A method for preparing sodium battery material

By real-time monitoring and adjustment of the fiber filament quality during the electrospinning process, the problems of low electrospinning efficiency and unstable fiber formation quality in the prior art are solved, and the conductivity and production efficiency of efficient preparation of sodium battery materials are achieved. promote.

CN117577927BActive Publication Date: 2024-11-05HEBEI GUONA NEW ENERGY TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202311545896.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-11-20
Publication Date
2024-11-05
Estimated Expiration
2043-11-20

AI Technical Summary

Technical Problem

In the existing preparation methods for sodium ion battery materials, electrospinning technology has low efficiency, large specific surface area of ​​the material, small compaction density, and the inability to monitor the quality of fiber filaments in real time, resulting in unstable fiber quality.

Method used

The carbon source of polymer and organic solvents are uniformly dispersed to form an electrospinning precursor liquid. The fiber filaments are formed by spraying, and the anisotropy and thickness uniformity of the fiber filaments are monitored in real time. The spinning parameters are adjusted according to the monitoring results to ensure that The precursor material quality is then mixed with other raw materials for drying and high temperature treatment.

Benefits of technology

It improves the production efficiency and fiber-forming quality of sodium battery materials, reduces the number of high-temperature treatments, saves energy, prevents the agglomeration of the positive electrode materials, forms a uniform conductive network, and enhances the conductivity of the material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117577927B_ABST
    Figure CN117577927B_ABST
Patent Text Reader

Abstract

The present invention relates to the technical field of sodium ion battery materials, and in particular to a method for preparing sodium battery materials, including selecting a high molecular polymer carbon source, one or more organic solvents and uniformly dispersing them in a set ratio to form a precursor solution for electrospinning; electrospinning the formed precursor solution to obtain a precursor material; determining various raw materials required for the sodium battery material, weighing the various raw materials according to chemical proportions and uniformly mixing them with the precursor material in a certain ratio to form a mixture; drying the formed mixture and high-temperature treating it to obtain the sodium battery material. The present invention does not need to mix the fiber precursor and the positive or negative electrode raw materials before preparing by electrospinning, which improves the production efficiency and the content of the positive electrode active substance, and monitors the fiber filaments formed by the electrospinning machine in real time, and makes timely adjustments based on the monitoring results, thereby ensuring the fiber quality.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of sodium ion battery materials, and in particular to a method for preparing sodium battery materials. Background Art

[0002] With the country's emphasis on the new energy development strategy, whether it is the development of power batteries or 3C batteries in recent years, sodium ion batteries and battery material preparation processes have made significant progress. Since the conductivity of sodium ion battery positive electrode materials (such as sodium vanadium phosphate, sodium manganate, Prussian blue, etc.) is generally poor, the conductivity of sodium ion battery positive electrode materials needs to be improved through ion doping, carbon coating and other processes during the preparation process. In the preparation process of existing battery materials, materials such as glucose and starch are often added, and carbonization is used to achieve the purpose of carbon coating of battery materials. This method has the advantages of simple preparation method and low material cost, but the battery materials are easy to agglomerate and have a large particle size. One-dimensional carbon materials (such as carbon nanotubes and carbon fibers) have received great attention due to their good conductivity. In order to improve the conductivity of battery materials, conductive agents such as carbon nanotubes and conductive carbon black need to be added during the batching process of the positive and negative electrodes of sodium ion batteries to reduce the internal resistance of the battery and increase the discharge rate of the battery. Some researchers have prepared battery materials / carbon nanofiber composite materials through electrospinning. The morphology prepared by this method is uniform and easy to control, and the one-dimensional structure has a short ion transmission path. It is a battery material preparation process with good application prospects.

[0003] In order to improve the conductivity of battery materials, the existing technology mainly adopts two routes: (1) the raw materials required for the positive or negative electrode are mixed with the carbon source precursor, prepared into a fiber precursor by electrostatic spinning technology, and then carbonized at high temperature. The main disadvantage of this method is that the preparation efficiency is low, mass production cannot be achieved, and the prepared material has a large specific surface area and a low compaction density or tap density; (2) the carbon source precursor is mixed and then electrostatically spun, the fiber precursor is carbonized at high temperature, the carbonized carbon fiber is mixed with the raw materials required for the positive or negative electrode, and then high-temperature treatment is performed again to obtain an electrode material / carbon fiber composite material. The main disadvantage of this method is that the method is complicated and energy consumption is high. Therefore, the existing technology still needs to be improved and developed.

[0004] Chinese Patent Publication No.: CN114906880A. A preparation method of a sodium ion battery positive electrode material and a sodium ion battery are disclosed, the preparation method comprising the following steps: dissolving a sodium source, a nickel source and a manganese source in deionized water to form a mixed solution; vigorously stirring the mixed solution, and adding a complexing agent to the mixed solution during the violent stirring process, and keeping the pH value of the mixed solution at 8-9; evaporating and concentrating the mixed solution after adding the complexing agent to obtain a gel, and drying the gel; pre-calcining the dried gel at a first temperature and keeping it warm for a first time period, and then calcining it at a second temperature and keeping it warm for a second time period to obtain a final positive electrode material.

[0005] It can be seen that the current method of preparing sodium battery materials requires mixing the fiber precursor and the positive or negative electrode raw materials and then using electrospinning for preparation, which results in low production efficiency, low content of positive electrode active substances, and inability to monitor the fiber filaments formed by the electrospinning machine in real time. It is impossible to make timely adjustments based on the monitoring results and cannot guarantee the quality of the fiber. Summary of the invention

[0006] To this end, the present invention provides a method for preparing sodium battery materials, which is used to overcome the problems in the prior art of mixing a fiber precursor and a positive electrode or a negative electrode raw material and then preparing the material by electrospinning, such as low production efficiency, low content of positive electrode active substances, inability to monitor the fiber filaments formed by the electrospinning machine in real time, inability to make timely adjustments based on the monitoring results, and inability to ensure the quality of the fiber.

[0007] To achieve the above object, the present invention provides a method for preparing a sodium battery material, comprising:

[0008] Step S1, selecting a polymer carbon source and one or more organic solvents and uniformly dispersing them in a set ratio to form an electrospinning precursor solution;

[0009] Step S2, the formed precursor solution is sprayed out in the form of a spray through a spray unit in the electrospinning machine, and the sprayed spray forms fiber filaments under the action of an electric field generating unit;

[0010] Step S3, real-time monitoring of the fiber filaments formed in step S2 is performed by a spinning monitoring unit, and a spinning determination unit analyzes the anisotropy inside a single fiber filament, the uniformity of a single fiber thickness, and the overall uniformity of all fiber filaments according to the monitoring results;

[0011] Step S4, timely adjustment or alarm is made according to the analysis results to obtain precursor materials that meet the requirements;

[0012] Step S5, determining various raw materials required for sodium battery materials, weighing various raw materials according to chemical proportions and uniformly mixing them with precursor materials in a certain proportion to form a mixture;

[0013] Step S6, drying and high-temperature treating the formed mixture to obtain sodium battery material.

[0014] Furthermore, based on the action of the electric field generating unit, the electrospinning machine sprays the precursor liquid in the form of a spray through the spray unit to form fiber filaments;

[0015] The spinning determination unit determines the rotation speed of the first rotating unit at each monitoring time according to the anisotropy inside the single fiber filament obtained at different monitoring times at a plurality of monitoring points;

[0016] Based on the single thickness standard uniformity evaluation interval set in the spinning determination unit, determine whether each nozzle is blocked according to the single thickness uniformity of the single fiber filament at each monitoring point, or determine the spinning distance between the nozzle and the receiving unit;

[0017] Based on the overall uniformity calculated from the single thickness uniformity of each monitoring point, the electric field strength of the electric field generating unit is determined, or an alarm is issued;

[0018] The obtained precursor material is mixed with other sodium battery raw materials to form a mixture which is dried and subjected to high temperature treatment to obtain a sodium battery material;

[0019] The first rotating unit can drive the first electrode plate and the second electrode plate in the electric field generating unit to rotate;

[0020] The receiving unit is capable of collecting the formed fiber filaments.

[0021] Furthermore, the spinning determination unit is provided with a period monitoring duration.

[0022] The spinning monitoring unit obtains the actual thickness value of a single fiber filament at each monitoring moment according to the periodic monitoring duration.

[0023] The spinning determination unit determines whether the anisotropy inside the single fiber filament meets the standard according to the actual thickness value combined with the set standard thickness value, or sends an adjustment signal.

[0024] After each monitoring period, the spinning determination unit collects the actual thickness value monitored by the spinning monitoring unit in real time, and calculates the collected data with the set standard thickness value to determine whether the actual thickness value of the fiber filament at this moment meets the standard. If it does not meet the standard, the spinning determination unit sends an adjustment signal.

[0025] The adjustment signal includes a first adjustment signal and a second adjustment signal.

[0026] Furthermore, a first difference evaluation value is provided in the spinning determination unit, and the selection of the adjustment signal is related to the anisotropic state inside the single fiber filament, including that the absolute value of the first difference is greater than the first difference evaluation value and the actual thickness value is less than the standard thickness value, and the spinning determination unit sends the first adjustment signal,

[0027] The absolute value of the first difference is greater than the first difference evaluation value and the actual thickness value is greater than the standard thickness value, and the spinning determination unit sends the second adjustment signal;

[0028] The first absolute value of the difference is the absolute value of the difference between the actual thickness value and the standard thickness value.

[0029] Further, the first rotation auxiliary unit can determine the actual rotation speed of the first rotation unit according to the adjustment signal sent by the spinning determination unit in combination with the initial rotation speed of the first rotation unit;

[0030] The spinning determination unit is set with a first calculation adjustment parameter and a second calculation adjustment parameter. When the spinning determination unit sends out the first adjustment signal, the initial rotational speed of the first rotating unit is obtained, and the spinning determination unit corrects the initial rotational speed according to the first calculation parameter to obtain the actual rotational speed; when the spinning determination unit sends out the second adjustment signal, the initial rotational speed of the first rotating unit is obtained, and the spinning determination unit corrects the initial rotational speed according to the second calculation parameter to obtain the actual rotational speed.

[0031] Furthermore, the monitored fiber filaments are divided into a number of monitoring points according to the different nozzles.

[0032] The spinning determination unit determines the working state of the electrospinning machine or issues an alarm by determining the thickness uniformity of the single strip at each monitoring point and the overall uniformity obtained after integration one by one;

[0033] The monitored fiber filaments are divided into several monitoring points according to the different nozzles, and different single thickness standard uniformity evaluation intervals are set for different monitoring points. The uniformity comparison is performed based on the single thickness uniformity obtained at each monitoring point and the single thickness standard uniformity evaluation interval. The uniformity comparison includes the single filament thickness uniformity comparison and the overall thickness uniformity comparison.

[0034] Further, the spinning determination unit can determine the blockage of the nozzle according to the calculated single thickness uniformity combined with the set single thickness standard uniformity evaluation interval, or determine the actual spinning distance;

[0035] If the single-strand thickness uniformity is less than the single-strand thickness standard uniformity evaluation interval, the spinning determination unit determines that the nozzle is blocked and sends out an alarm signal; if the single-strand thickness uniformity is greater than the single-strand thickness standard uniformity evaluation interval, the spinning determination unit sends out a third adjustment signal to correct the initial spinning distance obtained to obtain the actual spinning distance.

[0036] Furthermore, the spinning determination unit is provided with an overall uniformity evaluation value and an alarm threshold.

[0037] The spinning determination unit can determine the overall uniformity according to the thickness uniformity of each single strand, and determine the electric field strength of the electric field generating unit according to the overall uniformity combined with the overall uniformity evaluation value and the alarm threshold, and determine whether the viscosity of the precursor solution is appropriate;

[0038] If it is determined that the overall uniformity is greater than or equal to the alarm threshold and less than or equal to the overall uniformity evaluation value, the spinning determination unit sends a fourth adjustment signal to correct the initial electric field strength of the electric field generating unit; if it is determined that the overall uniformity is less than the alarm threshold, the spinning determination unit sends an alarm signal and determines that the viscosity of the precursor liquid is inappropriate.

[0039] Furthermore, the standard mixing ratio of the remaining sodium battery raw materials to the precursor material is in the range of 60:40-99:1.

[0040] Among them, the preferred mixing ratio of the remaining sodium battery raw materials and the precursor materials is 95:5.

[0041] Furthermore, there are several mixing methods between the remaining sodium battery raw materials and the precursor material, including sol-gel method, co-precipitation method and solid phase mixing.

[0042] Furthermore, the mixture is dried to remove the solvent, which may include several drying methods: baking, freeze drying and spray drying.

[0043] Wherein, nitrogen or argon can be used for protection or vacuum drying during the drying process.

[0044] Compared with the prior art, the beneficial effect of the present invention lies in that, when judging the fiber quality of the electrospinning machine, different monitoring points are set for fiber filaments formed by spraying precursor liquid droplets from different nozzles to monitor, and the data obtained at different monitoring times at each monitoring point are sorted and summarized, so as to comprehensively analyze the anisotropy inside a single fiber filament and the thickness uniformity of a single fiber filament, so as to more accurately and scientifically judge whether it is necessary to adjust the speed of the first rotating unit; for different monitoring points, different single thickness standard uniformity evaluation intervals are set, so as to better determine the fiber formation situation of each monitoring point, through By analyzing the fiber quality at each monitoring point, determining the blockage status of each nozzle and whether the spinning distance is appropriate, and adjusting the spinning distance in time, it is avoided that the fibers are too thin due to the blockage of the nozzle cannot be discovered in time or the fibers are too thick due to the spinning distance being too close, and the fiber thickness uniformity is improved. The overall uniformity is determined based on the single thickness uniformity obtained at each monitoring point, and the overall uniformity is analyzed to determine whether the overall fiber filaments meet the requirements. If not, the electric field strength of the electric field generating unit can be adjusted in time or an alarm can be issued in time to adjust the viscosity of the precursor liquid to ensure the fiber quality.

[0045] In particular, by monitoring the fiber filaments ejected from different nozzles and compiling and summarizing the data obtained from each monitoring point, the anisotropy of the force on each fiber filament can be more accurately reflected, making it more balanced, and the uniformity of the fiber filament thickness can be analyzed as a whole, the fiber quality of the electrospinning machine can be judged, and whether corresponding adjustments are needed can be determined more accurately and scientifically.

[0046] In particular, setting different first difference evaluation values ​​for different monitoring points can better determine whether the thickness of the fiber filaments at each monitoring point is uniform. By analyzing the thickness status of the fiber filaments at different times at each monitoring point, it can prevent the uneven thickness of single fiber filaments due to the anisotropy inside the fiber filaments. This provides data support for reducing the anisotropy inside single fiber filaments during the spinning process and improving the uniformity of the fiber filament thickness, thereby ensuring the quality of fiber formation.

[0047] In particular, the data of different thin and thick moments of a single fiber filament are sorted and summarized, and a single thickness standard uniformity evaluation range is set. By judging the thickness uniformity of a single fiber filament as a whole, data support is provided for determining whether it meets the standards and making corresponding adjustments, thereby ensuring the quality of fiber formation.

[0048] In particular, the actual thickness values ​​of single fiber filaments at different times during the spinning process are summarized to calculate the thickness uniformity of the single fiber filament, and the single thickness uniformity is compared with the preset single thickness standard uniformity evaluation interval to determine whether each nozzle is blocked or whether the spinning distance is adjusted. This avoids fibers that are too thin due to the failure to detect nozzle blockage in time or fibers that are too thick due to too close spinning distance, improves the fiber thickness uniformity, and ensures the fiber quality.

[0049] In particular, polyvinyl pyrrolidone and N, N-dimethylacetamide are uniformly dispersed in a set ratio to form a second type of precursor solution for electrospinning, and the second type of precursor solution is subjected to electrospinning to obtain a second type of precursor material; vanadium pentoxide, dihydrated oxalic acid, sodium carbonate, diammonium phosphate, and molybdenum trioxide are weighed according to a chemical ratio, added to deionized water, and stirred to form a uniform solution, and a coprecipitation method is used to form a second type of precursor, and then the obtained solution is freeze-dried and pretreated at 350°C for 4 hours under a N2 atmosphere, and finally treated at 800°C for 10 hours under a N2 atmosphere to obtain Na2.94 V1.98Mo0.02(PO4)3, this preparation method does not require repeated high-temperature treatment, which can effectively save energy. It is not necessary to mix the fiber precursor and the positive or negative electrode raw materials before electrospinning, thereby effectively improving the production efficiency and the content of positive electrode active substances. The electrospinning precursor will release a certain amount of gas at high temperature, which can prevent the agglomeration of the positive electrode material; by coating the surface of the positive electrode material with carbon fiber, the conductivity of the material can be effectively improved; this method can form a uniform conductive network, and there is no need to add carbon nanotubes or carbon fibers when formulating the positive electrode material. BRIEF DESCRIPTION OF THE DRAWINGS

[0050] Figure 1 A flow chart of a method for preparing sodium battery materials;

[0051] Figure 2 is a structural diagram of an electrospinning machine;

[0052] Figure 3 It is a logic diagram for comparing the thickness uniformity of a single filament;

[0053] Figure 4 This is a logic diagram for comparing the overall thickness and uniformity;

[0054] The figure includes: an injection unit 1, a nozzle 2, a receiving unit 3, a first electrode plate 4, a second electrode plate 5, a first rotating unit 6, a spinning monitoring unit 7, and a first rotating auxiliary unit 8. DETAILED DESCRIPTION

[0055] In order to make the objects and advantages of the present invention more clearly understood, the present invention is further described below in conjunction with embodiments; it should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.

[0056] The preferred embodiments of the present invention are described below with reference to the accompanying drawings. It should be understood by those skilled in the art that these embodiments are only used to explain the technical principles of the present invention and are not intended to limit the protection scope of the present invention.

[0057] It should be noted that, in the description of the present invention, terms such as "up", "down", "left", "right", "inside" and "outside" indicating directions or positional relationships are based on the directions or positional relationships shown in the drawings. This is merely for the convenience of description and does not indicate or imply that the device or element must have a specific orientation, be constructed and operated in a specific orientation. Therefore, it cannot be understood as a limitation on the present invention.

[0058] In addition, it should be noted that in the description of the present invention, unless otherwise clearly specified and limited, the terms "installed", "connected", and "connected" should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection, or it can be indirectly connected through an intermediate medium, or it can be the internal communication of two components. For those skilled in the art, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.

[0059] See also Figure 1-Figure 4 As shown, Figure 1 A flow chart of a method for preparing sodium battery materials; Figure 2 is a structural diagram of an electrospinning machine; Figure 3 It is a logic diagram for comparing the thickness uniformity of a single filament; Figure 4 This is a logical diagram for comparing the overall thickness uniformity.

[0060] The present invention provides a method for preparing a sodium battery material, comprising:

[0061] Step S1, selecting a polymer carbon source and one or more organic solvents and uniformly dispersing them in a set ratio to form an electrospinning precursor solution;

[0062] Step S2, electrospinning the formed precursor solution through an electrospinning machine to obtain a precursor material;

[0063] Step S3, determining various raw materials required for sodium battery materials, weighing various raw materials according to chemical proportions and uniformly mixing them with precursor materials in a certain proportion to form a mixture;

[0064] Step S4, drying and high-temperature treating the formed mixture to obtain sodium battery material.

[0065] Specifically, the polymer carbon source in step S1 of this embodiment includes polyacrylonitrile, polyvinylidene fluoride, polyvinyl pyrrolidone, polypropylene alcohol and polymethyl acrylate;

[0066] The organic solvent includes water, N,N-dimethylformamide, N,N-dimethylacetamide, ethanol, acetonitrile, isopropanol and acetone.

[0067] Specifically, the sodium battery raw material in this embodiment is a polyanion compound or an ion doping or hybridization of the polyanion compound material;

[0068] The polyanion compound includes sodium dihydrogen phosphate dihydrate, ammonium metavanadate, oxalic acid dihydrate, vanadium pentoxide, oxalic acid dihydrate, sodium carbonate, ammonium dihydrogen phosphate, molybdenum trioxide, sodium hydroxide, sodium fluoride, ferrous phosphate, phosphoric acid and ascorbic acid.

[0069] Specifically, in step S3 of this embodiment, the standard range of the mixing ratio of the raw material to the precursor material is 60:40-99:1, wherein the preferred mixing ratio of the raw material to the precursor material is 95:5.

[0070] Specifically, there are several mixing methods between the raw materials and the precursor materials in this embodiment, including sol-gel method, co-precipitation method and solid phase mixing.

[0071] Specifically, in this embodiment, the mixture is dried to remove the solvent, including several drying methods: baking, freeze drying and spray drying.

[0072] Wherein, nitrogen or argon can be used for protection or vacuum drying during the drying process.

[0073] Specifically, in this embodiment, the dried mixture is subjected to high-temperature synthesis at a specific temperature, and vacuum, nitrogen, argon or other inert gases may be used for protection during the synthesis process.

[0074] Specifically, in this embodiment, different polymer carbon sources and different organic solvents are selected to form different precursor solutions, including a first type of precursor solution, a second type of precursor solution, and a third type of precursor solution.

[0075] The first type of precursor solution comprises the polyacrylonitrile selected from the high molecular polymer carbon source, the N,N-dimethylformamide selected from the organic solvent, and the polyacrylonitrile and the N,N-dimethylformamide are uniformly dispersed in a set ratio to form a first type of precursor solution for electrostatic spinning, and the first type of precursor solution is electrostatically spun to obtain a first type of precursor material;

[0076] The second type of precursor solution uses the polyvinyl pyrrolidone in the high molecular polymer carbon source and the N, N-dimethylacetamide in the organic solvent, and the polyvinyl pyrrolidone and N, N-dimethylacetamide are evenly dispersed according to a set ratio to form the second type of precursor solution for electrospinning, and the second type of precursor solution is electrospun to obtain the second type of precursor material;

[0077] The three types of precursor solutions are selected from the polypropylene alcohol in the high molecular polymer carbon source and the acetone in the organic solvent, and the polypropylene alcohol and acetone are evenly dispersed in a set ratio to form three types of precursor solutions for electrospinning, and the three types of precursor solutions are electrospun to obtain three types of precursor materials.

[0078] Specifically, in this embodiment, different experiments are set according to the different selected precursor solutions, different raw materials, different mixing methods, different drying methods and different gas atmospheres for protection, including Example 1, Example 2 and Example 3.

[0079] In the embodiment 1, the sodium dihydrogen phosphate dihydrate is weighed according to the chemical ratio, the ammonium metavanadate and the oxalic acid dihydrate are mixed with the first type of precursor material in deionized water at a mixing ratio of 95:5, and the first type of precursor is formed by the sol-gel method. The prepared first type of precursor is dried under the protection of a nitrogen atmosphere and solid-phase sintered at a corresponding temperature to obtain Na3V2(P04)3 / C composite nanofibers;

[0080] In the embodiment 2, vanadium pentoxide, dihydrated oxalic acid, sodium carbonate, ammonium dihydrogen phosphate, molybdenum trioxide and the two types of precursor materials are weighed according to the chemical ratio, added to deionized water and stirred to form a uniform solution, and then the obtained solution is freeze-dried and pre-treated at 350°C for 4h under N2 atmosphere. Finally, Na2.94V1.98Mo0.02(PO4)3 is obtained by treating it at 800°C for 10h under N2 atmosphere;

[0081] In the embodiment 3, sodium hydroxide, sodium fluoride, ferrous phosphate, phosphoric acid and a small amount of ascorbic acid are weighed according to chemical proportions, added to a mixed solution of deionized water and ethylene glycol in turn and stirred until completely dissolved, and then mixed evenly with the three types of precursor materials in a ratio of 85:15, and the pH value is adjusted to about 10 with a dilute NaOH aqueous solution; the mixed solution is placed in a constant temperature drying oven and reacted at 160°C for 12 hours, the obtained reactant is repeatedly washed and dried again, and then calcined at 600°C under the protection of high-purity argon and kept warm for 6 hours to obtain Na2FePO4F / C composite nanofibers.

[0082] Specifically, when determining the content of the positive electrode active material in the prepared sodium battery material in this embodiment, a first simulation group is provided, including the embodiment 1 and the comparative example 1,

[0083] Among them, the comparative example 1 weighs sodium dihydrogen phosphate dihydrate, ammonium metavanadate, and oxalic acid dihydrate according to the chemical proportion, and forms a precursor by a sol-gel method. The prepared precursor is dried under the protection of a nitrogen atmosphere and solid-phase sintered at a corresponding temperature to obtain Na3V2(P04)3.

[0084] Specifically, in this embodiment, the morphologies of the Na3V2(P04)3 / C composite nanofibers and the Na3V2(P04)3 are compared. The Na3V2(P04)3 / C composite nanofibers are coated on the surface of the Na3V2(P04)3 material. Compared with the Na3V2(P04)3 material formed in Comparative Example 1, the material is relatively dispersed without obvious agglomeration. It is judged that the fiber precursor and the positive or negative electrode raw materials are mixed and then prepared by electrospinning, resulting in low production efficiency and low content of positive electrode active substances.

[0085] Specifically, in this embodiment, the first sodium battery material prepared in Example 1, the second sodium battery material prepared in Example 2, the third sodium battery material prepared in Example 3, and the fourth sodium battery material prepared in Comparative Example 1 are respectively used as positive electrode materials, and the positive electrode materials, conductive carbon black, and polyvinylidene fluoride are respectively weighed at a mass ratio of 90:5:5. The weighed materials are mixed evenly with N-methylpyrrolidone and then coated on aluminum foil, and then dried and cut into the size required by the process; according to the mass ratio of 90:5:2 .5:2.5 ratio of hard carbon, conductive carbon black, sodium carboxymethyl cellulose, styrene-butadiene rubber are weighed respectively, the weighed materials are mixed evenly with deionized water and coated on aluminum foil, and then dried and cut into the size required by the process, and the positive electrode sheet, separator and negative electrode sheet are made into battery cells according to the stacking process requirements, and prepared into soft-package sodium ion batteries through processes such as ear welding, aluminum-plastic film top and side sealing, liquid injection, sealing, standing, formation, vacuum sealing, and capacity division, including a first sodium ion battery, a second sodium ion battery, a third sodium ion battery and a fourth sodium ion battery.

[0086] Specifically, in this embodiment, each soft-package sodium ion battery prepared was subjected to a charge and discharge test at a current density of 1C to determine the capacity retention rate of each soft-package sodium ion battery, wherein the charge and discharge cut-off voltage was 2.0-4.0V (Na2FePO4F / C) or 1.5-3.8V (Na3V2(P04)3 / C), and the charge and discharge cycle curve was obtained as shown in FIG. Figure 3 shown.

[0087] It can be seen from the figure that the capacity retention rates of the embodiments are much higher than those of the comparative examples, and the capacity retention rate of the embodiment 2 is higher than that of the embodiments 1 and 3.

[0088] In this embodiment, polyvinyl pyrrolidone and N, N-dimethylacetamide are uniformly dispersed in a set ratio to form a second type of precursor solution for electrospinning, and the second type of precursor solution is subjected to electrospinning to obtain a second type of precursor material; vanadium pentoxide, dihydrated oxalic acid, sodium carbonate, ammonium dihydrogen phosphate, and molybdenum trioxide are weighed according to a chemical ratio, added to deionized water, and stirred to form a uniform solution, and a coprecipitation method is used to form a second type of precursor, and then the obtained solution is freeze-dried and pretreated at 350°C for 4h under a N2 atmosphere, and finally treated at 800°C for 10h under a N2 atmosphere to obtain Na2.94 V1.98Mo0.02(PO4)3, this preparation method does not require repeated high-temperature treatment, which can effectively save energy. It is not necessary to mix the fiber precursor and the positive or negative electrode raw materials before electrospinning, thereby effectively improving the production efficiency and the content of positive electrode active substances. The electrospinning precursor will release a certain amount of gas at high temperature, which can prevent the agglomeration of the positive electrode material; by coating the surface of the positive electrode material with carbon fiber, the conductivity of the material can be effectively improved; this method can form a uniform conductive network, and there is no need to add carbon nanotubes or carbon fibers when formulating the positive electrode material.

[0089] Specifically, the electrospinning machine in step S2 of this embodiment includes:

[0090] A spray unit 1, comprising a plurality of nozzles 2, for uniformly spraying the precursor liquid;

[0091] A receiving unit 3, which is used to collect the formed fiber filaments;

[0092] An electric field generating unit, comprising a first electrode plate 4 and a second electrode plate 5, wherein the first electrode plate 4 and the second electrode plate 5 are arranged on both sides of the central axis between the spraying unit 1 and the receiving unit 3, and are used to stretch the precursor liquid droplets sprayed by the spraying unit 1 to form fiber filaments;

[0093] A spinning monitoring unit 7, which is used to monitor the thickness uniformity of the formed fiber filaments in real time;

[0094] A first rotating unit 6, which is connected to the first electrode plate 4 and the second electrode plate 5, and is used to drive the first electrode plate 4 and the second electrode plate 5 to rotate along the central axis;

[0095] A first rotation auxiliary unit 8, which is used to adjust the rotation speed of the first rotation unit 6;

[0096] The spinning determination unit is connected to the injection unit 1, the receiving unit 3, the electric field generating unit, the spinning monitoring unit 7 and the first rotation auxiliary unit 8 respectively. By setting different monitoring points, the data obtained at different monitoring times at each monitoring point are sorted and summarized, and the anisotropy inside the single fiber filament and the thickness uniformity of the single fiber filament are analyzed as a whole to determine whether it is necessary to send an adjustment signal to the first rotation auxiliary unit 8. For different monitoring points, different single thickness standard uniformity evaluation intervals are set to determine the single thickness uniformity of each monitoring point, determine the blockage of each nozzle 2 and whether the spinning distance is appropriate and make timely adjustments, determine the overall uniformity based on the single thickness uniformity of each monitoring point, analyze the overall uniformity, and determine whether the overall fiber filament meets the requirements. If it does not meet the requirements, adjust the electric field strength of the electric field generating unit in time or give an alarm in time.

[0097] Specifically, the injection unit 1 in this embodiment is provided with a plurality of nozzles 2, and different monitoring points are provided for the fiber filaments formed by the precursor liquid droplets ejected from different nozzles 2, including a first monitoring point, a second monitoring point, ..., an nth monitoring point. For any monitoring point, the spinning determination unit is provided with a single thickness standard uniformity evaluation interval for it. The spinning determination unit determines whether corresponding adjustment or alarm is needed based on the relationship between the single thickness uniformity of the fiber filaments obtained at each monitoring point and the single thickness standard uniformity evaluation interval. In the process of determination, it is necessary to compare the thickness uniformity of the single filament and the overall thickness uniformity.

[0098] By monitoring the fiber filaments ejected from different nozzles and summarizing the data obtained from each monitoring point, the anisotropy of the force on each fiber filament can be more accurately reflected, making it more balanced, and the uniformity of the fiber filament thickness can be analyzed as a whole, the fiber quality of the electrospinning machine can be judged, and it can be determined more accurately and scientifically whether corresponding adjustments are needed.

[0099] Specifically, in this embodiment, for the i-th monitoring point Ai, the spinning determination unit is provided with a monitoring cycle t. After each monitoring cycle t, the spinning monitoring unit performs real-time monitoring of the actual thickness value Ci of the fiber filament at the i-th monitoring point Ai at that moment, i=1, 2, ...n, the spinning determination unit calculates the obtained actual thickness value Ci and the standard thickness value C0 set in the spinning determination unit to obtain the first difference absolute value Si between the actual thickness value Ci and the standard thickness value C0, Si=|Ci-C0|,

[0100] If Si≤S0i, it is determined that the thickness of the fiber filaments at that moment meets the standard;

[0101] If Si>S0i, and Ci<C0, it is determined that the thickness of the fiber filament at this moment does not meet the standard and is too thin, and the spinning determination unit sends a first adjustment signal;

[0102] If Si>S0i, and Ci>C0, it is determined that the thickness of the fiber filament at this moment does not meet the standard and is too thick, and the spinning determination unit sends a second adjustment signal;

[0103] Among them, S0i is the first difference evaluation value of the fiber filament corresponding to the i-th monitoring point Ai set in the spinning determination unit, and the value of the first difference evaluation value is different according to the different positions of the nozzle 2.

[0104] For different monitoring points, different first difference evaluation values ​​are set, which can better determine whether the thickness of the fiber filaments at each monitoring point is uniform. By analyzing the thickness status of the fiber filaments at different times at each monitoring point, the uneven thickness of single fiber filaments caused by the anisotropy inside the fiber filaments can be prevented. This provides data support for reducing the anisotropy inside single fiber filaments during the spinning process and improving the uniformity of the fiber filament thickness, thereby ensuring the quality of fiber formation.

[0105] Specifically, in this embodiment, the first rotating unit 6 drives the first electrode plate 4 and the second electrode plate 5 to rotate along the central axis at an initial rotation speed V0. When Si>S0i, the first rotation auxiliary unit adjusts the initial rotation speed V0 according to the actual thickness value Ci and the standard thickness value C0.

[0106] If Ci<C0, the first rotation auxiliary unit reduces the initial rotation speed V0 to obtain an actual rotation speed V1, V1=[1-(C0-Ci)×a]×V0,

[0107] If Ci>C0, the first rotation auxiliary unit increases the initial rotation speed V0 to obtain an actual rotation speed V1, V1=[1+(Ci-C0)×b]×V0,

[0108] Wherein, a is a first calculation adjustment parameter of the difference between the standard thickness value C0 and the actual thickness value Ci for the actual rotation speed V1;

[0109] b is a second calculation adjustment parameter of the difference between the actual coarseness value Ci and the standard coarseness value C0 for the actual rotation speed V1.

[0110] Specifically, the spinning determination unit in this embodiment integrates the actual thickness values ​​of the fiber filaments at the i-th monitoring point Ai at different times, obtains the number of monitoring moments when the thickness values ​​of the fiber filaments do not meet the standard and are too thin, and calculates the first score, obtains the number of monitoring moments when the thickness values ​​of the fiber filaments do not meet the standard and are too thick, and calculates the second score, including:

[0111] 1) Number the number of fine monitoring moments, record them as the first fine moment A11, the second fine moment A12...the mth fine moment A1m,

[0112] 2) Number the coarse monitoring moments, record them as the first coarse moment A21, the second coarse moment A22, ... the kth coarse moment A2k,

[0113] Determine the thickness uniformity Di of a single fiber filament at the i-th monitoring point Ai, and set

[0114]

[0115] Wherein, Si2y is the coarse difference value at the yth coarse moment, Ey is the first calculation compensation parameter of the coarse actual value Si2y at the yth coarse moment for the single thickness uniformity Di; Si 1x is the fine difference value at the xth fine moment, Gx is the second calculation compensation parameter of the fine difference value Si 1x at the xth fine moment for the single thickness uniformity Di, and the values ​​of the first calculation compensation parameter Ey and the second calculation compensation parameter Gx are different according to the different nozzle positions;

[0116] If Doimin≤Di≤D0imax, it is determined that the thickness uniformity of a single fiber filament at the i-th monitoring point Ai meets the standard.

[0117] If Di<D0imin, the thickness uniformity of the single fiber filament at the i-th monitoring point Ai does not meet the standard, and the spinning determination unit sends an alarm signal to determine that the nozzle 2 is blocked;

[0118] If Di>D0imax, it is determined that the thickness uniformity of the single fiber filament at the i-th monitoring point Ai does not meet the standard, and the spinning determination unit sends a third adjustment signal;

[0119] Wherein, a single thickness standard uniformity evaluation interval [D0imin, D0imax] is provided in the spinning determination unit;

[0120] D0imin is the minimum evaluation value of the uniformity of the single thickness standard set in the spinning determination unit;

[0121] D0imax is the maximum evaluation value of the uniformity of the single thickness standard set in the spinning determination unit.

[0122] The data of different thin and thick moments of a single fiber filament are sorted and summarized, and a single thickness standard uniformity evaluation range is set. The thickness uniformity of a single fiber filament is judged as a whole, providing data support for judging whether it meets the standard and making corresponding adjustments, thereby ensuring the quality of fiber formation.

[0123] Specifically, in this embodiment, the initial spinning distance between the nozzle corresponding to the i-th monitoring point Ai and the receiving unit 3 is L0. When Di>D0imax, the spinning determination unit adjusts the initial spinning distance L0 to obtain an actual spinning distance Li that meets the single thickness standard uniformity evaluation interval.

[0124] Li=[1+(Di-D0imax)×h]×L0,

[0125] Among them, h is the third calculation adjustment parameter for the actual spinning distance Li based on the difference between the single thickness uniformity Di and the single thickness standard uniformity maximum evaluation value Doimax.

[0126] In this embodiment, the actual thickness values ​​of single fiber filaments at different times during the spinning process are summarized to calculate the thickness uniformity of the single fiber filament, and the single thickness uniformity is compared with the preset single thickness standard uniformity evaluation interval to determine whether each nozzle is blocked or whether the spinning distance is adjusted. This avoids fibers that are too thin due to the failure to detect nozzle blockage in time or fibers that are too thick due to too close spinning distance, improves the fiber thickness uniformity, and ensures the fiber quality.

[0127] Specifically, in this embodiment, the overall uniformity Z is determined based on the single thickness uniformity. During the determination process, the single thickness uniformity of the fiber filaments at each monitoring point is summarized;

[0128]

[0129] If Z>Z0, it is determined that the overall uniformity Z meets the requirements.

[0130] If Z0min≤Z≤Z0, it is determined that the overall uniformity Z does not meet the requirements, the spinning determination unit sends a fourth adjustment signal, and the electric field generating unit adjusts its initial electric field strength;

[0131] If Z<Z0min, it is determined that the overall uniformity Z does not meet the requirements and the number of blockages of the nozzles 2 in the injection unit is too large, and the viscosity of the precursor liquid is determined to be inappropriate, and the spinning determination unit sends an alarm signal;

[0132] Among them, Z0 is the overall uniformity evaluation value set in the spinning determination unit, and its value varies according to the type of the precursor liquid. Z0min is the alarm threshold set in the spinning determination unit; j represents the number of monitoring points; and i represents the i-th monitoring point.

[0133] When judging the fiber quality of the electrospinning machine, the present invention monitors different monitoring points set for fiber filaments formed by spraying precursor liquid droplets from different nozzles, and summarizes the data obtained at different monitoring times at each monitoring point, comprehensively analyzes the anisotropy inside a single fiber filament and the thickness uniformity of a single fiber filament, and more accurately and scientifically determines whether it is necessary to adjust the speed of the first rotating unit; for different monitoring points, different single thickness standard uniformity evaluation intervals are set, which can better determine the fiber formation situation of each monitoring point, and by evaluating each monitoring point The fiber quality is analyzed to determine the blockage status of each nozzle and whether the spinning distance is appropriate, and the spinning distance is adjusted in time to avoid fibers that are too thin due to nozzle blockage that cannot be discovered in time or fibers that are too thick due to spinning distance that is too close, thereby improving the uniformity of fiber thickness. The overall uniformity is determined based on the single thickness uniformity obtained at each monitoring point, and the overall uniformity is analyzed to determine whether the overall fiber filaments meet the requirements. If not, the electric field strength of the electric field generating unit can be adjusted in time or an alarm can be issued in time to adjust the viscosity of the precursor liquid to ensure the fiber quality.

[0134] The calculation compensation parameters and the calculation adjustment parameters described in the present invention have two functions: one is to balance the left and right dimensions of the formula, and the other is to adjust the numerical results. No specific assignment is performed in this embodiment. In addition, the calculation formulas in this embodiment are used to intuitively reflect the adjustment relationship between the various numerical values, such as positive correlation and negative correlation. Unless otherwise specified, the parameter values ​​that are not specifically limited to numerical values ​​are all positive.

[0135] So far, the technical solutions of the present invention have been described in conjunction with the preferred embodiments shown in the accompanying drawings. However, it is easy for those skilled in the art to understand that the protection scope of the present invention is obviously not limited to these specific embodiments. Without departing from the principle of the present invention, those skilled in the art can make equivalent changes or substitutions to the relevant technical features, and the technical solutions after these changes or substitutions will fall within the protection scope of the present invention.

[0136] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A method for preparing sodium battery materials, characterized in that: include, Polyvinyl pyrrolidone and N, N-dimethylacetamide are uniformly dispersed in a set ratio to form a precursor solution for electrospinning, and the precursor solution is subjected to electrospinning to obtain a precursor material; vanadium pentoxide, dihydrated oxalic acid, sodium carbonate, ammonium dihydrogen phosphate, and molybdenum trioxide are weighed according to a chemical ratio and added to deionized water and stirred to form a uniform solution, a precursor is formed by a coprecipitation method, and then the obtained solution is freeze-dried and pretreated at 350°C for 4h under a N2 atmosphere, and finally treated at 800°C for 10h under a N2 atmosphere to obtain Na 2.94 V 1.98 Mo 0.02 (PO4)3; Based on the action of the electric field generating unit, the electrospinning machine sprays the precursor liquid in the form of a spray through the spray unit to form fiber filaments; The spinning determination unit determines the rotation speed of the first rotating unit at each monitoring time according to the anisotropy inside the single fiber filament obtained at different monitoring times at a plurality of monitoring points; Based on the single thickness standard uniformity evaluation interval set in the spinning determination unit, determine whether each nozzle is blocked according to the single thickness uniformity of the single fiber filament at each monitoring point, or determine the spinning distance between the nozzle and the receiving unit; The overall uniformity is calculated based on the obtained single thickness uniformity of each monitoring point, and whether to adjust the electric field strength of the electric field generating unit is determined according to the value of the overall uniformity: If Z>Z0, it is determined that the overall uniformity Z meets the requirement, and the electric field strength of the electric field generating unit is not adjusted; If Z0min≤Z≤Z0, it is determined that the overall uniformity Z does not meet the requirements, the spinning determination unit sends a fourth adjustment signal, and the electric field generating unit adjusts its initial electric field strength; If Z<Z0min, it is determined that the overall uniformity Z does not meet the requirements and the number of nozzles in the injection unit that are blocked is too large, and the viscosity of the precursor liquid is determined to be inappropriate, and the spinning determination unit sends an alarm signal; Wherein, Z0 is the overall uniformity evaluation value set in the spinning determination unit, and its value varies according to the type of the precursor solution, and Z0min is the alarm threshold set in the spinning determination unit; The obtained precursor material is mixed with other sodium battery raw materials to form a mixture which is dried and subjected to high temperature treatment to obtain a sodium battery material; The first rotating unit can drive the first electrode plate and the second electrode plate in the electric field generating unit to rotate; The receiving unit is capable of collecting the formed fiber filaments; The spinning determination unit is provided with a period monitoring duration. The spinning monitoring unit obtains the actual thickness value of a single fiber filament at each monitoring moment according to the periodic monitoring duration. The spinning determination unit determines whether the anisotropy inside the single fiber filament meets the standard according to the actual thickness value combined with the set standard thickness value, or sends an adjustment signal. Wherein, the adjustment signal includes a first adjustment signal and a second adjustment signal; The spinning determination unit is provided with a first difference evaluation value, and the selection of the adjustment signal is related to the anisotropic state inside the single fiber filament, including that if the absolute value of the first difference is greater than the first difference evaluation value and the actual thickness value is less than the standard thickness value, it is determined that the thickness value of the single fiber filament does not meet the standard and is too thin, and the spinning determination unit sends the first adjustment signal, If the absolute value of the first difference is greater than the first difference evaluation value and the actual thickness value is greater than the standard thickness value, it is determined that the thickness value of the single fiber filament does not meet the standard and is too thick, and the spinning determination unit sends the second adjustment signal; Wherein, the first difference absolute value is the absolute value of the difference between the actual thickness value and the standard thickness value; The first rotation auxiliary unit can determine the actual rotation speed of the first rotation unit according to the adjustment signal sent by the spinning determination unit and the initial rotation speed of the first rotation unit; The first rotation auxiliary unit reduces the initial rotation speed V0 according to the first adjustment signal to obtain an actual rotation speed V1. V1=[1-(C0-Ci)×a]×V0, The first rotation auxiliary unit increases the initial rotation speed V0 according to the second adjustment signal to obtain an actual rotation speed V1. V1=[1+(Ci-C0)×b]×V0, Wherein, a is a first calculation adjustment parameter of the difference between the standard thickness value C0 and the actual thickness value Ci for the actual rotation speed V1; b is a second calculation adjustment parameter of the difference between the actual thickness value Ci and the standard thickness value C0 for the actual rotation speed V1; The fiber filaments to be monitored are divided into several monitoring points according to the different nozzles. The actual thickness values ​​of the fiber filaments at different times at any monitoring point are integrated, the number of monitoring moments when the thickness values ​​of the fiber filaments do not meet the standard and are thin is obtained, and a first score is calculated. The number of monitoring moments when the thickness values ​​of the fiber filaments do not meet the standard and are thick is obtained and a second score is calculated. The single thickness uniformity Di of a single fiber filament at any monitoring point is calculated according to the first score and the second score, and set: Among them, Si2y is the coarseness difference value at the yth coarse moment, Ey is the coarseness actual value at the yth coarse moment, Si2y is the first calculated compensation parameter for the single thickness uniformity Di; Si 1x is the thinness difference value at the xth thin moment, Gx is the second calculated compensation parameter for the single thickness uniformity Di of the thinness difference value Si 1x at the xth thin moment, and the values ​​of the first calculated compensation parameter Ey and the second calculated compensation parameter Gx are different according to the nozzle position.

2. The method for preparing sodium battery material according to claim 1, characterized in that: The spinning determination unit can determine the blockage condition of the nozzle according to the calculated single thickness uniformity combined with the set single thickness standard uniformity evaluation interval, or determine the actual spinning distance; If Doimin≤Di≤D0imax, it is determined that the thickness uniformity of the single strip meets the standard. If Di<D0imin, the thickness uniformity of the single strand does not meet the standard, and the spinning determination unit sends an alarm signal to determine that the corresponding nozzle is blocked; If Di>D0imax, it is determined that the thickness uniformity of the single strand does not meet the standard, and the spinning determination unit sends a third adjustment signal; Wherein, a single thickness standard uniformity evaluation interval [D0imin, D0imax] is provided in the spinning determination unit; D0imin is the minimum evaluation value of the uniformity of the single thickness standard set in the spinning determination unit; Doimax is the maximum evaluation value of the uniformity of the single thickness standard set in the spinning determination unit; The spinning determination unit adjusts the initial spinning distance L0 according to the third adjustment signal to obtain an actual spinning distance Li that meets the single thickness standard uniformity evaluation interval, Li=[1+(Di-D0imax)×h]×L0, Among them, h is the third calculation adjustment parameter for the actual spinning distance Li based on the difference between the single thickness uniformity Di and the single thickness standard uniformity maximum evaluation value Doimax.

3. The method for preparing sodium battery material according to claim 2, characterized in that: The spinning determination unit can determine the overall uniformity according to the thickness uniformity of each single strand, and determine the electric field strength of the electric field generating unit according to the overall uniformity combined with the overall uniformity evaluation value and the alarm threshold, and determine whether the viscosity of the precursor solution is appropriate; The thickness uniformity of the single fiber filaments at each monitoring point is summarized to obtain the overall uniformity Z: Among them, j represents the number of monitoring points; i represents the i-th monitoring point.

4. The method for preparing sodium battery material according to claim 1, characterized in that: The mixing ratio of the remaining sodium battery raw materials to the precursor material is 60:40-99:

1.

5. The method for preparing sodium battery material according to claim 4, characterized in that: The mixing ratio of the remaining sodium battery raw materials to the precursor material is 95:

5.

6. The method for preparing sodium battery material according to claim 1, characterized in that: The remaining sodium battery raw materials are mixed with the precursor material by a sol-gel method, a coprecipitation method or a solid phase mixing.

7. The method for preparing sodium battery material according to claim 1, characterized in that: Drying the mixture to remove the solvent by baking, freeze drying or spray drying; In the drying process, nitrogen or argon is used for protection or vacuum drying.