A sol-gel composite coating and its preparation method and application

Through the preparation method of sol-gel composite coating, combined with zeolite imidazole ester skeleton and nitrogen-doped carbon quantum dots, the problems of insufficient corrosion resistance and single function of microarc oxidation coating are solved, and excellent photocatalytic antibacterials are achieved and corrosion resistance, providing industrial applications of bifunctional coatings.

CN117603598BActive Publication Date: 2024-11-08BEIJING INSTITUTE OF PETROCHEMICAL TECHNOLOGY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202311529131.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-11-16
Publication Date
2024-11-08
Estimated Expiration
2043-11-16

AI Technical Summary

Technical Problem

The existing microarc oxidation coatings have shortcomings in corrosion resistance and are relatively single in function, which cannot effectively prevent the growth and reproduction of microorganisms.

Method used

Using the preparation method of sol-gel composite coating, the zeolite imidazole ester skeleton is mixed with nitrogen-doped carbon quantum dots and mixed with sol-gel solution and aged treatment, forming excellent photocatalytic antibacterial and corrosion resistance. Performance coating.

Benefits of technology

It realizes long-term protection of metal surfaces, significantly improves corrosion resistance and antibacterial effects, and provides a dual-functional coating solution with low cost, simple process, environmental protection and pollution-free.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117603598B_ABST
    Figure CN117603598B_ABST
Patent Text Reader

Abstract

The present invention provides a sol-gel composite coating and a preparation method and application thereof, which belongs to the technical field of metal coating development. The present invention uses zeolite imidazolate skeleton and nitrogen-doped carbon quantum dots as raw materials to successfully prepare a sol-gel composite coating with excellent photocatalytic antibacterial and corrosion resistance. The sol-gel composite coating provided by the present invention can solve the problem that the corrosion resistance of micro-arc oxidation coatings in the prior art still needs to be improved and the functions are relatively single. The sol-gel composite coating provided by the present invention has excellent photocatalytic antibacterial and corrosion resistance, can effectively prevent the growth and reproduction of microorganisms, and realize the long-term service of metals; the preparation method provided by the present invention can obtain a sol-gel composite coating with excellent performance, which has the advantages of low cost, simple process, environmental protection and pollution-free, and provides a new idea for the industrial application of antibacterial and anticorrosive dual-functional coatings.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of metal coating development, in particular to a sol-gel composite coating and a preparation method and application thereof. Background Art

[0002] Micro-arc oxidation (MAO), also known as plasma electrolytic oxidation (PEO), is a process developed from anodizing technology, and the resulting coating is superior to anodizing. The MAO process primarily relies on the matching and regulation of electrolyte and electrical parameters. Under the instantaneous high temperature and high pressure generated by arc discharge, a modified ceramic coating composed primarily of matrix metal oxides and supplemented with electrolyte components grows on the surface of valve metals such as aluminum, magnesium, and titanium, and their alloys. Its corrosion and wear resistance are significantly superior to traditional anodized coatings. However, existing MAO coatings still suffer from problems such as excessive porosity and poor corrosion resistance.

[0003] Chinese patent CN107460453A discloses a method for preparing a magnesium alloy micro-arc oxidation-sol-gel composite coating. The composite coating has good bonding strength and a dense structure. It uses a multi-component SiO2-CeO2-TiO2 oxide coating to overcome the limitations of single-component or two-component oxide coatings and improve coating performance.

[0004] However, the corrosion resistance of existing micro-arc oxidation still needs to be improved, and its function is relatively simple. Summary of the Invention

[0005] The object of the present invention is to provide a sol-gel composite coating and a preparation method and application thereof, which has excellent photocatalytic antibacterial and corrosion resistance properties.

[0006] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:

[0007] The present invention provides a method for preparing a sol-gel composite coating, comprising the following steps:

[0008] Mixing the zeolite imidazolate framework with nitrogen-doped carbon quantum dots to obtain a mixture 1;

[0009] The mixture 1 is sequentially subjected to ultrasonic treatment, washing and vacuum drying to obtain a composite material;

[0010] mixing the sol-gel liquid A, the sol-gel liquid B and the composite material to obtain a mixture 2;

[0011] The mixture is subjected to aging treatment to obtain a sol-gel composite coating.

[0012] Preferably, the sol-gel solution A contains anhydrous ethanol, water and trimethoxysilane, and the volume ratio of anhydrous ethanol, water and trimethoxysilane in the sol-gel solution A is 13-17:5-9:10-14;

[0013] The sol-gel liquid B contains anhydrous ethanol, ethyl acetoacetate and tetraethoxysilane, and the volume ratio of anhydrous ethanol, ethyl acetoacetate and tetraethoxysilane in the sol-gel liquid B is 7=1.8-2.2:0.8-1.2:1.8-2.2.

[0014] Preferably, the vacuum drying temperature is 95-110°C;

[0015] The vacuum drying time is 10 to 14 hours;

[0016] The aging time is 20 to 30 hours.

[0017] Preferably, the addition amount of the composite material is 0.02-0.1 wt % based on the total weight of the sol-gel solution A and the sol-gel solution B.

[0018] Preferably, the nitrogen-doped carbon quantum dots are obtained by a preparation method comprising the following steps:

[0019] Nitrogen-doped carbon quantum dots were prepared by thermal decomposition method using citric acid as carbon source and urea as nitrogen source.

[0020] Preferably, the weight ratio of citric acid to urea is 2 to 4:1;

[0021] The temperature of the thermal decomposition method is 150 to 250°C;

[0022] The time of the thermal decomposition method is 4 to 8 hours.

[0023] Preferably, the zeolite imidazolate framework is obtained by a preparation method comprising the following steps:

[0024] The zeolitic imidazolate framework is prepared by using Zn(NO3)2·6H2O as a metal salt through a hydrothermal method, a solvothermal method, a solvent azeotropic method or a microwave method;

[0025] Preferably, the zeolite imidazolate framework is obtained by a preparation method comprising the following steps:

[0026] Zn(NO3)2·6H2O is mixed with methanol and 2-methylimidazole and reacted for 0.5 to 1.5 hours to obtain a zeolite imidazole ester framework;

[0027] The mass ratio of the Zn(NO3)2·6H2O to the volume ratio of methanol is 1 g:8-12 mL;

[0028] The mass ratio of the Zn(NO3)2·6H2O to 2-methylimidazole is 1:2-2.5.

[0029] The present invention also provides a sol-gel composite coating obtained by the preparation method.

[0030] The present invention also provides the use of the sol-gel composite coating in protecting a metal micro-arc oxidation layer.

[0031] The present invention also provides a coated substrate, characterized in that it comprises a metal substrate treated with micro-arc oxidation and the above-mentioned sol-gel composite coating, wherein the sol-gel composite coating is coated on at least a portion of the metal substrate;

[0032] The coating is achieved by a dip-coating method.

[0033] Beneficial effects of the present invention:

[0034] The sol-gel composite coating provided by the present invention has excellent photocatalytic antibacterial and corrosion-resistant properties, can effectively prevent the growth and reproduction of microorganisms, and realize the long-term service of metals; the preparation method provided by the present invention can obtain a sol-gel composite coating with excellent performance, which has the advantages of low cost, simple process, environmental protection and pollution-free, and provides a new idea for the industrial application of antibacterial and anticorrosive dual-functional coatings. BRIEF DESCRIPTION OF THE DRAWINGS

[0035] Figure 1 Electrochemical impedance spectroscopy and polarization curves of the unsoaked Blank (LA91), MAO, MAO / SG, and MAO / SG+ZIF-8 / N-CQDs film samples in Example 1 of the present invention; wherein: (a) is the Nernquist plot of the electrochemical impedance spectroscopy; (b) is the Bode plot of the electrochemical impedance spectroscopy; (c) is the phase angle diagram of the electrochemical impedance spectroscopy; and (d) is the polarization curve.

[0036] Figure 2 This is a graph showing the plate count of Escherichia coli against Blank (LA91), MAO, MAO / SG, and MAO / SG+ZIF-8 / N-CQDs film samples (under dark and light conditions) in Example 1 of the present invention;

[0037] Figure 3 This is a graph showing the test results of LA91, MAO, MAO / SG, and MAO / SG+ZIF-8 / N-CQDs (under dark and light conditions) film samples on Escherichia coli in Example 1 of the present invention. DETAILED DESCRIPTION

[0038] The present invention provides a method for preparing a sol-gel composite coating, comprising the following steps:

[0039] Mixing the zeolite imidazolate framework with nitrogen-doped carbon quantum dots to obtain a mixture 1;

[0040] The mixture 1 is sequentially subjected to ultrasonic treatment, washing and vacuum drying to obtain a composite material;

[0041] mixing the sol-gel liquid A, the sol-gel liquid B and the composite material to obtain a mixture 2;

[0042] The mixture is subjected to aging treatment to obtain a sol-gel composite coating.

[0043] In the present invention, the sol-gel liquid A preferably contains anhydrous ethanol, water and trimethoxysilane, and the volume ratio of anhydrous ethanol, water and trimethoxysilane in the sol-gel liquid A is 13-17:5-9:10-14; the sol-gel liquid B preferably contains anhydrous ethanol, ethyl acetoacetate and tetraethoxysilane, and the volume ratio of anhydrous ethanol, ethyl acetoacetate and tetraethoxysilane in the sol-gel liquid B is 7=1.8-2.2:0.8-1.2:1.8-2.2.

[0044] In the present invention, the vacuum drying temperature is preferably 95 to 110° C.; the vacuum drying time is preferably 10 to 14 hours; the aging time is preferably 20 to 30 hours; and the addition amount of the composite material is preferably 0.02 to 0.1 wt % based on the total weight of the sol-gel A solution and the sol-gel B solution.

[0045] In the present invention, the nitrogen-doped carbon quantum dots are preferably obtained by a preparation method comprising the following steps: using citric acid as a carbon source and urea as a nitrogen source, and preparing nitrogen-doped carbon quantum dots by thermal decomposition; the weight ratio of citric acid and urea is preferably 2 to 4:1; the temperature of the thermal decomposition method is preferably 150 to 250°C; and the time of the thermal decomposition method is preferably 4 to 8 hours.

[0046] In the present invention, the zeolite imidazole ester skeleton is preferably obtained by a preparation method comprising the following steps: using Zn(NO3)2·6H2O as a metal salt, and preparing the zeolite imidazole ester skeleton by a hydrothermal method, a solvent thermal method, a solvent azeotropic method or a microwave method; further, the zeolite imidazole ester skeleton is preferably obtained by a preparation method comprising the following steps: mixing Zn(NO3)2·6H2O with methanol and 2-methylimidazole, and reacting for 0.5 to 1.5 hours to obtain a zeolite imidazole ester skeleton; the mass ratio of the Zn(NO3)2·6H2O to the volume of methanol is preferably 1g:8 to 12mL; the mass ratio of the Zn(NO3)2·6H2O to 2-methylimidazole is preferably 1:2 to 2.5.

[0047] The present invention also provides a sol-gel composite coating obtained by the preparation method.

[0048] The present invention also provides the use of the aforementioned sol-gel composite coating for metal micro-arc oxidation layer protection. The present invention also provides a coated substrate, characterized by comprising a metal substrate treated with micro-arc oxidation and the aforementioned sol-gel composite coating, wherein the sol-gel composite coating is coated on at least a portion of the metal substrate.

[0049] In the present invention, the coating is achieved by a dipping and pulling method.

[0050] The technical solutions provided by the present invention are described in detail below with reference to the embodiments, but they should not be construed as limiting the scope of protection of the present invention.

[0051] Example 1

[0052] (1) Synthesis of MAO: A metal block polished to #2000 with sandpaper was ultrasonically cleaned with deionized water and anhydrous ethanol in turn; each ultrasonic cleaning step lasted 10 minutes; the surface solution of the cleaned metal block was blown dry with a hair dryer; the metal substrate implemented in this example was LA91 magnesium-lithium alloy. A low-energy silicate electrolyte system was used, including NaOH (50 g / L), Na2SiO3 (40 g / L), Na2B4O7·10H2O (30 g / L) and C6H5Na3O7·2H2O (40 g / L). The MAO coating was prepared by a constant current method, where the current density was 10 mA / cm 2 , voltage range is 0-130V, and growth time is 20min.

[0053] (2) Synthesis of ZIF-8 / N-CQDs: Solution A was prepared by dissolving 12.0 g of citric acid and 4.0 g of urea in 40 mL of deionized water and ultrasonicating for 10 min. The mixture was placed in a reactor and kept at 200 °C for 6 h.

[0054] Solution B was prepared by adding 2 g of Zn(NO3)2·6H2O to 20 mL of methanol and ultrasonicating for 10 min. 4.4 g of 2-methylimidazole was then added and mixed. The mixture was stirred for 1 h. While stirring, the heated solution A was added dropwise to solution B. The mixture was ultrasonicated for 10 min. The mixture was centrifuged three times with deionized water at 8000 rpm and dried under vacuum at 100 °C for 12 h to obtain ZIF-8 / N-CQDs.

[0055] (3) Synthesis of MAO / SG+ZIF-8 / N-CQDs: Preparation of SG A sol: 45 mL of anhydrous ethanol was added to 21 mL of deionized water. After stirring with a glass rod for a while, 36 mL of GPTMS was slowly added. A magnetic stirring bar was placed in the beaker, and the beaker was sealed with plastic wrap. The mixture was stirred on a stirrer for 1 h.

[0056] Prepare SG B sol: add 9 mL of ethyl acetoacetate to 18 mL of anhydrous ethanol, then slowly add 18 mL of LTEOS, add 1.8 mL of acetic acid to adjust the pH value, add a magnetic stirring bar, seal the beaker with plastic wrap, and stir for 1 hour.

[0057] After stirring, the prepared B sol was dripped into the A sol with a dropper, and after mixing, 0.05 wt% of ZIF-8 / N-CQDs filler was added, stirred for 30 min, and aged for 24 h.

[0058] The metal block containing the MAO coating was slowly immersed into the prepared sol-gel through an immersion and pulling coating machine until the sample was completely immersed. After immersion for 5 minutes, the sample was pulled upward until it completely left the solution surface and then stood for 15 minutes. The above coating steps were repeated twice to finally obtain the MAO / SG+ZIF-8 / N-CQDs film sample.

[0059] Example 2

[0060] (1) Synthesis of MAO: Same as Example 1.

[0061] (2) Synthesis of ZIF-8 / N-CQDs: Solution A was prepared by dissolving 12.0 g of citric acid and 4.0 g of ethylenediamine in 40 mL of deionized water and ultrasonicating for 10 min. The mixture was placed in a reactor and kept at 200 °C for 6 h.

[0062] Prepare solution B: Add 2 g of Zn(NO3)2·6H2O to 20 mL of methanol and sonicate for 10 min. Then add 4.4 g of 2-methylimidazole and mix. Stir for 1 h. While stirring, add the heated solution A dropwise to solution B. Sonicate for 10 min. Centrifuge three times with deionized water at 8000 rpm and dry under vacuum at 100°C for 12 h.

[0063] (3) Synthesis of MAO / SG+ZIF-8 / N-CQDs: Preparation of SG A sol: 15 mL of anhydrous ethanol was added to 7 mL of deionized water. After stirring with a glass rod for a while, 12 mL of GPTMS was slowly added. A magnetic stirring bar was placed in the beaker, and the beaker was sealed with plastic wrap. The mixture was stirred on a stirrer for 1 h.

[0064] Prepare SG B sol: add 3 mL of ethyl acetoacetate to 6 mL of anhydrous ethanol, then slowly add 6 mL of LTEOS, add 0.6 mL of acetic acid to adjust the pH value, add a magnetic stirring bar, seal the beaker with plastic wrap, and stir for 1 hour.

[0065] After stirring, the prepared B sol was dripped into the A sol with a dropper, and after mixing, 0.05 wt% of ZIF-8 / N-CQDs filler was added, stirred for 30 min, and aged for 24 h.

[0066] Example 3

[0067] (1) Synthesis of MAO: A metal block polished to #2000 with sandpaper was ultrasonically cleaned with deionized water and then anhydrous ethanol. Each ultrasonic cleaning step lasted 10 min. The surface solution of the cleaned metal block was blown dry with a hair dryer. The metal substrate in this example was AZ31 magnesium alloy. A low-energy silicate electrolyte system was used, including NaOH (50 g / L), Na2SiO3 (40 g / L), Na2B4O7·10H2O (30 g / L), and C6H5Na3O7·2H2O (40 g / L).

[0068] (2) Synthesis of ZIF-8 / N-CQDs: Solution A was prepared by dissolving 12.0 g of citric acid and 4.0 g of urea in 40 mL of deionized water and ultrasonicating for 10 min. The mixture was placed in a reactor and kept at 200 °C for 6 h.

[0069] Prepare solution B: Add 2 g of Zn(NO3)2·6H2O to 20 mL of methanol and sonicate for 10 min. Then add 4.4 g of 2-methylimidazole and mix. Stir for 1 h. While stirring, add the heated solution A dropwise to solution B. Sonicate for 10 min. Centrifuge three times with deionized water at 8000 rpm and dry under vacuum at 100°C for 12 h.

[0070] (3) Synthesis of MAO / SG+ZIF-8 / N-CQDs: Prepare SG A solution: add 45 mL of anhydrous ethanol to 21 mL of deionized water, stir with a glass rod for a while, then slowly add 36 mL of GPTMS, add a magnetic stirrer, seal the beaker with plastic wrap, and stir on a stirrer for 1 h.

[0071] Prepare SG B sol: add 9 mL of ethyl acetoacetate to 18 mL of anhydrous ethanol, then slowly add 18 mL of LTEOS. Add 1.8 mL of acetic acid to adjust the pH value. Place a magnetic stirrer, seal the beaker with plastic wrap, and stir for 1 hour.

[0072] After stirring, the prepared B sol was dripped into the A sol with a dropper, and after mixing, 0.2 wt% of ZIF-8 / N-CQDs filler was added, stirred for 30 min, and aged for 24 h.

[0073] Comparative Example 1

[0074] (1) Synthesis of MAO: Same as Example 1.

[0075] (2) Synthesis of MAO / SG: Preparation of SG A sol: Same as in Example 1.

[0076] Preparation of SG B sol: same as in Example 1.

[0077] After stirring, the prepared B sol was dripped into the A sol using a dropper, stirred for 30 minutes, and aged for 24 hours.

[0078] The metal block containing the MAO coating was slowly immersed into the prepared sol-gel through an immersion and pulling coating machine until the sample was completely immersed. After immersion for 5 minutes, the sample was pulled upward until it completely left the solution surface and then stood for 15 minutes. The above coating steps were repeated twice to finally obtain the MAO / SG film layer sample.

[0079] Experimental Example 1

[0080] The Blank (LA91), MAO, MAO / SG+ZIF-8 / N-CQDs film samples prepared in Example 1 and the MAO / SG film sample prepared in Comparative Example 1 were subjected to electrochemical impedance spectroscopy testing using a Wuhan Corrtest CS350 electrochemical workstation to test the corrosion resistance of the composite film on magnesium alloy.

[0081] A three-electrode system was used, with the sample as the working electrode, the Ag / AgCl electrode as the reference electrode, and the platinum mesh as the auxiliary electrode. The corrosion medium was 3.5 wt.% NaCl solution, and the test area was 1 cm 2 .

[0082] The results are as follows Figure 1 As shown in the figure, it can be seen that the MAO / SG+ZIF-8 / N-CQDs film has the largest impedance modulus value in the low-frequency region, reaching 5.07×10 4 Ω·cm 2 Compared with MAO / SG without adding ZIF-8 / N-CQDs, it is improved by about one order of magnitude, and among all the film layers, the corrosion current density of the MAO / SG+ZIF-8 / N-CQDs film layer is the smallest and the corrosion potential is the largest, indicating that the sol-gel composite coating provided by the present invention can exhibit excellent corrosion resistance when used for MAO coating.

[0083] Experimental Example 2

[0084] The plate count method was used to evaluate the antibacterial effects of Blank (LA91), MAO, MAO / SG+ZIF-8 / N-CQDs film samples prepared in Example 1 and the MAO / SG film sample prepared in Comparative Example 1 on Escherichia coli. The test results are as follows: Figures 2-3 shown.

[0085] Escherichia coli was cultured in LB liquid culture medium at 37°C for 16 h. Blank (LA91), MAO, MAO / SG, and MAO / SG+ZIF-8 / N-CQDs film samples with a size of 4 cm × 4 cm × 5 mm were first irradiated with UV light to fully kill the bacteria on the surface. After UV irradiation for 10 min, 100 μL of 10% ZIF-8 was added to the surface of each film. 8 CFU / mL of Escherichia coli liquid was added, and each was covered with a polyethylene film disinfected with alcohol to make the bacterial liquid evenly dispersed in the membrane layer. All membrane samples were cultured in a 37°C incubator (dark conditions) for 3 hours. In addition, the MAO / SG+ZIF-8 / N-CQDs membrane sample was cultured under simulated sunlight for 3 hours. After the culture was completed, 10 mL of liquid culture medium (nutrient broth) was used to rinse the bacteria on the surface of the polyethylene film and membrane samples into a clean centrifuge tube, and the bacterial liquid washed on the surface of the LA91 substrate was diluted 10 times, and the bacterial liquid washed on the surface of other membrane layers was diluted 102 times. 150 μL of the above diluted bacterial liquid was taken and dispersed in the agar medium, cultured at 37°C for 16 hours, and the number of colonies was counted by taking pictures. Figure 2 As shown. Figure 2 It can be seen that the number of colonies in all film samples is significantly less than that in the LA91 group. Among them, the number of bacteria in the MAO / SG+ZIF-8 / N-CQDs sample is the lowest under light conditions, and the inhibition rate reaches 99.28% ( Figure 3 ), showing excellent antibacterial properties.

[0086] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principles of the present invention. These improvements and modifications should also be regarded as within the scope of protection of the present invention.

Claims

1. Application of a sol-gel composite coating in metal micro-arc oxidation layer protection, characterized in that: The sol-gel composite coating is prepared by a preparation method consisting of the following steps: The zeolite imidazolate framework is mixed with nitrogen-doped carbon quantum dots to obtain a mixture 1; The mixture 1 is sequentially subjected to ultrasonic treatment, washing and vacuum drying to obtain a composite material; The sol-gel A solution, the sol-gel B solution and the composite material are mixed to obtain a mixture 2; The mixture 2 is subjected to an aging treatment to obtain a sol-gel composite coating; The sol-gel liquid A contains anhydrous ethanol, water and trimethoxysilane, and the volume ratio of anhydrous ethanol, water and trimethoxysilane in the sol-gel liquid A is 13-17:5-9:10-14; The sol-gel liquid B contains anhydrous ethanol, ethyl acetoacetate and tetraethoxysilane, and the volume ratio of anhydrous ethanol, ethyl acetoacetate and tetraethoxysilane in the sol-gel liquid B is 1.8-2.2:0.8-1.2:1.8-2.2; Based on the total weight of sol-gel A solution and sol-gel B solution, the addition amount of the composite material is 0.02-0.1wt%; The vacuum drying temperature is 95-110°C; The vacuum drying time is 10 to 14 hours; The aging time is 20 to 30 hours; The nitrogen-doped carbon quantum dots are obtained by a preparation method comprising the following steps: Using citric acid as a carbon source and urea as a nitrogen source, nitrogen-doped carbon quantum dots were prepared by thermal decomposition. The weight ratio of citric acid to urea is 2-4:1; The temperature of the thermal decomposition method is 150-250°C; The time of the thermal decomposition method is 4 to 8 hours; The zeolite imidazolate framework is obtained by a preparation method comprising the following steps: Zn(NO3)2·6H2O was mixed with methanol and 2-methylimidazole and reacted for 0.5-1.5h to obtain a zeolite imidazole ester framework; The mass ratio of Zn(NO3)2·6H2O to the volume ratio of methanol is 1g:8~12mL; The mass ratio of Zn(NO3)2·6H2O to 2-methylimidazole is 1:2-2.

5.

2. A coated substrate, characterized in that The invention comprises a metal substrate treated by micro-arc oxidation and a sol-gel composite coating, wherein the sol-gel composite coating is coated on at least a portion of the metal substrate; The coating is achieved by a dip-coating method; The sol-gel composite coating is prepared by a preparation method consisting of the following steps: The zeolite imidazolate framework is mixed with nitrogen-doped carbon quantum dots to obtain a mixture 1; The mixture 1 is sequentially subjected to ultrasonic treatment, washing and vacuum drying to obtain a composite material; The sol-gel A solution, the sol-gel B solution and the composite material are mixed to obtain a mixture 2; The mixture 2 is subjected to an aging treatment to obtain a sol-gel composite coating; The sol-gel liquid A contains anhydrous ethanol, water and trimethoxysilane, and the volume ratio of anhydrous ethanol, water and trimethoxysilane in the sol-gel liquid A is 13-17:5-9:10-14; The sol-gel liquid B contains anhydrous ethanol, ethyl acetoacetate and tetraethoxysilane, and the volume ratio of anhydrous ethanol, ethyl acetoacetate and tetraethoxysilane in the sol-gel liquid B is 1.8-2.2:0.8-1.2:1.8-2.2; Based on the total weight of sol-gel A solution and sol-gel B solution, the addition amount of the composite material is 0.02-0.1wt%; The vacuum drying temperature is 95-110°C; The vacuum drying time is 10 to 14 hours; The aging time is 20 to 30 hours; The nitrogen-doped carbon quantum dots are obtained by a preparation method comprising the following steps: Using citric acid as a carbon source and urea as a nitrogen source, nitrogen-doped carbon quantum dots were prepared by thermal decomposition. The weight ratio of citric acid to urea is 2-4:1; The temperature of the thermal decomposition method is 150-250°C; The time of the thermal decomposition method is 4 to 8 hours; The zeolite imidazolate framework is obtained by a preparation method comprising the following steps: Using Zn(NO3)2·6H2O as metal salt, the zeolite imidazole ester framework is prepared by hydrothermal method, solvothermal method, solvent azeotropic method or microwave method; The zeolite imidazolate framework is obtained by a preparation method comprising the following steps: Zn(NO3)2·6H2O was mixed with methanol and 2-methylimidazole and reacted for 0.5-1.5h to obtain a zeolite imidazole ester framework; The mass ratio of Zn(NO3)2·6H2O to the volume ratio of methanol is 1g:8~12mL; The mass ratio of Zn(NO3)2·6H2O to 2-methylimidazole is 1:2-2.5.