Combined glaze suitable for laminated glaze and preparation method thereof
Through the laminated glaze structure, a combination of high-expansion and low-expansion glass powder is used to form a laminated glaze layer, which solves the problem of uneven impact resistance of a single glaze layer of semi-tempered glass on the photovoltaic backplane and achieves a glazed surface. Unification with smooth surface impact resistance and higher breakage resistance of glass.
Patent Information
- Application Number
- CN202310949788.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-06-30
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2042-06-30
AI Technical Summary
The single glaze layer of the existing 2.0mm semi-tempered glazed glass on the existing photovoltaic backplane has uneven impact resistance. The impact resistance of the glazed glaze strips and the non-glazed glaze strips on the smooth surface is poor, especially when the smooth surface is not The impact resistance of the glazed glaze strip is low and it is difficult to meet higher impact resistance requirements.
It adopts a laminated glaze structure. The bottom glaze contains high-expansion glass powder, and the surface glaze contains low-expansion glass powder and titanium dioxide. By forming a laminated glaze layer, the dry film thickness is controlled so that the overall average linear expansion coefficient is consistent with the photovoltaic backside. Plate glass is equivalent, eliminating stress unevenness and improving impact resistance.
The impact resistance of the glazed surface and the smooth non-glazed surface is consistent, and the ball drop height reaches 1.2m, which reduces the breakage rate of the glass, provides excellent static and dynamic onboard performance for large-format components, and solves the problem of outdoor installation. Strength issue.
Smart Images

Figure BDA0004367846600000081 
Figure BDA0004367846600000091
Abstract
Description
[0001] This application is a divisional application of the invention patent application with application date of June 30, 2022, application number 2022107689876, and invention name “A combination glaze suitable for laminated glaze, its preparation method and application”. Technical Field
[0002] The invention relates to the technical field of glazes and photovoltaic modules, and in particular to a method for preparing a composite glaze suitable for laminated glaze plating and the composite glaze prepared by the preparation method. Background Art
[0003] As a green energy, countries around the world are making the most of solar energy through technological development and innovation. my country has introduced a series of policies and regulations to promote the development of the solar energy industry, which has led to the rapid development of the solar photovoltaic industry. In terms of improving the efficiency of solar cell power generation, with the gradual improvement of technologies represented by double-sided PERC cells, the double-glass market has once again developed rapidly.
[0004] In order to effectively improve the power generation efficiency of double-glass photovoltaic modules, the photovoltaic backplane glass is used as the base, and a high-reflective glaze is silk-screened on the surface of the light-transmitting part where the battery cells are connected. After curing and tempering treatment, a high-reflective glaze layer is formed. The sunlight at the light-transmitting part where the battery cells are connected can be reflected back to the battery cells for use, thereby improving the output power of the photovoltaic module.
[0005] At present, the reflectivity SCI (550nm) of the high-reflective glaze layer of the photovoltaic backplane semi-tempered glazed glass can reach more than 80%. With the thinning of photovoltaic glass and the gradual popularization of 182 cells and 210 cells, 2.0mm wide panel semi-tempered glazed glass needs to meet higher impact resistance requirements. The breakage rate of this type of semi-tempered glass is higher than that of traditional 3.2mm semi-tempered glass.
[0006] At present, the 2.0 mm semi-tempered glazed glass of photovoltaic backplane uses a single glaze layer. The linear expansion coefficient of the glass powder of the glaze used is smaller than that of the 2.0 mm semi-tempered glass of photovoltaic backplane. The glaze layer is subjected to the compression given by the semi-tempered glass to produce compressive stress, and the compressive strength of the glaze layer is greater than the tensile strength (Wang Deqiang et al. Research Progress of Low Melting Point Glass for Glass Color Glaze [J]. Glass and Enamel, 2006, 034(004): 43-48.), so that the impact resistance of the glazed strip on the glazed surface is the same as that of the non-glazed strip on the glazed surface and the non-glazed strip on the smooth surface (non-glazed surface). The minimum value for not breaking a 227 g (diameter of about 38.1 mm) smooth steel ball falling on the glazed strip on the 2.0 mm semi-tempered glazed glass of photovoltaic backplane is 1.2 m. But in contrast, the glaze strip on the smooth surface (non-glazed surface) is stretched by the glaze layer to produce tensile stress, and the maximum impact resistance height of the falling ball here reaches 0.7m. Summary of the invention
[0007] In order to overcome the defects of the prior art solutions, the purpose of the present invention is to provide a method for preparing a combined glaze suitable for laminated glazing, by forming different glazes with water-soluble varnish and high-expansion glass powder or low-expansion glass powder respectively, and successively glazing the two different glazes on the 2.0mm glass surface of the photovoltaic backboard where the battery cells are connected and the light-transmitting part forms a laminated glaze layer, and the impact-resistant falling ball height at the glaze strip on the smooth surface (non-glazed surface) reaches 1.2m.
[0008] The present invention adopts the following technical solutions:
[0009] A composite glaze suitable for laminated glaze plating, comprising a bottom glaze and a surface glaze, wherein the bottom glaze comprises 30-40 parts of water-soluble varnish and 60-70 parts of high-expansion glass powder, and the surface glaze comprises 15-25 parts of water-soluble varnish, 35-45 parts of low-expansion glass powder and 40-50 parts of titanium dioxide; the average linear expansion coefficient of the high-expansion glass powder is greater than the average linear expansion coefficient of 2.0 mm semi-tempered glass of photovoltaic backboard, and the average linear expansion coefficient of 2.0 mm semi-tempered glass of photovoltaic backboard is greater than the average linear expansion coefficient of the low-expansion glass powder. The surface glaze is a high-reflection surface glaze, and its reflectivity SCI (550 nm) can reach more than 80%.
[0010] The photovoltaic back panel 2.0mm semi-tempered glass surface cell connection transparent part (i.e. the gap between adjacent cells) uses the combined glaze to form a laminated glaze layer, and the high-reflection laminated glaze layer includes a bottom glaze layer formed by the bottom glaze and a surface glaze layer formed by the surface glaze.
[0011] The surface glaze layer is compressed by the bottom glaze layer to produce compressive stress, and its compressive strength is greater than the tensile strength, so that the glaze strip on the glazed surface has the same impact resistance as the non-glazed strip on the glazed surface and the non-glazed strip on the smooth surface (non-glazed surface), and the ball falling height reaches 1.2m; by controlling the dry film thickness of the bottom glaze layer and the surface glaze layer, the overall average linear expansion coefficient of the laminated glaze layer is made equivalent to the average linear expansion coefficient of the 2.0mm semi-tempered glass of the photovoltaic backplane, eliminating the stress on the glaze strip on the smooth surface (non-glazed surface), making it have the same impact resistance as the glaze strip on the glazed surface, the non-glazed strip on the glazed surface, and the non-glazed strip on the smooth surface (non-glazed surface), and the ball falling height reaches 1.2m.
[0012] The combined glaze can be melted and sintered at a tempering temperature of 600-720° C. The titanium dioxide in the surface glaze is selected from one or more of Lomon Billions R-996, Chemours R-902+ and Chemours R-706.
[0013] According to some preferred embodiments of the present invention, the average linear expansion coefficient of the high expansion glass powder in the temperature range of 50-300°C is (95±5)×10 -7 / K; the average linear expansion coefficient of the low expansion glass powder in the temperature range of 50-300°C is (80±5)×10 -7 / K; the average linear expansion coefficient of 2.0mm semi-tempered glass of photovoltaic backplane in the temperature range of 50-300℃ is (87-88)×10 -7 / K.
[0014] According to some preferred embodiments of the present invention, the high expansion glass powder includes the following components, measured by mass: 40-45 parts of silicon dioxide, 15-25 parts of zinc oxide, 5-10 parts of bismuth oxide, 15-20 parts of boron oxide, 10-15 parts of sodium carbonate, 5-10 parts of titanium dioxide, and 1-5 parts of potassium carbonate.
[0015] According to some preferred embodiments of the present invention, the low expansion glass powder includes the following components, measured by mass: 40-60 parts of zinc oxide, 25-35 parts of silicon dioxide, 5-10 parts of aluminum oxide, 5-10 parts of titanium dioxide, 3-6 parts of zirconium dioxide, 2-3 parts of calcium oxide, 1-2 parts of potassium carbonate, 0.5-1 parts of phosphorus pentoxide, 0.5-1 parts of sodium hexafluorosilicate, and 0.1-0.5 parts of potassium chloride.
[0016] According to some preferred embodiments of the present invention, the particle size D of the high expansion glass powder and the low expansion glass powder is 50 The value is 1.5-2μm, D 97 The value is 3.5-4μm.
[0017] According to some preferred embodiments of the present invention, the water-soluble varnish component includes the following components, measured by mass: 30-40 parts of dipropylene glycol butyl ether, 15-25 parts of tripropylene glycol methyl ether, 15-25 parts of diethylene glycol butyl ether, 20-40 parts of water-soluble acrylic resin, 1-5 parts of polyethylene oxide, 1-5 parts of ethyl cellulose and 1-5 parts of aqueous dispersant.
[0018] The present invention provides a method for preparing the above-mentioned combined glaze, comprising the following steps:
[0019] Preparation of water-soluble varnish: mixing and stirring dipropylene glycol butyl ether, tripropylene glycol methyl ether, diethylene glycol butyl ether, water-soluble acrylic resin, polyethylene oxide and ethyl cellulose, heating, keeping warm to dissolve, adding aqueous dispersant, mixing evenly and cooling to room temperature to obtain water-soluble varnish;
[0020] Preparation of the bottom glaze: water-soluble varnish and high expansion glass powder are mixed and dispersed at high speed (1000-1200 rpm) until uniform, ground to a fineness of less than 20 μm by a three-roll grinder, and vibrated and filtered to obtain the bottom glaze;
[0021] Preparation of surface glaze: water-soluble varnish, low expansion glass powder and titanium dioxide are mixed and dispersed at high speed (1000-1200 rpm) until uniform, ground to a fineness of less than 20 μm by a three-roll grinder, and vibrated and filtered to obtain the surface glaze.
[0022] According to some preferred embodiments of the present invention, the high expansion glass powder and the low expansion glass powder are obtained by mixing, melting, quenching, grinding and homogenizing. The melting temperature is 1150-1300°C and the temperature is kept for 1-2 hours; the homogenized sieve particle size D 50 The value is 1.5-2μm, D 97 The value is 3.5-4μm.
[0023] In some embodiments, the preparation of high expansion glass powder and low expansion glass powder specifically includes the following steps:
[0024] 1) Mixing the ingredients: adding the ingredients by weight into a container and mixing them in an oscillating mixer to obtain a premix;
[0025] 2) Melting: The premix is loaded into a corundum crucible, placed in a muffle furnace, heated to the melting temperature and kept warm to complete the melting to obtain glass liquid;
[0026] 3) Quenching: Take out the corundum crucible, pour the glass liquid into cold water for water quenching, and obtain glass frit;
[0027] 4) Grinding: Place the glass frit in a ball mill, add pure water medium and zirconium balls for wet grinding to obtain glass slurry;
[0028] 5) Homogenization: Vibrate and sieve the glass slurry, dry it, and evenly crush it with high-pressure airflow, detect the sieved particle size, and obtain glass powder.
[0029] The present invention provides an application of the above-mentioned combined glaze in a photovoltaic backboard 2.0 mm semi-tempered glass, i.e., a photovoltaic backboard 2.0 mm semi-tempered glazed glass, wherein a laminated glaze layer formed by the combined glaze is provided at a light-transmitting portion where solar cells are connected on the surface of the photovoltaic backboard 2.0 mm semi-tempered glazed glass (i.e., a gap between adjacent solar cells), wherein the laminated glaze layer comprises a bottom glaze layer formed by the bottom glaze and a surface glaze layer formed by the surface glaze, wherein the dry film thickness of the bottom glaze layer is 10-20 μm, the dry film thickness of the surface glaze layer is 10-20 μm, and the dry film thickness of the laminated glaze layer is 20-40 μm.
[0030] Taking the photovoltaic backboard 2.0mm glass as the base, the bottom glaze is screen-printed and glazed at the light-transmitting part of the surface battery cell connection, solidified into a film, cooled down to form a bottom glaze layer, and the surface of the bottom glaze layer is then screen-printed and glazed with a surface glaze, solidified into a film, to form a surface glaze layer, and then the whole is tempered to form a laminated glaze layer. By controlling the dry film thickness of the bottom glaze layer and the surface glaze layer, the overall average linear expansion coefficient of the laminated glaze layer is made equivalent to the average linear expansion coefficient of the photovoltaic backboard 2.0mm semi-tempered glass, and the stress at the glaze strip on the smooth surface (non-glazed surface) is eliminated, so that the impact resistance is the same as that at the glazed surface glaze strip, the glazed surface non-glazed strip, and the smooth surface (non-glazed surface) non-glazed strip, and the falling ball height reaches 1.2m.
[0031] The present invention provides a photovoltaic module, comprising a front glass panel, a front packaging material layer, a battery layer, a rear packaging material layer, and a back glass panel, which are arranged in sequence from top to bottom, characterized in that the back glass panel is the photovoltaic back panel 2.0 mm semi-tempered glazed glass as described above.
[0032] Due to the adoption of the above technical solution, the present invention has the following advantages compared with the prior art: the preparation method of the composite glaze suitable for laminated glaze of the present invention, the prepared bottom glaze contains high expansion glass powder, the surface glaze contains low expansion glass powder and titanium dioxide; the average linear expansion coefficient of the high expansion glass powder is (95±5)×10 -7 / K(50-300℃)>Average linear expansion coefficient of 2.0mm semi-tempered glass for photovoltaic backsheet>Average linear expansion coefficient of low expansion glass powder (80±5)×10 -7 / K (50-300℃); the bottom glaze and the surface glaze successively form the bottom glaze layer and the surface glaze layer on the 2.0mm glass of the photovoltaic back panel, and then the whole is tempered to form a laminated glaze layer; the surface glaze layer is compressed by the bottom glaze layer to produce compressive stress, and its compressive strength is greater than the tensile strength, so that the glazed surface glaze strip and the glazed surface non-glazed strip, the smooth surface (non-glazed surface) non-glazed strip have the same impact resistance, and the ball drop height reaches 1.2m; by controlling the dry film thickness of the bottom glaze layer and the surface glaze layer, The overall average linear expansion coefficient of the laminated glaze layer is made equivalent to that of the 2.0mm semi-tempered glass of the photovoltaic backplane, eliminating the stress at the glaze strip on the smooth surface (non-glazed surface), making it have the same impact resistance as the glaze strip on the glazed surface, the non-glazed strip on the glazed surface, and the non-glazed strip on the smooth surface (non-glazed surface), with a falling ball height of 1.2m; the laminated glaze layer reduces the breakage rate of glass transportation / lamination, provides excellent static and dynamic airborne performance for large-panel modules, and effectively solves the problem of outdoor installation strength of large-panel modules. DETAILED DESCRIPTION
[0033] In order to enable those skilled in the art to better understand the technical solution of the present invention, the technical solution will be clearly and completely described below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work should fall within the scope of protection of the present invention.
[0034] Example 1 Preparation method of low expansion glass powder
[0035] The low expansion glass powder in this embodiment specifically includes the following preparation steps:
[0036] S1 ingredients are mixed evenly
[0037] The ingredients are mixed in proportion, added into a container, and placed in an oscillating mixer for uniform mixing to obtain a premix.
[0038] S2 Melt
[0039] The premix is loaded into a corundum crucible, placed in a muffle furnace, heated to a melting temperature of 1250°C and kept warm for 2 hours to complete the melting and obtain glass liquid.
[0040] S3 Quenching
[0041] Take out the corundum crucible, pour the glass liquid into cold water for water quenching, and obtain a glass frit.
[0042] S4 grinding
[0043] The glass frit is placed in a ball mill, and pure water medium and zirconium balls are added for wet grinding to obtain glass slurry.
[0044] S5 Homogenization
[0045] The glass slurry is vibrated, sieved and dried; crushed evenly by high-pressure airflow, and the sieved particle size D is tested 50 The value is 1.5-2μm, D 97 The value is 3.5-4μm, and low expansion glass powder is obtained.
[0046] Example 2 Combination glaze suitable for laminated glazing and 2.0 mm semi-tempered glazed glass for photovoltaic back panel The combination glaze suitable for laminated glazing in this example is prepared as follows:
[0047] 1) Preparation of water-soluble varnish
[0048] Mix 35 parts of dipropylene glycol butyl ether, 20 parts of tripropylene glycol methyl ether, 15 parts of diethylene glycol butyl ether, 26 parts of water-soluble acrylic resin, 1 part of polyethylene oxide and 2 parts of ethyl cellulose, stir and heat to 60°C, keep warm for 2 hours to dissolve, add 1 part of aqueous dispersant, mix well, cool to room temperature to obtain water-soluble varnish.
[0049] 2) Preparation of high expansion glass powder:
[0050] 2.1) Mixing the ingredients: weigh 42 parts of silicon dioxide, 18 parts of zinc oxide, 6 parts of bismuth oxide, 15 parts of boron oxide, 12 parts of sodium carbonate, 5 parts of titanium dioxide, and 2 parts of potassium carbonate, by mass, add them into a container, place it in an oscillating mixer and mix well to obtain a premix;
[0051] 2.2) Melting: The premix is placed in a corundum crucible, placed in a muffle furnace, heated to 1200°C and kept at this temperature for 2 hours to complete the melting and obtain glass liquid;
[0052] 2.3) Quenching: Take out the corundum crucible and pour the glass liquid into cold water for water quenching to obtain a glass frit;
[0053] 2.4) Grinding: Place the glass frit in a ball mill, add pure water medium and zirconium balls for wet grinding to obtain glass slurry;
[0054] 2.5) Homogenization: Vibrate the glass slurry, sieve it, dry it, crush it evenly with high-pressure airflow, and measure the sieved particle size D 50 The value is 1.5-2μm, D 97 The value is 3.5-4μm, and high expansion glass powder is obtained.
[0055] 3) Preparation of low expansion glass powder:
[0056] In parts by mass, the ingredients include 49 parts of zinc oxide, 30 parts of silicon dioxide, 8 parts of aluminum oxide, 5 parts of titanium dioxide, 4 parts of zirconium dioxide, 2 parts of calcium oxide, 2 parts of potassium carbonate, 0.5 parts of phosphorus pentoxide, 0.5 parts of sodium hexafluorosilicate and 0.2 parts of potassium chloride. The low expansion glass powder was prepared by the steps in Example 1.
[0057] 4) Preparation of bottom glaze: By weight, 32 parts of the water-soluble varnish of step 1) and 68 parts of the high expansion glass powder of step 2) are mixed and dispersed at high speed until uniform, ground to a fineness of less than 20 μm by a three-roll grinder, and filtered by vibration to obtain a bottom glaze.
[0058] 5) Preparation of surface glaze: By mass, 20 parts of the water-soluble varnish of step 1), 40 parts of step 3) and 40 parts of Chemours R-902 + titanium dioxide are mixed and dispersed at high speed until uniform, ground to a fineness of less than 20 μm by a three-roll grinder, and filtered by vibration to obtain a surface glaze.
[0059] The prepared composite glaze is applied to a 2.0 mm glass photovoltaic back panel. Specifically, the 2.0 mm glass photovoltaic back panel is used as the base, and the bottom glaze is screen-printed and glazed at the light-transmitting part of the surface where the solar cells are connected. The glaze is cured into a film and cooled to form a bottom glaze layer. The surface of the bottom glaze layer is then screen-printed and glazed with a surface glaze, which is cured into a film to form a surface glaze layer. The whole is then tempered to form a laminated glaze layer.
[0060] Example 3 Combination glaze suitable for laminated glazing and 2.0 mm semi-tempered glazed glass for photovoltaic backplane The combination glaze suitable for laminated glazing in this example is prepared in the following steps:
[0061] 1) Preparation of water-soluble varnish
[0062] Mix 33 parts of dipropylene glycol butyl ether, 18 parts of tripropylene glycol methyl ether, 15 parts of diethylene glycol butyl ether, 30 parts of water-soluble acrylic resin, 1 part of polyethylene oxide and 2 parts of ethyl cellulose, stir and heat to 60°C, keep warm for 2 hours to dissolve, add 1 part of aqueous dispersant, mix well, cool to room temperature to obtain water-soluble varnish.
[0063] 2) Preparation of high expansion glass powder:
[0064] 2.1) Mixing the ingredients: weigh 42 parts of silicon dioxide, 16 parts of zinc oxide, 6 parts of bismuth oxide, 17 parts of boron oxide, 12 parts of sodium carbonate, 5 parts of titanium dioxide, and 2 parts of potassium carbonate, by mass, add them into a container, place it in an oscillating mixer and mix well to obtain a premix;
[0065] 2.2) Melting: The premix is loaded into a corundum crucible, placed in a muffle furnace, heated to a melting temperature of 1200°C and kept at this temperature for 2 hours to complete the melting and obtain a glass liquid;
[0066] 2.3) Quenching: Take out the corundum crucible and pour the glass liquid into cold water for water quenching to obtain a glass frit;
[0067] 2.4) Grinding: Place the glass frit in a ball mill, add pure water medium and zirconium balls for wet grinding to obtain glass slurry;
[0068] 2.5) Homogenization: Vibrate the glass slurry, sieve it, dry it, crush it evenly with high-pressure airflow, and measure the sieved particle size D 50 The value is 1.5-2μm, D 97 The value is 3.5-4μm, and glass powder is obtained.
[0069] 3) Preparation of low expansion glass powder:
[0070] By mass, weigh 45 parts of zinc oxide, 34 parts of silicon dioxide, 8 parts of aluminum oxide, 5 parts of titanium dioxide, 4 parts of zirconium dioxide, 2 parts of calcium oxide, 2 parts of potassium carbonate, 0.5 parts of phosphorus pentoxide, 0.5 parts of sodium hexafluorosilicate, and 0.2 parts of potassium chloride; and prepare low expansion glass powder using the steps in Example 1.
[0071] 4) Preparation of bottom glaze: By weight, 35 parts of the water-soluble varnish of step 1) and 65 parts of the high expansion glass powder of step 2) are mixed and dispersed at high speed until uniform, ground to a fineness of less than 20 μm by a three-roll grinder, and filtered by vibration to obtain a bottom glaze.
[0072] 5) Preparation of surface glaze: By weight, 18 parts of the water-soluble varnish of step 1), 42 parts of the low-expansion glass powder of step 3) and 40 parts of Chemours R-706 titanium dioxide are mixed and dispersed at high speed until uniform, ground to a fineness of less than 20 μm by a three-roll grinder, and filtered by vibration to obtain a surface glaze.
[0073] The prepared composite glaze is applied to a 2.0 mm glass photovoltaic back panel. Specifically, the 2.0 mm glass photovoltaic back panel is used as the base, and the bottom glaze is screen-printed and glazed at the light-transmitting part of the surface where the solar cells are connected. The glaze is cured into a film and cooled to form a bottom glaze layer. The surface of the bottom glaze layer is then screen-printed and glazed with a surface glaze, which is cured into a film to form a surface glaze layer. The whole is then tempered to form a laminated glaze layer.
[0074] Comparative Example 1
[0075] The difference between this comparative example and Example 2 is that the photovoltaic backboard 2.0 mm semi-tempered glazed glass in this comparative example only has the surface glaze prepared in Example 2 silk-screened glaze, a surface glaze layer formed by solidification film formation and tempering treatment, and no bottom glaze layer. The preparation of water-soluble varnish and low-expansion glass powder and the titanium dioxide used are the same as in Example 2.
[0076] Comparative Example 2
[0077] The glass powder used for the base glaze in this comparative example is the low-expansion glass powder prepared in Example 2. The preparation of the base glaze in this comparative example is as follows: by weight, 32 parts of water-soluble varnish and 68 parts of low-expansion glass powder are mixed and dispersed at high speed until uniform, and then ground to a fineness of less than 20 μm by a three-roll grinder, and filtered by vibration to obtain the base glaze.
[0078] The preparation of water-soluble varnish, low expansion glass powder and surface glaze is the same as that of Example 2. That is, in this comparative example, the high expansion glass powder of the bottom glaze in Example 2 is replaced by the low expansion glass powder used in Example 2.
[0079] Comparative Example 3
[0080] The glass powder used for the surface glaze in this comparative example is the high expansion glass powder prepared in Example 2. The preparation of the surface glaze in this comparative example is as follows: by weight, 20 parts of water-soluble varnish, 40 parts of high expansion glass powder and 40 parts of Chemours R-902 + titanium dioxide are mixed and dispersed at high speed until uniform, ground by a three-roll grinder to a fineness of less than 20 μm, and filtered by vibration to obtain a surface glaze.
[0081] The preparation of water-soluble varnish, high expansion glass powder and bottom glaze is the same as that of Example 2. That is, in this comparative example, the low expansion glass powder of the surface glaze in Example 2 is replaced by the high expansion glass powder used in Example 2.
[0082] Example 4
[0083] 1) Glass powder particle size and average linear expansion coefficient
[0084] The particle size values and average linear expansion coefficient test results of the high expansion glass powder and low expansion glass powder in the embodiment are shown in Table 1. Among them, the average linear expansion coefficient of the 2.0 mm semi-tempered glass of the photovoltaic back panel is 87×10 -7 / K(50-300℃).
[0085] Table 1 Particle size and average linear expansion coefficient of glass powder
[0086]
[0087] The results in Table 1 show that the particle size values of the glass powder in the high expansion glass powder and the low expansion glass powder in the embodiment meet the sieve particle size D 50 The value is 1.5-2μm, D 97 The average linear expansion coefficient of the high expansion glass powder in the embodiment meets the requirement of (95±5)×10 -7 / K(50-300℃), the average linear expansion coefficient of the low expansion glass powder in the embodiment meets the requirements of (80±5)×10 -7 / K (50-300℃) index requirements.
[0088] 2) Impact resistance
[0089] The test results of the reflectivity SCI (550nm) of the 2.0mm semi-tempered glazed glass of the photovoltaic back panel at the glazed stripe, the glazed stripe, the glazed non-glazed stripe, the smooth surface (non-glazed surface) glazed stripe and the smooth surface (non-glazed surface) non-glazed stripe are shown in Table 2 below.
[0090] Impact resistance test method: A 227g (about 38.1mm in diameter) smooth steel ball is dropped onto the designated area of the 2.0mm semi-tempered glazed glass on the photovoltaic backsheet, and the lowest value without breakage is recorded.
[0091] Table 2 Impact resistance test results
[0092]
[0093] The results in Table 2 show that the reflectivity SCI (550nm) of the 2.0mm semi-tempered glazed glass glazed strip of the photovoltaic backsheet prepared by Examples 2-3 of the present invention reaches more than 80%, and the impact resistance of the glazed strip on the smooth surface (non-glazed surface) is the same as that of the glazed strip on the glazed surface, the glazed non-glazed strip, and the smooth surface (non-glazed surface) The non-glazed strip has the same impact resistance, and the ball drop height reaches 1.2m; in Comparative Example 1, only the surface glaze prepared in Example 2 is screen-printed, and its smooth surface (non-glazed surface) is ) The impact-resistant ball drop height at the glaze strip is 0.7m; the glass powder used for the bottom glaze in Comparative Example 2 is the low-expansion glass powder prepared in Example 2, and the impact-resistant ball drop height at the smooth surface (non-glazed surface) glaze strip is 0.6m; the glass powder used for the surface glaze in Comparative Example 3 is the high-expansion glass powder prepared in Example 2, and the impact-resistant ball drop height at the glazed surface strip is only 0.4m, and the impact-resistant ball drop height at the smooth surface (non-glazed surface) glaze strip is 0.8m.
[0094] The average linear expansion coefficient of the glass powder of the glaze used in the single glaze layer of the prior art is smaller than the average linear expansion coefficient of the 2.0 mm semi-tempered glass of the photovoltaic back panel, so that the impact resistance of the glazed strip on the glazed surface and the non-glazed strip on the glazed surface and the non-glazed strip on the smooth surface (non-glazed surface) is the same, and the ball falling height reaches 1.2m; but the maximum impact resistance of the smooth surface (non-glazed surface) is 0.7m.
[0095] In order to overcome the shortcomings and deficiencies of the prior art, the present invention aims to provide a composite glaze suitable for laminated glazing: 1. The bottom glaze contains high expansion glass powder, the surface glaze contains low expansion glass powder and titanium dioxide, and the average linear expansion coefficient of the high expansion glass powder is (95±5)×10 -7 / K(50-300℃)>Average linear expansion coefficient of 2.0mm semi-tempered glass for photovoltaic backsheet>Average linear expansion coefficient of low expansion glass powder (80±5)×10 -7 / K (50-300℃); 2. The bottom glaze and the surface glaze are successively formed on the 2.0mm glass of the photovoltaic back panel to form a bottom glaze layer and a surface glaze layer, and then the whole is tempered to form a laminated glaze layer. The surface glaze layer is compressed by the bottom glaze layer to produce compressive stress, and its compressive strength is greater than the tensile strength, so that the glazed surface glaze strips and the glazed surface non-glazed strips and the smooth surface (non-glazed surface) non-glazed strips have the same impact resistance, and the ball drop height reaches 1.2m; 3. By controlling the dry film thickness of the bottom glaze layer and the surface glaze layer The degree makes the average linear expansion coefficient of the laminated glaze layer as a whole equivalent to that of the 2.0mm semi-tempered glass of the photovoltaic backplane, eliminates the stress at the glaze strip on the smooth surface (non-glazed surface), and makes it have the same impact resistance as the glaze strip on the glazed surface, the non-glazed strip on the glazed surface, and the non-glazed strip on the smooth surface (non-glazed surface), and the drop ball height reaches 1.2m; the laminated glaze layer reduces the breakage rate of glass transportation / lamination, provides excellent static and dynamic airborne performance for large-panel modules, and effectively solves the problem of outdoor installation strength of large-panel modules.
[0096] The above embodiments are only for illustrating the technical concept and features of the present invention, and their purpose is to enable people familiar with this technology to understand the contents of the present invention and implement them accordingly. They cannot be used to limit the protection scope of the present invention. Any equivalent changes or modifications made according to the spirit of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for preparing a composite glaze suitable for photovoltaic backboard semi-tempered glass laminated glaze in photovoltaic modules, characterized in that: The steps include: Preparation of bottom glaze: mixing water-soluble varnish oil and high expansion glass powder and dispersing them uniformly, grinding and vibrating and filtering to obtain bottom glaze; Preparation of surface glaze: mixing and evenly dispersing water-soluble varnish, low expansion glass powder and titanium dioxide, grinding and vibrating and filtering to obtain surface glaze; The average linear expansion coefficient of the high expansion glass powder is greater than the average linear expansion coefficient of the heat-strengthened glass, and the average linear expansion coefficient of the heat-strengthened glass is greater than the average linear expansion coefficient of the low expansion glass powder; the combined glaze is used to form a laminated glaze layer on the photovoltaic glass; The high expansion glass powder comprises the following components by mass: 40-45 parts of silicon dioxide, 15-25 parts of zinc oxide, 5-10 parts of bismuth oxide, 15-20 parts of boron oxide, 10-15 parts of sodium carbonate, 5-10 parts of titanium dioxide, and 1-5 parts of potassium carbonate; The low expansion glass powder comprises the following components: 40-60 parts of zinc oxide, 25-35 parts of silicon dioxide, 5-10 parts of aluminum oxide, 5-10 parts of titanium dioxide, 3-6 parts of zirconium dioxide, 2-3 parts of calcium oxide, 1-2 parts of potassium carbonate, 0.5-1 parts of phosphorus pentoxide, 0.5-1 parts of sodium hexafluorosilicate, and 0.1-0.5 parts of potassium chloride; In parts by mass, the bottom glaze comprises 30-40 parts of water-soluble varnish and 60-70 parts of high-expansion glass powder; the surface glaze comprises 15-25 parts of water-soluble varnish, 35-45 parts of low-expansion glass powder and 40-50 parts of titanium dioxide.
2. The preparation method according to claim 1, characterized in that: The average linear expansion coefficient of the high expansion glass powder in the temperature range of 50-300°C is (95±5)×10 -7 / K; the average linear expansion coefficient of the low expansion glass powder in the temperature range of 50-300°C is (80±5)×10 -7 / K.
3. The preparation method according to claim 1, characterized in that: The preparation of the high expansion glass powder and the low expansion glass powder comprises the following steps: 1) Mix the ingredients uniformly: Mix the ingredients by weight and mix them uniformly to obtain a premix; 2) Melting: The premix is heated to the melting temperature and kept warm to complete the melting and obtain glass liquid; 3) Quenching: Pour the glass liquid into cold water for water quenching to obtain glass frit; 4) Grinding: wet grinding the glass frit to obtain glass slurry; 5) Homogenization: Vibrate the glass slurry, sieve it and dry it; The powder is crushed evenly, and the particle size is detected and sieved to obtain glass powder.
4. The preparation method according to claim 3, characterized in that: The smelting temperature is 1150-1300°C, and the temperature is kept for 1-2 hours; the homogenized screening particle size D 50 The value is 1.5-2μm, D 97 The value is 3.5-4μm.
5. The preparation method according to claim 1, characterized in that: The water-soluble varnish includes the following components by mass: 30-40 parts of dipropylene glycol butyl ether, 15-25 parts of tripropylene glycol methyl ether, 15-25 parts of diethylene glycol butyl ether, 20-40 parts of water-soluble acrylic resin, 1-5 parts of polyethylene oxide, 1-5 parts of ethyl cellulose and 1-5 parts of aqueous dispersant.
6. The preparation method according to claim 1 or 5, characterized in that: The water-soluble varnish is prepared by the following method: dipropylene glycol butyl ether, tripropylene glycol methyl ether, diethylene glycol butyl ether, water-soluble acrylic resin, polyethylene oxide, and ethyl cellulose are mixed, stirred, heated, and dissolved by heat preservation, and an aqueous dispersant is added, mixed evenly, and then cooled to room temperature to obtain the water-soluble varnish.
7. A composite glaze suitable for laminated glazing prepared by the preparation method according to any one of claims 1 to 6.