A shield mortar
By optimizing the basic components and expansion agent formula of the shield mortar, the problems of insufficient slurry stability and consolidation rate under high water-to-cement ratio were solved, achieving a consolidation rate of more than 100%, reducing project costs and secondary injection. Pulp workload.
Patent Information
- Application Number
- CN202311350788.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-10-18
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2043-10-18
AI Technical Summary
Under the condition of high water-cement ratio, the existing shield mortar has poor slurry stability, high bleeding rate, and less than 100% consolidation rate, resulting in pipe blockage and loose molding, which increases project costs and secondary grouting workload.
Using 2000 parts of basic components (240 parts of cement, 200 parts of bentonite, 280.6 parts of coarse sand, 420.8 parts of fine sand, 599.4-601.4 parts of heavy calcium, 257.2 parts of coal ash and 1.2 parts of hydroxypropyl methylcellulose) and 0.4- The formula of 1.6 parts of expansion agent optimizes the dry powder gradation ratio and slurry performance through reasonable gradation and addition of expansion agent and polymer active ingredients.
The bleeding rate is significantly reduced, the consolidation rate is increased to more than 100%, the slurry density and pumping performance are improved, the secondary grouting workload is reduced, and the project cost is reduced.
Smart Images

Figure BDA0004500207270000051 
Figure BDA0004500207270000061 
Figure BDA0004500207270000071
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of construction materials, and in particular to a shield mortar. Background Art
[0002] With the development of urban, highway and tunnel engineering and the continuous improvement of technology, the supporting auxiliary materials are also being standardized. Shield mortar is widely used in tunnel engineering. Its main function is to fill the gap between the tunnel segments and the soil, stabilize the segments, block groundwater, control stratum deformation and reduce settlement. The shield mortar on the current market is generally a simple compound of cement, sand and fly ash.
[0003] 1. At present, the shield mortar industry adjusts the ratio of sand and cement, which is affected by the fluctuation of raw materials, easily leading to poor pumpability and unstable mortar state, resulting in pipe blockage and looseness after molding.
[0004] 2. Shield mortar is mainly grouting through grouting pipe pressure. The technical requirements for slurry are good slurry flow and low slurry rate. In order to meet the technical requirements of the project, the water-binder ratio needs to be adjusted, which leads to a larger slurry bleeding rate, which indirectly affects the shrinkage of the finished product after solidification. The consolidation rate is far from 100%, and the project needs secondary grouting, which relatively increases the cost of the project.
[0005] Therefore, how to maintain the stability and uniformity of the slurry under a high water-binder ratio; how to solve the problem of shrinkage after slurry solidification while ensuring the slurry yield and achieve the consolidation rate requirement of 100% are issues that need to be addressed urgently. Summary of the invention
[0006] The embodiment of the present application provides a shield mortar to solve the problems existing in the related technology. The technical solution is as follows:
[0007] The embodiment of the present application provides a shield mortar, which includes, by weight: 2000 parts of a basic component, 780 parts of water, and 0.4-1.6 parts of an expansion agent;
[0008] The basic components include 240 parts of cement, 200 parts of bentonite, 280.6 parts of coarse sand, 420.8 parts of fine sand, 599.4-601.4 parts of heavy calcium, 257.2 parts of fly ash and 1.2 parts of hydroxypropyl methylcellulose.
[0009] In one embodiment, the composition comprises, by weight: 2000 parts of a base component, 780 parts of water and 0.4 parts of a swelling agent;
[0010] The basic components include 240 parts of cement, 200 parts of bentonite, 280.6 parts of coarse sand, 420.8 parts of fine sand, 600.2 parts of heavy calcium, 257.2 parts of fly ash and 1.2 parts of hydroxypropyl methylcellulose.
[0011] In one embodiment, the composition comprises, by weight: 2000 parts of a base component, 780 parts of water and 0.6 parts of a swelling agent;
[0012] The basic components include 240 parts of cement, 200 parts of bentonite, 280.6 parts of coarse sand, 420.8 parts of fine sand, 600.2 parts of heavy calcium, 257.2 parts of fly ash and 1.2 parts of hydroxypropyl methylcellulose.
[0013] In one embodiment, the composition comprises, by weight: 2000 parts of a base component, 780 parts of water and 0.8 parts of a swelling agent;
[0014] The basic components include 240 parts of cement, 200 parts of bentonite, 280.6 parts of coarse sand, 420.8 parts of fine sand, 600.2 parts of heavy calcium, 257.2 parts of fly ash and 1.2 parts of hydroxypropyl methylcellulose.
[0015] In one embodiment, the composition comprises, by weight: 2000 parts of a base component, 780 parts of water and 1.2 parts of a swelling agent;
[0016] The basic components include 240 parts of cement, 200 parts of bentonite, 280.6 parts of coarse sand, 420.8 parts of fine sand, 600.2 parts of heavy calcium, 257.2 parts of fly ash and 1.2 parts of hydroxypropyl methylcellulose.
[0017] In one embodiment, the composition comprises, by weight, 2000 parts of a base component, 780 parts of water and 1.6 parts of a swelling agent;
[0018] The basic components include 240 parts of cement, 200 parts of bentonite, 280.6 parts of coarse sand, 420.8 parts of fine sand, 600.2 parts of heavy calcium, 257.2 parts of fly ash and 1.2 parts of hydroxypropyl methylcellulose.
[0019] In one embodiment, the expansion agent is a plastic expansion agent.
[0020] In one embodiment, the swelling agent is azodicarbonamide.
[0021] The advantages or beneficial effects of the above technical solution include at least:
[0022] 1. Compared with shield mortars from other manufacturers, this solution has a significantly higher water-cement ratio and a lower slurry yield. When the same products are used, it effectively reduces the material cost of the project and responds to energy conservation and emission reduction.
[0023] 2. Under the condition of ensuring the slurry discharge rate, the water seepage rate of the mortar is reduced and the consolidation rate of the finished product is improved. The consolidation rate reaches more than 100%, which is significantly higher than the 94-96% on the market, effectively reducing the secondary grouting workload of the project.
[0024] 3. By using reasonable grading interval matching, each material can be reasonably configured according to the grading interval, which greatly improves the density of the slurry and effectively improves the slurry pumping performance and the strength of the slurry after forming.
[0025] 4. The dry powder gradation ratio of shield mortar is optimized. The gradation is optimized by matching coarse sand, fine sand, heavy calcium and fly ash, making the slurry performance stable.
[0026] 5. Adding expansion agent can effectively provide expansion while maintaining the performance of slurry. After the specimen is formed, it can ensure the micro-expansion effect of the product and make the consolidation rate reach more than 100%.
[0027] 6. Adding the polymer active ingredient hydroxypropyl methylcellulose can significantly improve the slurry bleeding rate under high water-binder ratio.
[0028] The above summary is for illustrative purposes only and is not intended to be limiting in any way. In addition to the illustrative aspects, embodiments and features described above, further aspects, embodiments and features of the present application will be readily apparent by reference to the following detailed description. DETAILED DESCRIPTION
[0029] In the following, only some exemplary embodiments are briefly described. As those skilled in the art will appreciate, the described embodiments may be modified in various ways without departing from the spirit or scope of the present application. Therefore, the description is considered to be exemplary rather than restrictive in nature.
[0030] The embodiment of the present application provides a shield mortar, which includes, by weight: 2000 parts of a basic component, 780 parts of water, and 0.4-1.6 parts of an expansion agent;
[0031] Among them, the basic components include 240 parts of cement, 200 parts of bentonite, 280.6 parts of coarse sand, 420.8 parts of fine sand, 599.4-601.4 parts of heavy calcium, 257.2 parts of fly ash and 1.2 parts of hydroxypropyl methylcellulose.
[0032] In one embodiment, the composition comprises, by weight: 2000 parts of a base component, 780 parts of water and 0.4 parts of a swelling agent;
[0033] Among them, the basic components include 240 parts of cement, 200 parts of bentonite, 280.6 parts of coarse sand, 420.8 parts of fine sand, 600.2 parts of heavy calcium, 257.2 parts of fly ash and 1.2 parts of hydroxypropyl methylcellulose.
[0034] In one embodiment, the composition comprises, by weight: 2000 parts of a base component, 780 parts of water and 0.6 parts of a swelling agent;
[0035] Among them, the basic components include 240 parts of cement, 200 parts of bentonite, 280.6 parts of coarse sand, 420.8 parts of fine sand, 600.2 parts of heavy calcium, 257.2 parts of fly ash and 1.2 parts of hydroxypropyl methylcellulose.
[0036] In one embodiment, the composition comprises, by weight: 2000 parts of a base component, 780 parts of water and 0.8 parts of a swelling agent;
[0037] Among them, the basic components include 240 parts of cement, 200 parts of bentonite, 280.6 parts of coarse sand, 420.8 parts of fine sand, 600.2 parts of heavy calcium, 257.2 parts of fly ash and 1.2 parts of hydroxypropyl methylcellulose.
[0038] In one embodiment, the composition comprises, by weight: 2000 parts of a base component, 780 parts of water and 1.2 parts of a swelling agent;
[0039] Among them, the basic components include 240 parts of cement, 200 parts of bentonite, 280.6 parts of coarse sand, 420.8 parts of fine sand, 600.2 parts of heavy calcium, 257.2 parts of fly ash and 1.2 parts of hydroxypropyl methylcellulose.
[0040] In one embodiment, the expansion agent is a plastic expansion agent.
[0041] In one embodiment, the swelling agent is azodicarbonamide.
[0042] Through the chemical mechanism of the plastic expansion agent, because it reacts slowly with water under alkaline conditions to produce tiny bubbles, it produces an expansion effect before the cement mixture solidifies.
[0043] Example 1
[0044] The shield mortar without expansion components of this embodiment includes 240g of cement, 200g of bentonite, 280.6g of coarse sand, 420.8g of fine sand, 600.2g of heavy calcium carbonate, 257.2g of fly ash and 1.2g of hydroxypropyl methylcellulose.
[0045] Example 2
[0046] The shield mortar without expansion components in this embodiment includes 240 g of cement, 200 g of bentonite, 280.6 g of coarse sand, 420.8 g of fine sand, 601.4 g of heavy calcium and 257.2 g of fly ash.
[0047] Comparative Example 1
[0048] The shield mortar of this embodiment includes 2000 g of the shield mortar without expansion component in Example 1, 0.4 g of expansion agent and 780 g of water.
[0049] Comparative Example 2
[0050] The shield mortar of this embodiment includes 2000 g of the shield mortar without expansion component in Example 1, 0.6 g of expansion agent and 780 g of water.
[0051] Comparative Example 3
[0052] The shield mortar of this embodiment includes 2000 g of the shield mortar without expansion component in Example 1, 0.8 g of expansion agent and 780 g of water.
[0053] Comparative Example 4
[0054] The shield mortar of this embodiment includes 2000 g of the shield mortar without expansion component in Example 1, 1.2 g of expansion agent and 780 g of water.
[0055] Comparative Example 5
[0056] The shield mortar of this embodiment includes 2000 g of the shield mortar without expansion component in Example 1, 1.6 g of expansion agent and 780 g of water.
[0057] Comparative Example 6
[0058] The shield mortar of this embodiment includes 2000 g of the shield mortar without expansion component in Example 2, 0.4 g of expansion agent and 780 g of water.
[0059] Comparative Example 7
[0060] The shield mortar of this embodiment includes 2000 g of the shield mortar without expansion component in Example 2, 0.6 g of expansion agent and 780 g of water.
[0061] Comparative Example 8
[0062] The shield mortar of this embodiment includes 2000 g of the shield mortar without expansion component in Example 2, 0.8 g of expansion agent and 780 g of water.
[0063] Comparative Example 9
[0064] The shield mortar of this embodiment includes 2000 g of the shield mortar without expansion component in Example 2, 1.2 g of expansion agent and 780 g of water.
[0065] Comparative Example 10
[0066] The shield mortar of this embodiment includes 2000 g of the shield mortar without expansion component in Example 2, 1.6 g of expansion agent and 780 g of water.
[0067] Azodicarbonamide was used as the expansion agent in all the embodiments and comparative examples.
[0068] The shield mortars obtained in the above-mentioned Examples 1 to 5 and Comparative Examples 1 to 5 were subjected to water seepage test, fluidity test, strength test and consolidation rate test respectively. The test comparison results are as follows:
[0069]
[0070]
[0071]
[0072] By comparing the data of Examples 1 to Comparative Examples 10, it can be concluded that when no water-retaining component (hydroxypropyl methylcellulose) is added, such as in Example 2 and Comparative Examples 6-10, the water seepage rate is 2.4% on average; when the water-retaining component (hydroxypropyl methylcellulose) is added, such as in Example 1 and Comparative Examples 1-5, the water seepage rate is 1.3%; after comparative analysis, after adding the water-retaining component (hydroxypropyl methylcellulose), the water seepage rate of the slurry is significantly reduced.
[0073] After experiments on Example 1 to Comparative Example 10, after data comparison and analysis, in Example 1 to Example 2, when no expansion agent component was added, the overall consolidation rate averaged 95%, while in the comparative example, the consolidation rate was 95% when the expansion agent was added at 0.4, the consolidation rate was 98% when it was added at 0.6, the consolidation rate was 104% when it was added at 0.8, the consolidation rate was 107% when it was added at 1.2, and the consolidation rate was 111% when it was added at 1.6. No obvious changes were found in the tests on other indicators except the change in consolidation rate between the formula with expansion agent and the formula without expansion agent. Therefore, it can also be indirectly analyzed that there is no effect on other technical indicators when the expansion agent is added.
[0074] The conclusion is: in the formula with appropriate amount of expansion agent, the consolidation rate is much higher than the formula without expansion agent.
[0075] For the confirmed dosage of plastic expansive agent, the same ratio was retested three times, and the consolidation rates were 102%, 103%, and 102% respectively, with an average value of 102%. The dosage of 0.04% had no effect on the slurry performance, and all the slurry data were excellent. Therefore, it was concluded that adding 0.04% of expansive agent can meet the requirement of 100% consolidation rate of shield mortar and achieve the goal of reducing costs and increasing efficiency.
[0076] The advantages or beneficial effects of the above technical solution include at least:
[0077] 1. Compared with shield mortars from other manufacturers, this solution has a significantly higher water-cement ratio and a lower slurry yield. When the same products are used, it effectively reduces the material cost of the project and responds to energy conservation and emission reduction.
[0078] 2. Under the condition of ensuring the slurry discharge rate, the water seepage rate of the mortar is reduced and the consolidation rate of the finished product is improved. The consolidation rate reaches more than 100%, which is significantly higher than the 94-96% on the market, effectively reducing the secondary grouting workload of the project.
[0079] 3. By using reasonable grading interval matching, each material can be reasonably configured according to the grading interval, which greatly improves the density of the slurry and effectively improves the slurry pumping performance and the strength of the slurry after forming.
[0080] 4. The dry powder gradation ratio of shield mortar is optimized. The gradation is optimized by matching coarse sand, fine sand, heavy calcium and fly ash, making the slurry performance stable.
[0081] 5. Adding expansion agent can effectively provide expansion while maintaining the performance of slurry. After the specimen is formed, it can ensure the micro-expansion effect of the product and make the consolidation rate reach more than 100%.
[0082] 6. Adding the polymer active ingredient hydroxypropyl methylcellulose can significantly improve the slurry bleeding rate under high water-binder ratio.
[0083] In the description of this specification, the description with reference to the terms "one embodiment", "some embodiments", "example", "specific example", or "some examples" means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present application. Moreover, the specific features, structures, materials or characteristics described may be combined in any one or more embodiments or examples in a suitable manner. In addition, those skilled in the art may combine and combine different embodiments or examples described in this specification and the features of different embodiments or examples, unless they are contradictory.
[0084] In addition, the terms "first" and "second" are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly indicating the number of technical features indicated. Therefore, a feature defined as "first" or "second" may explicitly or implicitly include at least one of the features. In the description of this application, the meaning of "plurality" is two or more, unless otherwise clearly and specifically defined.
[0085] The above is only a specific implementation of the present application, but the protection scope of the present application is not limited thereto. Any technician familiar with the technical field can easily think of various changes or substitutions within the technical scope disclosed in the present application, which should be included in the protection scope of the present application. Therefore, the protection scope of the present application should be based on the protection scope of the claims.
Claims
1. A shield mortar, It is characterized in that The composition is composed of 2000 parts of basic components, 780 parts of water and 0.8-1.6 parts of expansion agent by weight; the expansion agent is azodicarbonamide; The basic components include 240 parts of cement, 200 parts of bentonite, 280.6 parts of coarse sand, 420.8 parts of fine sand, 599.4-601.4 parts of heavy calcium, 257.2 parts of fly ash and 1.2 parts of hydroxypropyl methylcellulose.
2. The shield mortar according to claim 1, It is characterized in that By mass, it is composed of 2000 parts of basic components, 780 parts of water and 0.8 parts of expansion agent; The basic components include 240 parts of cement, 200 parts of bentonite, 280.6 parts of coarse sand, 420.8 parts of fine sand, 600.2 parts of heavy calcium, 257.2 parts of fly ash and 1.2 parts of hydroxypropyl methylcellulose.
3. The shield mortar according to claim 1, It is characterized in that By mass, it is composed of 2000 parts of basic components, 780 parts of water and 1.2 parts of expansion agent; The basic components include 240 parts of cement, 200 parts of bentonite, 280.6 parts of coarse sand, 420.8 parts of fine sand, 600.2 parts of heavy calcium, 257.2 parts of fly ash and 1.2 parts of hydroxypropyl methylcellulose.
4. The shield mortar according to claim 1, It is characterized in that The composition is composed of 2000 parts of a base component, 780 parts of water and 1.6 parts of an expansion agent, calculated by weight; The basic components include 240 parts of cement, 200 parts of bentonite, 280.6 parts of coarse sand, 420.8 parts of fine sand, 600.2 parts of heavy calcium, 257.2 parts of fly ash and 1.2 parts of hydroxypropyl methylcellulose.