that the conductivity and structural stability of the first lithium-rich material 10 and the second lithium-rich material 20 can be improved by utilizing the coating material 30 .
[0073] In one implementation, please refer to Figure 5 The coating material 30 has a channel 32 therein, and the channel 32 connects the cavity 31 and the external space. Specifically, the channel 32 is opened from the inner surface of the coating material 30 (the side facing the second lithium-rich material 20) and extends to the outer surface of the coating material 30 (the side facing away from the second lithium-rich material 20).
[0074] Optionally, the cross-sectional shape of the pores 32 may be circular, elliptical or polygonal, and there is no specific limitation. The extension path and manner of the pores 32 in the coating material 30 are also not limited.
[0075] When the second lithium-rich material 20 is accommodated in the cavity 31, the second lithium-rich material 20 can flow into the cavity 31 through the pores 32 in the coating material 30. It can be understood that after the L solution is mixed with the MOFs, the L solution will form an etching effect on the outer surface of the MOFs, thereby forming LDHs and some holes, and during sintering, due to the different stress shrinkage of the two, the cavity 31 is formed while the holes are retained.
[0076] Optionally, since MOFs contain organic ligands, during the process of converting the organic ligands into carbon materials by heat, pores may also be formed in the generated metal oxides due to the shrinkage and pyrolysis of the materials.
[0077] Therefore, after the second lithium-rich material 20 and the coating material 30 are mixed and sintered, the second lithium-rich material 20 in a molten state can be received in the cavity 31 through the pores 32 .
[0078] In addition, the first lithium-rich material 10 is a ternary lithium-rich material, so the first lithium-rich material 10 has a higher gas production rate. After the first lithium-rich material 10 is discharged, the lattice oxygen at the outer surface combines with each other to form oxygen and escapes. The coating material 30 combined with the outer layer of the first lithium-rich material 10 has pores 32, and the pores 32 can absorb these gases through the pinhole effect.
[0079] Therefore, by setting the pores 32 on the coating material 30 and utilizing the small hole effect formed by the pores 32, the gas generated on the surface of the first lithium-rich material 10 can be adsorbed by the pores 32, and the adsorbed gas can be accommodated in the cavity 31 in the coating material 30, thereby achieving the purpose of reducing the gas production of the positive electrode lithium supplement material.
[0080] In one implementation, please refer to Figure 5 , part of the second lithium-rich material 20 is filled in the pores 32. Based on the above embodiment, since the second lithium-rich material 20 flows through the pores 32, the second lithium-rich material 20 can also be retained in the pores 32.
[0081] Therefore, it can be understood that in the positive electrode lithium supplement material, the pores 32 on the coating material 30 can be observed, that is, the pores left after not being completely filled by the second lithium-rich material 20. Alternatively, the pores 32 on the coating material 30 may not be observed, that is, they are completely filled by the second lithium-rich material 20.
[0082] By filling the pores 32 with the second lithium-rich material 20 , it is possible to reduce the amount of external water vapor entering the cavity 31 through the pores 32 , thereby improving the stability of the second lithium-rich material 20 inside the cavity 31 .
[0083] In one implementation, please refer to Figure 6 The number of cavities 31 is multiple, and the multiple cavities 31 are interconnected, or the multiple cavities 31 are independent of each other. Figure 6 As shown, there may be a plurality of cavities 31 in the coating material 30 , and the plurality of cavities 31 may be distributed in the coating material 30 in a point-like manner.
[0084] Optionally, the volumes of the plurality of cavities 31 are not all the same, and each cavity 31 may contain the second lithium-rich material 20 ; or part of the cavities 31 may contain the second lithium-rich material 20 .
[0085] Optionally, as shown in the figure, the plurality of cavities 31 are interconnected and can be connected through the pores 32 inside the coating material 30. The interconnected cavities 31 are conducive to increasing the volume of the second lithium-rich material 20 in the coating material 30.
[0086] Optionally, as shown in the figure, the multiple cavities 31 are independent of each other and can be connected to the external space through the pores 32 inside the coating material 30. Alternatively, the multiple cavities 31 are independent of each other and no pores 32 are connected to them. The independent cavities 31 can improve the surface stability of the second lithium-rich material 20 and reduce the alkalinity of the second lithium-rich material 20.
[0087] By setting the number of cavities 31 in the coating material 30 to be multiple, and multiple connected or independent cavities 31 can increase the volume inside the coating material 30, thereby increasing the carrying capacity of the coating material 30 for the second lithium-rich material 20, which is beneficial to increasing the lithium replenishment capacity of the positive electrode lithium replenishment material.
[0088] In one implementation, please refer to Figure 7 The outer surface of the first lithium-rich material 10 is coated with a coating layer 40, and the coating layer 40 includes a coating material 30. Specifically, the coating layer 40 is composed of the coating material 30, and is coated on the outer surface of the first lithium-rich material 10.
[0089] Optionally, the coating layer 40 may have a plurality of particles of the coating material 30, and the particles of the coating material 30 are continuously distributed on the outer surface of the first material, that is, the particles are interconnected to form the coating layer 40. The advantage of this structure is that there are gaps between the particles in the coating layer 40, which is conducive to increasing the specific surface area of the positive electrode lithium supplement material.
[0090] Optionally, the coating layer 40 can also be a dense layer, that is, the coating material 30 is non-granular, and the coating material 30 forms a dense coating shell on the outer surface of the first lithium-rich material 10, and the coating shell has a cavity 31. The dense coating layer 40 is more conducive to isolating the intrusion of water vapor in the external environment.
[0091] By making the coating material 30 form a coating layer 40 on the outer surface of the first lithium-rich material 10, the first lithium-rich material 10 can be fully coated. On the one hand, it can reduce the intrusion of water vapor from the external environment and improve the stability of the first lithium-rich material 10 in the air; on the other hand, the metal oxide and carbon material in the coating layer 40 can improve the conductivity of the positive electrode lithium supplement material and improve the electrical conductivity.
[0092] In one embodiment, the coating layer has a thickness ranging from 500 nm to 5 μm. Specifically, the coating layer may have a thickness of 500 nm, 800 nm, 1 μm, 1.5 μm, 2 μm, 2.5 μm, 3 μm, 3.5 μm, 4 μm, 4.5 μm, or 5 μm.
[0093] The coating layer that meets the above range can, on the one hand, completely cover the first lithium-rich material to avoid the invasion of external water vapor and provide a good conductive environment; on the other hand, it can also form a cavity with a larger total volume inside it to accommodate more second lithium-rich material and ensure the lithium replenishment capacity.
[0094] When the thickness of the coating layer is less than the above range, the coating layer (coating material) is thinner, and the volume provided for forming the cavity is smaller; thus, the cavity volume in the coating material is smaller, and the distribution density of the cavity in the coating layer is smaller; ultimately, the proportion of the second lithium-rich material in the positive electrode lithium supplement material is smaller, which is not conducive to improving the capacity of the positive electrode lithium supplement material. When the thickness of the coating layer is greater than the above range, the coating layer (coating material) is thicker, and the proportion of the coating material in the positive electrode lithium supplement material is higher; since the coating material does not contribute lithium ions, the gram capacity of the positive electrode lithium supplement material will be reduced.
[0095] In one embodiment, the mass ratio of the first lithium-rich material, the second lithium-rich material and the coating material is 100:(1-10):(2-20). Specifically, the mass ratio of the first lithium-rich material, the second lithium-rich material and the coating material can be 100:1:2, 100:5:2, 100:10:2, 100:1:10, 100:1:20, 100:5:10, 100:10:10, 100:5:5, 100:5:15, 100:10:15, 100:10:20.
[0096] The positive electrode lithium replenishing material that meets the above mass ratio can ensure the capacity of the positive electrode lithium replenishing material on the one hand, and on the other hand, can also ensure the conductivity and structural stability of the positive electrode lithium replenishing material.
[0097] When the mass ratio of the coating material is less than the above range, the content of the coating material is too little, resulting in a low proportion of the cavity, or a thin wall thickness of the coating material; it will result in less second lithium-rich material contained in the cavity, or incomplete protection of the second lithium-rich material by the coating material; thus, the surface residual alkali in the positive electrode lithium supplement material is high, and the interface stability of the second lithium-rich material is poor. When the mass ratio of the coating material is greater than the above range, the content of the coating material is too much, and the proportion of the coating material in the positive electrode lithium supplement material is high; because the coating material does not contribute lithium ions, the gram capacity of the positive electrode lithium supplement material will be reduced.
[0098] In one embodiment, the volume ratio of the second lithium-rich material to the cavity is 0 to 1: 1. Specifically, the volume ratio of the second lithium-rich material to the cavity can be 0: 1, 0.1: 1, 0.2: 1, 0.3: 1, 0.4: 1, 0.5: 1, 0.6: 1, 0.7: 1, 0.8: 1, 0.9: 1, 1: 1.
[0099] The positive electrode lithium replenishing material that meets the above volume and volume ratio can make the specific gravity of the accommodated second lithium-rich material reach a relatively suitable state. On the one hand, the cavity can capture the gas generated by the first lithium-rich material, and on the other hand, it can ensure the lithium replenishing capacity.
[0100] When the volume of the second lithium-rich material is smaller than the above range, the proportion of the second lithium-rich material is small, resulting in limited capacity of the positive electrode lithium-replenishing material to be increased by the second lithium-rich material, and the positive electrode lithium-replenishing material cannot reach the maximum lithium-replenishing capacity. When the volume of the second lithium-rich material is larger than the above range, there is less unfilled space in the cavity, resulting in the gas generated by the first lithium-rich material being unable to be captured and contained by the cavity, and the gas production of the positive electrode lithium-replenishing material increases.
[0101] In one embodiment, the wall thickness of the coating material is 50 nm to 500 nm. Specifically, the wall thickness of the coating material can be 50 nm, 100 nm, 150 nm, 200 nm, 250 nm, 300 nm, 350 nm, 400 nm, 450 nm, or 500 nm.
[0102] The wall thickness of the coating material satisfies the above range, and the coating material has a good wrapping effect on the second lithium-rich material. The coating material has a consistent thickness and a suitable mass ratio, which can ensure the capacity of the positive electrode lithium-supplementing material.
[0103] When the wall thickness of the coating material is less than the above range, the wall thickness of the coating material on the periphery of the second lithium-rich material is too thin, resulting in the coating material being unable to effectively stabilize the surface cross-section of the second lithium-rich material and reduce the surface alkalinity of the second lithium-rich material. When the wall thickness of the coating material is greater than the above range, the wall thickness of the coating material on the periphery of the second lithium-rich material is too thick, and the coating material accounts for a high proportion, which is not conducive to improving the capacity of the positive electrode lithium supplement material.
[0104] In one embodiment, the particle size of the first lithium-rich material is larger than that of the second lithium-rich material. When the particle size of the first lithium-rich material is too small, it is not conducive to the uniform dispersion of the material in the slurry, and when the particle size of the first lithium-rich material is too large, the lithium ion transmission path is too long and the delithiation voltage is too high. When the particle size of the second lithium-rich material is too small, it is easy to agglomerate; when the particle size of the second lithium-rich material is too large, it is difficult to fill into the cavity.
[0105] In one embodiment, the volume ratio of the first metal oxide to the second metal oxide is (2.5-6): 1. Specifically, the volume ratio of the first metal oxide to the second metal oxide may be 2.5:1, 3:1, 3.5:1, 4:1, 4.5:1, 5:1, 5.5:1, 6:1.
[0106] In one embodiment, the specific surface area of the positive electrode lithium supplement material is 0.5 m 2 / g~60m 2 / g. Specifically, the specific surface area of the positive electrode lithium supplement material can be 0.5m 2 / g, 1m 2 / g, 5m 2 / g, 10m 2 / g, 15m 2 / g, 20m 2 / g, 25m 2 / g, 30m 2 / g, 35m 2 / g, 40m 2 / g, 45m 2 / g, 50m 2 / g, 55m 2 / g, 60m 2 / g.
[0107] When the specific surface area is smaller than the above range, the lithium ion transmission rate is low. When the specific surface area is larger than the above range, the compaction density of the positive electrode sheet is affected.
[0108] In a second aspect, the present invention also provides a method for preparing a positive electrode lithium supplement material, please refer to Figure 8 , specifically used for preparing the positive electrode lithium supplement material in the first aspect. The preparation method comprises the following steps:
[0109] Step S10: mixing the precursors of the first lithium-rich material and the coating material and sintering them, so that the coating material is bonded to the outer surface of the first lithium-rich material and a cavity is formed in the coating material.
[0110] Step S20, mixing the second lithium-rich material and the first lithium-rich material combined with the coating material and sintering them so that the second lithium-rich material is accommodated in the cavity to obtain a positive electrode lithium supplement material.
[0111] Specifically, the selection of the first lithium-rich material and the second lithium-rich material may refer to the above embodiments, which will not be described in detail here.
[0112] Optionally, in the above step S10, the first lithium-rich material can be obtained by mixing the M source and the lithium source according to a molar ratio and sintering under a protective atmosphere. The sintering temperature can be 600° C. to 900° C., and the sintering time can be 3 h to 24 h. The lithium source includes at least one of lithium hydroxide, lithium carbonate, lithium oxide, lithium acetate and lithium oxalate.
[0113] Optionally, in the above step S10, the precursor of the coating material includes MOFs material and LDHs material, wherein the MOFs material needs to be first prepared on the outer surface of the first lithium-rich material, and then the LDHs material needs to be prepared on the outer surface of the MOFs.
[0114] Optionally, MOFs material is prepared on the outer surface of the first lithium-rich material, including: dissolving dimethylimidazole in a solvent and recording it as solution A, then dissolving M1 metal salt in a solvent and recording it as solution B, ultrasonically dispersing the first lithium-rich material in solution A, and then mixing solution A and solution B, and letting it stand for 24-48 hours to obtain the first lithium-rich material with MOFs bound to the surface.
[0115] Optionally, LDHs material is then prepared on the outer surface of the first lithium-rich material, including: adding the first lithium-rich material with MOFs bound to the surface to a solution of M2 metal salt, and after 30 to 60 minutes of reaction, obtaining the first lithium-rich material bound to LDHs@MOFs.
[0116] Optionally, the M1 metal salt and the M2 metal salt include one or more of nitrates, sulfates, and acetates.
[0117] It needs to be explained that the above reaction process is to allow LDHs to combine with MOFs and form etching. When the reaction time is too short, the cavity finally formed will be smaller and insufficient to accommodate the second lithium-rich material; when the reaction time is too long, the MOFs will be completely converted and etched, and a coating material with a cavity cannot be formed.
[0118] Optionally, in the above step S10, the first lithium-rich material combined with LDHs@MOFs needs to be sintered to obtain the first lithium-rich material having a coating material with cavities combined on the surface.
[0119] Optionally, the sintering temperature of the first lithium-rich material combined with LDHs@MOFs can be 300°C to 700°C.
[0120] Optionally, in the above step S20, the second lithium-rich material with a smaller particle size can be mixed with the first lithium-rich material combined with the coating material and sintered so that the second lithium-rich material in a molten state can be filled into the cavity. The sintering temperature can be 500° C. to 900° C., and the sintering time can be 6 h to 20 h.
[0121] The present invention prepares a coating material through MOF material and LDH material, and combines the coating material on the outer surface of the first lithium-rich material, thereby reducing the contact area between the first lithium-rich material and the external environment and improving the air stability of the first lithium-rich material; a cavity is also formed in the coating material to utilize the cavity to adsorb the gas generated after the first lithium-rich material is delithiated, thereby reducing the gas production of the material; at the same time, the present invention also fills the second lithium-rich material into the cavity of the coating material to prepare a new positive electrode lithium-supplementing material with stable structure, low alkalinity and high lithium-supplementing capacity; further, because the coating material is derived from MOF, the carbon material remaining after calcination can also improve the conductivity and structural stability of the first lithium-rich material, thereby improving the lithium ion release rate of the first lithium-rich material, and the second lithium-rich material with unstable surface interface is filled in the cavity of the coating material, so its conductivity and surface interface stability are also improved.
[0122] In a third aspect, the present invention further provides a positive electrode plate, which includes a current collector and an active material layer arranged on the current collector, the active material layer includes the positive electrode lithium replenishing material of the first aspect, or the active material layer includes the positive electrode lithium replenishing material obtained by the preparation method of the positive electrode lithium replenishing material of the second aspect.
[0123] In one embodiment, the positive electrode sheet includes a positive current collector, and the positive current collector has a positive active layer, and the positive active layer includes components such as positive active materials, positive lithium supplement materials, conductive agents, and binders. The present invention does not specifically limit these materials, and suitable materials can be selected according to actual application requirements. The positive current collector includes but is not limited to any one of copper foil and aluminum foil. The positive electrode active material can be a phosphate positive electrode active material and a ternary positive electrode active material. In a specific embodiment, it includes one or more of lithium cobaltate, lithium manganate, lithium iron phosphate, lithium manganese iron phosphate, lithium vanadium phosphate, lithium vanadium phosphate, fluoro vanadium lithium phosphate, lithium titanate, lithium nickel cobalt manganese oxide, and lithium nickel cobalt aluminum oxide. The conductive agent includes one or more of graphite, carbon black, acetylene black, graphene, carbon fiber, C60, and carbon nanotubes, and the content of the conductive agent in the positive electrode active layer is 3wt% to 5wt%. The types of binders include one or more of polyvinylidene chloride, soluble polytetrafluoroethylene, styrene-butadiene rubber, hydroxypropyl methylcellulose, methylcellulose, carboxymethyl cellulose, polyvinyl alcohol, acrylonitrile copolymer, sodium alginate, chitosan and chitosan derivatives, and the content of the binder in the positive electrode active layer is 2wt% to 4wt%.
[0124] In one possible implementation, the content of the positive electrode lithium replenishing material in the positive electrode active material can be controlled at 1% to 6% of the mass of the positive electrode active material. This ratio can just make up for the loss of active lithium in the battery during the first charging process. If the amount of positive electrode lithium replenishing material added to the positive electrode plate is too low, the active lithium lost in the positive electrode active material cannot be fully replenished, which is not conducive to improving the energy density and capacity retention rate of the battery. If the amount of positive electrode lithium replenishing material added to the positive electrode active material is too high, the negative electrode lithium plating may become serious and increase the cost. In some specific embodiments, in the positive electrode active material, the mass percentage of the positive electrode lithium replenishing material can be 1%, 2%, 4%, 6%, etc.
[0125] In a fourth aspect, the present invention further provides a secondary battery, wherein the secondary battery comprises the above-mentioned positive electrode plate, wherein the above-mentioned positive electrode lithium supplement material is added to the positive electrode plate, or the secondary battery comprises the positive electrode lithium supplement material obtained by the above-mentioned preparation method.
[0126] The technical solution of the present invention is described in detail below through specific embodiments.
[0127] Example 1
[0128] The positive electrode lithium supplement material provided in this embodiment includes a ternary lithium-rich material (Li6CoO4), a binary lithium-rich material (Li2S) and a coating material (NiCo2O4@Co3O4), wherein the coating material forms a coating layer on the outer surface of the first lithium-rich material. The mass ratio of the first lithium-rich material, the second lithium-rich material and the coating material is 100:5:10; the volume ratio of the first metal oxide to the second metal oxide is 3:1, and the average thickness of the coating layer is 3μm.
[0129] The preparation method of the positive electrode lithium supplement material comprises the following steps:
[0130] (1) The lithium source and the metal source are mixed, sintered at 700°C for 24 hours in a nitrogen atmosphere, and crushed to obtain a ternary lithium-rich material.
[0131] (2) Dissolve dimethylimidazole in methanol, denoted as solution A, dissolve cobalt nitrate in methanol solution, denoted as solution B, and ultrasonically disperse the ternary lithium-rich material in solution A. Mix solution A and solution B and let stand for 48 hours to obtain the Co-MOF-coated ternary lithium-rich material.
[0132] (3) The Co-MOF-coated ternary lithium-rich material was added to the nickel nitrate solution and stirred for 60 minutes to obtain the NiCo-LDH@Co-MOF-coated ternary lithium-rich material.
[0133] (4) The NiCo-LDH@Co-MOF-coated ternary lithium-rich material is calcined at 300-700°C. Due to the different shrinkage volumes of Co-MOF and NiCo-LDH under heat, a NiCo2O4@Co3O4-coated ternary lithium-rich material with a cavity is obtained.
[0134] (5) Li2S with smaller particle size is mixed with the ternary lithium-rich material in a certain mass ratio and sintered at 900℃ for 20h. The molten Li2S is filled into the cavity of NiCo2O4@Co3O4.
[0135] The coating material in the positive electrode lithium supplement material provided in this embodiment has a cavity formed therein, and the second lithium-rich material is accommodated in the cavity.
[0136] Example 2
[0137] The positive electrode lithium supplement material provided in this embodiment includes a ternary lithium-rich material (Li6CoO4), a binary lithium-rich material (Li2S) and a coating material (Co3O4), and the coating material forms a coating layer on the outer surface of the first lithium-rich material. Among them, the mass ratio of the first lithium-rich material, the second lithium-rich material and the coating material is 100:5:10; the average thickness of the coating layer is 3μm. The difference between the positive electrode lithium supplement material in this embodiment and that in embodiment 1 is that the coating material does not contain the second metal oxide NiCo2O4.
[0138] The difference between the preparation method of the positive electrode lithium supplement material and that of Example 1 is that step (3) is omitted, etching in a nickel nitrate solution is not performed, and calcination is performed directly.
[0139] Example 3
[0140] The positive electrode lithium supplement material provided in this embodiment includes a ternary lithium-rich material (Li6CoO4), a binary lithium-rich material (Li2S) and a coating material (FeCo2O4@ZnO), and the coating material forms a coating layer on the outer surface of the first lithium-rich material. Among them, the mass ratio of the first lithium-rich material, the second lithium-rich material and the coating material is 100:5:10; the thickness of the coating layer is 3μm. The difference between the positive electrode lithium supplement material in this embodiment and that in embodiment 1 is that different coating materials are used.
[0141] The difference between the preparation method of the positive electrode lithium supplement material and that of Example 1 is that the solution B in step (2) is replaced by a zinc nitrate solution, and the nickel nitrate in step (3) is replaced by a ferric nitrate solution.
[0142] Example 4
[0143] The positive electrode lithium supplement material provided in this embodiment includes a ternary lithium-rich material (Li6CoO4), a binary lithium-rich material (Li2S) and a coating material (NiCo2O4@Co3O4), and the coating material forms a coating layer on the outer surface of the first lithium-rich material. Among them, the mass ratio of the first lithium-rich material, the second lithium-rich material and the coating material is 100:5:10; the volume ratio of the first metal oxide to the second metal oxide is 5:1; the thickness of the coating layer is 3μm. The difference between the positive electrode lithium supplement material in this embodiment and that in embodiment 1 is that the volume proportion of NiCo2O4 in the coating material is increased.
[0144] The difference between the preparation method of the positive electrode lithium supplement material and that of Example 1 is that the etching time in step (3) is extended to 120 min.
[0145] Example 5
[0146] The positive electrode lithium supplement material provided in this embodiment includes a ternary lithium-rich material (Li6CoO4), a binary lithium-rich material (Li2S) and a coating material (NiCo2O4@Co3O4), and the coating material forms a coating layer on the outer surface of the first lithium-rich material. Among them, the mass ratio of the first lithium-rich material, the second lithium-rich material and the coating material is 100:5:20; the thickness of the coating layer is 3μm. The difference between the positive electrode lithium supplement material in this embodiment and that in embodiment 1 is that the mass proportion of the second lithium-rich material is increased.
[0147] The difference between the preparation method of the positive electrode lithium supplement material and that of Example 1 is that the mixing amount of Li2S in step (5) is increased.
[0148] Example 6
[0149] The positive electrode lithium supplement material provided in this embodiment includes a ternary lithium-rich material (Li5FeO4), a binary lithium-rich material (Li3N) and a coating material (NiCo2O4@Co3O4), and the coating material forms a coating layer on the outer surface of the first lithium-rich material. Among them, the mass ratio of the first lithium-rich material, the second lithium-rich material and the coating material is 100:5:10; the thickness of the coating layer is 3μm. The difference between the positive electrode lithium supplement material in this embodiment and that in embodiment 1 is that the first lithium supplement material is replaced by Li5FeO4, and the second lithium supplement material is replaced by Li3N.
[0150] The difference between the method for preparing the positive electrode lithium supplement material and that of Example 1 is that the lithium-rich material in step (1) and step (5) is replaced.
[0151] Comparative Example 1
[0152] This comparative example provides an uncoated ternary lithium-rich material (Li6CoO4).
[0153] Comparative Example 2
[0154] This comparative example provides an uncoated binary lithium-rich material (Li2S).
[0155] The positive electrode lithium replenishing materials provided in the above-mentioned Examples 1-6 and the positive electrode lithium replenishing materials provided in Comparative Examples 1-2 are respectively assembled into positive electrode sheets and lithium-ion batteries according to the following methods:
[0156] Positive electrode: The positive electrode lithium supplement material, SP and PVDF are mixed in a mass ratio of 90:4:6 to prepare a positive electrode slurry, the positive electrode slurry is coated on the surface of an aluminum foil, vacuum dried at 110°C overnight, and rolled to obtain a positive electrode sheet;
[0157] Negative electrode: Graphite, carboxymethyl cellulose (CMC), SBR and SP were mixed in a mass ratio of 95.8:1.2:2:1, and the mixture was ball-milled and stirred to obtain a negative electrode slurry. The negative electrode slurry was coated on the surface of copper foil, and vacuum dried at 110°C overnight to obtain a negative electrode sheet.
[0158] Electrolyte: Ethylene carbonate and ethyl methyl carbonate were mixed in a volume ratio of 3:7, and LiPF6 was added to form an electrolyte, and the concentration of LiPF6 was 1 mol / L;
[0159] Diaphragm: Polypropylene microporous separator;
[0160] Lithium-ion battery assembly: Assemble button-type lithium-ion full batteries in an inert atmosphere glove box in the order of graphite negative electrode sheet - separator - electrolyte - positive electrode sheet.
[0161] Related performance tests
[0162] Electrochemical performance test:
[0163] The electrochemical performance of each lithium-ion battery assembled in the above lithium-ion battery embodiment was tested under the following test conditions:
[0164] Constant current and constant voltage charging, the first cycle charge and discharge voltage is 2.5-4.3V, the current is 0.1C, and the cut-off current is 0.01C.
[0165] The gas production test method is as follows:
[0166] At 25°C, the battery was formed at room temperature at a rate of 0.055C, with a formation cut-off voltage of 2.0-4.15V. A battery gas production test device was used to detect the gas production of the battery after the formation to evaluate the gas production phenomenon of the battery.
[0167] The water absorption rate test method is as follows:
[0168] First, control the room humidity at 25°C, 30-35% relative humidity.
[0169] Second, take out 0.3-0.5g of sample from the glove box, one sample at a time, and take out another sample from the glove box after the test.
[0170] Third, place the weighing bottle in an analytical balance with a precision of 1 part per 100,000, close the door, and reset to zero.
[0171] Fourth, weigh 0.17-0.19 grams of the sample to be tested into the container, spread the material with a spoon, close the hatch, stabilize for 3-5 seconds, turn on the timer, and record the mass of the analytical balance as the value of 0min. Then record the values of 5min, 10min, 15min, and 20min respectively, and calculate the average absorption data for 10-20 minutes.
[0172] Calculation formula:
[0173] V=(w t2 -w t1 ) / w0*(t2-t1); unit: ppm / s. Where t1 and t2 represent time, w0 represents initial mass, and w t1 represents the mass at t1, w t2 represents the mass at t2.
[0174] The test results are shown in Table 1 below:
[0175] Table 1. Test results of embodiments and comparative examples
[0176]
[0177] From the test results of Example 1 and Comparative Examples 1-2 in Table 1, it can be seen that the first cycle charging capacity and cycle retention rate of the battery provided by Example 1 are higher than those of Comparative Examples 1 and 2, while the gas production and water absorption rate are lower than those of Comparative Examples 1 and 2. This shows that the compounding of ternary lithium-rich materials and binary lithium-rich materials in the present invention can effectively combine the advantages of the two, reduce the residual alkalinity value and water absorption rate of the ternary lithium-rich materials, and effectively give play to the advantages of high charging capacity of binary lithium-rich materials.
[0178] It can be seen from the test results of Example 1 and Example 2 in Table 1 that, compared with the use of a single metal oxide, the use of two metal oxides can easily form a larger cavity to better accommodate the second lithium-rich material and more effectively absorb the gas produced by the ternary lithium-rich material, thereby significantly reducing the corresponding water absorption rate and gas production.
[0179] It can be seen from the test results of Example 1 and Example 3 in Table 1 that the positive electrode lithium supplement material obtained by replacing different coating materials can also produce similar effects, which shows that the solution provided by the present invention has high applicability and industrial advantages.
[0180] It can be seen from the test results of Example 1 and Example 4 in Table 1 that by prolonging the etching time to increase the proportion of the outer layer material in the coating material, the stability of the positive electrode lithium supplement material will decrease. Since the MOFs material is over-etched, it cannot effectively coat the ternary lithium supplement material after being converted into a transition metal oxide, and the sealing of the cavity deteriorates, resulting in a significant increase in the gas production and water absorption rate of the corresponding positive electrode lithium supplement material, thereby causing the battery retention rate to decrease after multiple cycles.
[0181] It can be seen from the test results of Example 1 and Example 5 in Table 1 that increasing the mass proportion of binary lithium-rich materials in the positive electrode lithium supplement material will lead to a significant increase in the gas production and water absorption rate of the positive electrode lithium supplement material. Since the binary lithium-rich material occupies too much cavity space, it is not conducive to absorbing the gas production of the ternary lithium-rich material. At the same time, the strong water absorption disadvantage of more binary lithium-rich materials leads to a significant increase in the water absorption rate of the positive electrode lithium supplement material.
[0182] It can be seen from the test results of Example 1 and Example 6 in Table 1 that the positive electrode lithium supplement material obtained by replacing different ternary lithium-rich materials and binary lithium-rich materials can also produce similar effects, indicating that the solution provided by the present invention has high applicability and has the advantage of industrialization.
[0183] In the description of the embodiments of the present invention, it should be noted that the orientation or positional relationship of terms such as "center", "up", "down", "left", "right", "vertical", "horizontal", "inside" and "outside" are based on the orientation or positional relationship described in the accompanying drawings, and are only for the convenience of describing the present invention and simplifying the description, rather than indicating or implying that the referred device or element must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as a limitation on the present invention.
[0184] What is disclosed above is only a preferred embodiment of the present invention, and it certainly cannot be used to limit the scope of rights of the present invention. Ordinary technicians in this field can understand that all or part of the processes of the above embodiment and equivalent changes made according to the claims of the present invention still fall within the scope covered by the present invention.
Claims
1. A positive electrode lithium supplement material, characterized in that: include: A first lithium-rich material, wherein the first lithium-rich material is a ternary lithium-rich material; A coating material, combined with the outer layer of the first lithium-rich material, the coating material has a cavity inside, and the coating material includes a metal oxide; A second lithium-rich material is contained in the cavity, and the second lithium-rich material is different from the first lithium-rich material, and the second lithium-rich material is a binary lithium-rich material; Wherein, the chemical formula of the first lithium-rich material includes Li a1 M b1 O c1 , wherein M is at least one element selected from Fe, Ni, Mn, Cu, Zn, Co, Cr, Zr, Sb, Ti, V, Mo, and Sn, 1≤a1≤8, 0<b1, 0<c1<7; the chemical formula of the second lithium-rich material includes Li a2 A b2 , wherein A is one or more elements selected from S, P, I, Br, F, O, B, and Se, 1≤a2≤5, and 0<b2.
2. The positive electrode lithium supplement material according to claim 1, characterized in that: The coating material includes at least two metal oxides, and the cavity is formed between two adjacent metal oxides.
3. The positive electrode lithium supplement material according to claim 2, characterized in that: The metal oxide has a porous structure.
4. The positive electrode lithium supplement material according to claim 2, characterized in that: The metal oxide includes a first metal oxide and a second metal oxide. The second metal oxide is coated on the outer layer of the first metal oxide. The cavity is formed between the first metal oxide and the second metal oxide.
5. The positive electrode lithium supplement material according to claim 4, characterized in that: The second metal oxide has pores, and the cavity is connected to the outside through the pores; the volume ratio of the first metal oxide to the second metal oxide is (2.5-6):
1.
6. The positive electrode lithium supplement material according to claim 5, characterized in that: Part of the second lithium-rich material is filled in the pores.
7. The positive electrode lithium supplement material according to claim 1, characterized in that: There are multiple cavities, and the multiple cavities are interconnected, or the multiple cavities are independent of each other.
8. The positive electrode lithium supplement material according to claim 1, characterized in that: The overall thickness of the coating material combined with the outer surface layer of the first lithium-rich material is in the range of 500 nm to 5 μm.
9. The positive electrode lithium supplement material according to claim 1, characterized in that: The coating material further includes a carbon material, and the carbon material is filled in the core of the coating material.
10. The positive electrode lithium supplement material according to any one of claims 1 to 9, characterized in that: The mass ratio of the first lithium-rich material, the second lithium-rich material and the coating material is 100:(1-10):(2-20); And / or, the volume ratio of the second lithium-rich material to the volume of the cavity is (0-1):1; and / or, the wall thickness of the coating material is 50 nm to 200 nm; And / or, the specific surface area of the positive electrode lithium supplement material is 0.5m 2 / g~60m 2 / g.
11. A method for preparing a positive electrode lithium supplement material, characterized in that: The preparation method is used to prepare the positive electrode lithium supplement material according to any one of claims 1 to 10, comprising: Mixing and sintering the precursors of a first lithium-rich material and a coating material so that the coating material is bonded to the outer surface of the first lithium-rich material and has a cavity inside the coating material, wherein the first lithium-rich material is a ternary lithium-rich material, and the coating material includes a metal oxide; The second lithium-rich material and the first lithium-rich material combined with the coating material are mixed and sintered so that the second lithium-rich material is accommodated in the cavity to obtain the positive electrode lithium supplement material, wherein the second lithium-rich material is a binary lithium-rich material.
12. A positive electrode sheet, characterized in that: The positive electrode plate includes a current collector and an active material layer arranged on the current collector, the active material layer includes the positive electrode lithium replenishing material according to any one of claims 1 to 10, or the active material layer includes the positive electrode lithium replenishing material obtained by the preparation method of the positive electrode lithium replenishing material according to claim 11.
13. A secondary battery, characterized in that: The positive electrode sheet as claimed in claim 12, or the secondary battery comprises the positive electrode lithium replenishing material as claimed in any one of claims 1 to 10, or the secondary battery comprises the positive electrode lithium replenishing material obtained by the preparation method of the positive electrode lithium replenishing material as claimed in claim 11.
Citation Information
Patent Citations
Lithium supplement material and preparation method and application thereof
CN116477661A