Negative electrode material and preparation method thereof, and lithium ion battery
By introducing Mg, Ca and Cu elements into the silicon-based anode material, heat treatment and carbon coating, the problems of low conductivity and poor circulation performance are solved, and the electrochemical performance of lithium-ion batteries is improved.
Patent Information
- Application Number
- CN202311830608.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-12-27
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2043-12-27
AI Technical Summary
The low conductivity and poor circulation performance of silicon-based anode materials in lithium-ion batteries limit their commercial applications.
Mg, Ca and Cu elements are introduced into the silicon-based negative electrode material, and the element ratio and particle size distribution are controlled through heat treatment and carbon coating treatment to form active substances with excellent structural stability, improving conductivity and cycling performance.
The first Coulomb efficiency, conductivity and cycling performance of the negative electrode material are significantly improved, the consumption of silicon oxide on lithium is reduced, and the structural stability and electrical contact effect are enhanced.
Smart Images

Figure CN117747802B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of lithium batteries, and in particular to negative electrode materials and preparation methods thereof, and lithium ion batteries. Background Art
[0002] Silicon-based negative electrode materials have the highest lithium storage capacity and lower voltage platform, and are one of the hot spots in the research of negative electrode materials for lithium-ion batteries. However, the huge volume expansion rate (>300%) and low conductivity of silicon materials limit their commercial application. The theoretical capacity of SiO is lower than that of silicon, but the strength of Si-O bond is twice that of Si-Si bond, and the Li2O compound generated during the first cycle of reaction has a buffering effect on volume expansion, so its cycle performance is much better than that of silicon, but at the same time, too much Li2O will increase the consumption of Li ions in the positive electrode material during the first charge, thereby increasing the irreversible capacity of the material and reducing the first coulombic efficiency.
[0003] In the prior art, some reducing Mg elements are doped into silicon-based negative electrode materials, and the three elements Si, O, and Mg in the negative electrode materials are evenly distributed to increase the irreversible capacity of the negative electrode materials. However, although the first coulombic efficiency of the silicon-based negative electrode materials thus prepared has been improved to a certain extent, they still have the problems of low conductivity and poor cycle performance. Summary of the invention
[0004] The present application provides a negative electrode material and a preparation method thereof, and a lithium-ion battery, which are beneficial to comprehensively improve the first coulombic efficiency, electrical conductivity and cycle performance of the negative electrode material.
[0005] In a first aspect, an embodiment of the present application provides a negative electrode material, wherein the negative electrode material includes an active substance, wherein the active substance includes Si element, O element and metal M element, wherein the metal M includes Mg, Ca and Cu;
[0006] In the negative electrode material, the mass content of Mg element is m Mg , the mass content of Ca element m Ca , the mass content of Cu element is m Cu , 0<m Ca / m Mg <0.1,0<m Cu / m Mg <0.01.
[0007] In some embodiments, in the active material, the Mg element, the Ca element, and the Cu element are uniformly distributed.
[0008] In some embodiments, in the negative electrode material, 0<m Mg <25%.
[0009] In some embodiments, in the negative electrode material, 0<m Ca <10%.
[0010] In some embodiments, in the negative electrode material, 0<m Cu <0.5%.
[0011] In some embodiments, the mass content of silicon in the negative electrode material is 24% to 36%.
[0012] In some embodiments, the mass content of oxygen in the negative electrode material is 44% to 59%;
[0013] In some embodiments, in the active material, the Si element exists in the form of silicon single substance and / or silicon oxide, and the Si crystallite size in the silicon single substance and / or the silicon oxide is ≤15 nm.
[0014] In some embodiments, in the active material, the Si element exists in the form of at least one of amorphous silicon, crystalline silicon, silicon oxide, silicon alloy, and a composite of crystalline silicon and amorphous silicon.
[0015] In some embodiments, the active material includes silicon oxide, and the general formula of the silicon oxide is SiOx, 0<x≤2.
[0016] In some embodiments, the metal M exists in the form of at least one of a silicate of M, an oxide of M, and a metal compound of M.
[0017] In some embodiments, the active material includes silicon, silicon oxide, calcium silicate, magnesium silicate, and copper silicide.
[0018] In some embodiments, the negative electrode material further includes a carbon material, and the carbon material is located on at least a portion of the surface of the active material.
[0019] In some embodiments, the carbon material includes at least one of graphite, graphene, amorphous carbon, diamond-like carbon, carbon nanotubes, and carbon fibers.
[0020] In some embodiments, the carbon material forms a carbon layer on the surface of the active material.
[0021] In some embodiments, the carbon layer has a thickness of 50 nm to 200 nm.
[0022] In some embodiments, the mass content of carbon in the negative electrode material is 1%-20%.
[0023] In some embodiments, the pH value of the negative electrode material is 8-10.
[0024] In some embodiments, the average particle size D50 of the negative electrode material is 1 μm to 100 μm.
[0025] In some embodiments, the specific surface area of the negative electrode material is 1 m 2 / g~120m 2 / g.
[0026] In a second aspect, the present application also proposes a method for preparing a negative electrode material, the preparation method comprising the following steps:
[0027] The raw material of the silicon-based active particles is mixed with a metal doping source containing an M element and subjected to heat treatment. The steam formed is mixed and then cooled to obtain an active material. The negative electrode material includes the active material. The active material includes Si element, O element and metal M element. The metal M includes Mg, Ca and Cu. In the negative electrode material, the mass content of Mg element is m Mg , the mass content of Ca element m Ca , the mass content of Cu element is m Cu , 0<m Ca / m Mg <0.1,0<m Cu / m Mg <0.01.
[0028] In some embodiments, the mass ratio of the metal doping source to the raw material of the silicon-based active particles is (1-35):100.
[0029] In some embodiments, the metal doping source includes at least one of a simple substance of metal M and a compound containing metal M.
[0030] In some embodiments, the raw material of the silicon-based active particles includes at least one of Si, a mixture of SiOy and SiO2, a mixture of SiOy and Si, and a mixture of Si and SiO2, wherein 0<y<2.
[0031] In some embodiments, the molar amount of the M element in the metal doping source is n M The molar amount of Si in the raw material of the silicon-based active particles is n Si , and n M :n Si =(0.02~0.62):1.
[0032] In some embodiments, the molar amount of the M element in the metal doping source is n M , 0<n Ca / n Mg <1.8,0<n Cu / n Mg <0.3.
[0033] In some embodiments, the heat treatment includes heating and keeping the mixture of the raw material of the silicon-based active particles and the metal doping source in a negative pressure environment.
[0034] In some embodiments, the vacuum degree of the negative pressure environment is 0.001Pa-100Pa.
[0035] In some embodiments, the heating temperature is 1100°C-1600°C.
[0036] In some embodiments, the insulation time is 4h-30h.
[0037] In some embodiments, the cooling temperature is ≤ 100°C.
[0038] In some embodiments, the method further comprises: subjecting the cooled active material to carbon coating to obtain a negative electrode material.
[0039] In some embodiments, the carbon coating treatment includes any one of a gas phase carbon coating treatment, a liquid phase carbon coating treatment, or a solid phase carbon coating treatment.
[0040] In some embodiments, the coating material used in the carbon coating treatment is a carbon material, and the carbon material includes at least one of graphite, graphene, amorphous carbon, diamond-like carbon, carbon nanotubes and carbon fibers.
[0041] In some embodiments, the carbon coating has a coating thickness of 50 nm to 200 nm.
[0042] In some embodiments, the mass content ratio of the carbon material to the active substance is (1-20):(80-99).
[0043] In some embodiments, the preparation method further comprises pulverizing and / or classifying the active substance obtained by cooling.
[0044] In some embodiments, the pulverization process is carried out by a method of ball milling, air flow pulverization, crushing or spheroidization.
[0045] In some embodiments, in the classification process, the average particle size D50 of 1 μm to 100 μm and the specific surface area of 1 m 2 / g~120m 2 / g of material.
[0046] In some embodiments, the active material obtained by cooling is subjected to pulverization treatment and classification treatment in sequence.
[0047] In a third aspect, the present application further proposes a lithium-ion battery, comprising the negative electrode material as described above, or comprising the negative electrode material prepared by the preparation method as described above.
[0048] Compared with the prior art, this technical solution has at least the following technical effects:
[0049] In the negative electrode material of the present application, by introducing Mg, Ca and Cu elements into the active material and limiting the ratio of Mg, Ca and Cu elements within an appropriate range, the first coulombic efficiency, electrical conductivity and cycle performance of the negative electrode material are comprehensively improved. In the present application, the introduced Mg and Ca elements are beneficial to reducing the content of silicon oxide in the negative electrode material, so that the amount of lithium that can be consumed by the silicon oxide in the negative electrode material can be reduced, thereby improving the first coulombic efficiency of the negative electrode material; and, the introduced Mg and Ca elements with an appropriate mass content ratio exist in the negative electrode material in the form of magnesium silicate and calcium silicate, and the stability of calcium silicate is better than that of magnesium silicate. Compared with a single magnesium silicate, the co-existence of magnesium silicate and calcium silicate in an appropriate ratio can further improve the structural stability of the negative electrode material, and can make the negative electrode sheet of the battery made of the negative electrode material still maintain a high electrical conductivity after long-term charging and discharging, that is, the cycle performance of the negative electrode material is improved; in addition, the introduced Cu element with an appropriate content can be combined with the Si element to exist in the form of copper silicide, and an appropriate amount of copper silicide has good conductivity and ductility, which can enhance the structural stability and electrical contact effect of the negative electrode material, thereby further improving the cycle performance and electrical conductivity of the negative electrode material.
[0050] In the preparation method of the present application, by doping appropriate amounts of Mg, Ca and Cu into silicon-based active particles during the preparation of the active material of the negative electrode material, the ratio of Ca and Cu to Mg in the final negative electrode material is controlled within an ideal range, thereby enabling the prepared negative electrode material to have a higher first coulombic efficiency, higher electrical conductivity, better cycle performance and faster lithium insertion and extraction rate. In the technical solution of the present application, the introduced Mg and Ca elements react with the silicon oxide in the silicon-based active particles to generate elemental silicon, which is beneficial to reduce the content of silicon oxide in the negative electrode material, so that the amount of lithium that can be consumed by the silicon oxide in the negative electrode material can be reduced, thereby improving the first coulomb efficiency of the negative electrode material; and, after reducing the silicon in the silicon oxide, the introduced Mg and Ca elements will also react with the silicon oxide to generate corresponding magnesium silicate and calcium silicate, and the stability of the calcium silicate is better than that of the magnesium silicate. Compared with a single magnesium silicate, the co-existence of magnesium silicate and calcium silicate in an appropriate ratio can further improve the structural stability of the negative electrode material, and can make the negative electrode sheet of the battery made of the negative electrode material still maintain a high conductivity after long-term charging and discharging, that is, the cycle performance of the negative electrode material is improved; in addition, the introduced Cu element will further react with the generated elemental silicon to generate a copper-silicon compound, which reduces the amount of free silicon in the negative electrode material, enhances the structural stability of the negative electrode material and the electrical contact effect between the negative electrode material particles, thereby further improving the cycle performance and conductivity of the negative electrode material. BRIEF DESCRIPTION OF THE DRAWINGS
[0051] The present invention is further described below in conjunction with the accompanying drawings and embodiments:
[0052] Figure 1 This is a diagram of the preparation process of the negative electrode material of this application. DETAILED DESCRIPTION
[0053] In order to better understand the technical solution of the present invention, the embodiments of the present invention are described in detail below with reference to the accompanying drawings.
[0054] It should be clear that the described embodiments are only some embodiments of the present invention, not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0055] The terms used in the embodiments of the present invention are only for the purpose of describing specific embodiments, and are not intended to limit the present invention. The singular forms "a", "said" and "the" used in the embodiments of the present invention and the appended claims are also intended to include plural forms, unless the context clearly indicates other meanings.
[0056] It should be understood that the term "and / or" used in this article is only a description of the association relationship of associated objects, indicating that there can be three relationships. For example, A and / or B can represent: A exists alone, A and B exist at the same time, and B exists alone. In addition, the character " / " in this article generally indicates that the associated objects before and after are in an "or" relationship.
[0057] In the prior art, some reducing Mg elements are doped into silicon-based negative electrode materials, and the three elements Si, O, and Mg in the negative electrode materials are evenly distributed to increase the irreversible capacity of the negative electrode materials. However, although the first coulombic efficiency of the silicon-based negative electrode materials thus prepared has been improved to a certain extent, they still have the problems of low conductivity and poor cycle performance.
[0058] In this regard, technical personnel in this field have also tried to comprehensively improve the conductivity and cycle performance of the negative electrode material by adjusting the content distribution of each element in the negative electrode material, but the above technical problems have not been solved. The main reason is that the elements in the negative electrode material are interrelated and synergistic with each other, and jointly affect the comprehensive performance of the material. As for the influence of multiple parameters, it is difficult to obtain the appropriate control range of each parameter in the product through simple experimental means.
[0059] In response to the above technical problems, in the first aspect, the present application proposes a negative electrode material.
[0060] In the embodiment of the present application, the negative electrode material includes an active substance, the active substance includes Si element, O element, C element and metal M element, the metal M includes Mg, Ca and Cu; in the negative electrode material, the mass content of Mg element is m Mg , the mass content of Ca element m Ca , the mass content of Cu element is m Cu , 0<m Ca / m Mg <0.1,0<m Cu / m Mg <0.01.
[0061] In the negative electrode material of the present application, by introducing Mg, Ca and Cu elements into the active material and limiting the ratio of Mg, Ca and Cu elements within an appropriate range, the first coulombic efficiency, electrical conductivity and cycle performance of the negative electrode material are comprehensively improved. In the present application, the introduced Mg and Ca elements are beneficial to reducing the content of silicon oxide in the negative electrode material, so that the amount of lithium that can be consumed by the silicon oxide in the negative electrode material can be reduced, thereby improving the first coulombic efficiency of the negative electrode material; and, the introduced Mg and Ca elements with an appropriate mass content ratio exist in the negative electrode material in the form of magnesium silicate and calcium silicate, and the stability of calcium silicate is better than that of magnesium silicate. Compared with a single magnesium silicate, the co-existence of magnesium silicate and calcium silicate in an appropriate ratio can further improve the structural stability of the negative electrode material, and can make the negative electrode sheet of the battery made of the negative electrode material still maintain a high electrical conductivity after long-term charging and discharging, that is, the cycle performance of the negative electrode material is improved; in addition, the introduced Cu element with an appropriate content can be combined with the Si element to exist in the form of copper silicide, and an appropriate amount of copper silicide has good conductivity and ductility, which can enhance the structural stability and electrical contact effect of the negative electrode material, thereby further improving the cycle performance and electrical conductivity of the negative electrode material.
[0062] In the negative electrode material of the present application, m Ca / m Mg Specifically, it can be 0.01, 0.02, 0.03, 0.04, 0.05, 0.06, 0.07, 0.08, 0.09, 0.099, etc. Of course, it can also be other values within the above range, which are not limited here. Ca / m Mg The value of is limited to the above range, and the size of silicon microcrystals generated by silicon oxide reaction can be controlled within 15nm or less; when m Ca / m Mg When the value is too large, the reaction between Ca and silicon oxide will be more violent, and a large amount of heat will be released during the reaction, which will cause the generated Si grains to be larger, thereby resulting in poor cycle performance of the negative electrode material.
[0063] In the negative electrode material of the present application, m Cu / m Mg Specifically, it can be 0.001, 0.002, 0.003, 0.004, 0.005, 0.006, 0.007, 0.008, 0.009, 0.0099, etc. Of course, it can also be other values within the above range, which are not limited here. When the mass content ratio of the Cu element to the Mg element is too large, the amount of copper silicide generated will also be too much, and too much copper silicide will cause the capacity of the material to decrease.
[0064] In some embodiments, in the active material, Si element, O element, Mg element, Ca element and Cu element are uniformly distributed, which is beneficial to improving the structural stability of the negative electrode material, thereby being more beneficial to improving the cycle performance of the negative electrode material.
[0065] In some embodiments, in the negative electrode material, 0<m Mg <25%,m Mg Specifically, it can be 0.01%, 1%, 5%, 10%, 15%, 20%, 24.99%, etc. Of course, it can also be other values within the above range, which are not limited here. Mg The value of is limited to the above range, which is beneficial to improving the cycle performance and conductivity of the negative electrode material while maintaining the capacity of the negative electrode material without being greatly affected.
[0066] In some embodiments, in the negative electrode material, 0<m Ca <10%,m Ca Specifically, it can be 0.01%, 1%, 2%, 4%, 6%, 8%, 9.99%, etc. Of course, it can also be other values within the above range, which is not limited here.
[0067] In some embodiments, in the negative electrode material, 0<m Cu <0.5%,m Cu Specifically, it can be 0.01%, 0.1%, 0.2%, 0.3%, 0.4%, 0.499%, etc. Of course, it can also be other values within the above range, which is not limited here.
[0068] In some embodiments, the mass content of silicon in the negative electrode material is 24% to 36%, specifically 24%, 28%, 30%, 32%, 34%, 36%, etc., and of course other values within the above range, which are not limited here.
[0069] In some embodiments, the mass content of oxygen in the negative electrode material is 44% to 59%, specifically 44%, 48%, 50%, 53%, 55%, 57%, 59, etc., and of course other values within the above range, which are not limited here.
[0070] In some embodiments, in the active material, the Si element exists in the form of silicon single substance and / or silicon oxide, and the size of Si crystallites in the silicon single substance and / or silicon oxide is ≤15 nm.
[0071] In some embodiments, in the active material, the Si element exists in the form of at least one of amorphous silicon, crystalline silicon, silicon oxide, silicon alloy, and a composite of crystalline silicon and amorphous silicon.
[0072] In some embodiments, the active material includes silicon oxide, and the general formula of the silicon oxide is SiOx, 0.5≤x<2.
[0073] In some embodiments, the metal M exists in the form of at least one of a silicate of M, an oxide of M, and a metal compound of M.
[0074] In some embodiments, the active material includes silicon, silicon oxide, calcium silicate, magnesium silicate, and copper silicide.
[0075] In some embodiments, the active material further includes copper.
[0076] In some embodiments, the negative electrode material further includes a carbon material, and the carbon material is located on at least a portion of the surface of the active material.
[0077] In some embodiments, the carbon material includes at least one of graphite, graphene, amorphous carbon, diamond-like carbon, carbon nanotubes, and carbon fibers.
[0078] In some embodiments, the carbon material forms a carbon layer on the surface of the active material.
[0079] In some embodiments, the carbon layer covers the active material, which can effectively reduce the volume expansion rate of the negative electrode material.
[0080] In some embodiments, the thickness of the carbon layer is 50nm-200nm, specifically 50nm, 80nm, 110nm, 140nm, 170nm, 200nm, etc., and of course, it can also be other values within the above range, which are not limited here. By limiting the thickness of the carbon layer to the above range, the carbon layer can completely cover the active material to prevent the active material from directly contacting the electrolyte and repeatedly generating an unstable SEI film, thereby causing excessive consumption of the electrolyte and a decrease in the cycle performance of the material, and the carbon layer will not be easily cracked due to the internal particle stress due to the excessive thickness of the carbon layer.
[0081] In some embodiments, the mass content of carbon in the negative electrode material is 1% to 20%, specifically 1%, 4%, 8%, 12%, 16%, 20%, etc., and of course other values within the above range, which are not limited here.
[0082] In some embodiments, the pH value of the negative electrode material is 8-10, specifically 8.00, 8.50, 9.00, 9.50, 10, etc., and of course, it can also be other values within the above range, which is not limited here.
[0083] In some embodiments, the average particle size D50 of the negative electrode material is 1 μm to 100 μm, specifically 1 um, 10 um, 20 um, 40 um, 60 um, 80 um or 100 um, etc., and of course, it can also be other values within the above range, which is not limited here.
[0084] In some embodiments, the specific surface area of the negative electrode material is 1 m 2 / g~120m 2 / g, specifically 1m 2 / g, 10m 2 / g, 20m 2 / g, 40m 2 / g, 6m 2 / g, 80m 2 / g、100m 2 / g or 120m 2 / g, etc., and may of course be other values within the above range, which are not limited here.
[0085] In a second aspect, the present application also proposes a method for preparing a negative electrode material.
[0086] In the embodiment of the present application, the preparation method comprises the following steps:
[0087] S1. The raw material of the silicon-based active particles is mixed with a metal doping source containing an M element and subjected to heat treatment. The steam formed is mixed and then cooled to obtain an active material. The negative electrode material includes the active material. The active material includes Si element, O element and metal M element. The metal M includes Mg, Ca and Cu. In the negative electrode material, the mass content of Mg element is m Mg , the mass content of Ca element m Ca , the mass content of Cu element is m Cu , 0<m Ca / m Mg <0.1,0<m Cu / m Mg <0.01.
[0088] In the preparation method of the present application, by doping appropriate amounts of Mg, Ca and Cu into silicon-based active particles during the preparation of the active material of the negative electrode material, the ratio of Ca and Cu to Mg in the final negative electrode material is controlled within an ideal range, thereby enabling the prepared negative electrode material to have a higher first coulombic efficiency, higher electrical conductivity, better cycle performance and faster lithium insertion and extraction rate. In the technical solution of the present application, the introduced Mg and Ca elements react with the silicon oxide in the silicon-based active particles to generate elemental silicon, which is beneficial to reduce the content of silicon oxide in the negative electrode material, so that the amount of lithium that can be consumed by the silicon oxide in the negative electrode material can be reduced, thereby improving the first coulomb efficiency of the negative electrode material; and, after reducing the silicon in the silicon oxide, the introduced Mg and Ca elements will also react with the silicon oxide to generate corresponding magnesium silicate and calcium silicate, and the stability of the calcium silicate is better than that of the magnesium silicate. Compared with a single magnesium silicate, the co-existence of magnesium silicate and calcium silicate in an appropriate ratio can further improve the structural stability of the negative electrode material, and can make the negative electrode sheet of the battery made of the negative electrode material still maintain a high conductivity after long-term charging and discharging, that is, the cycle performance of the negative electrode material is improved; in addition, the introduced Cu element will further react with the generated elemental silicon to generate a copper-silicon compound, which reduces the amount of free silicon in the negative electrode material, enhances the structural stability of the negative electrode material and the electrical contact effect between the negative electrode material particles, thereby further improving the cycle performance and conductivity of the negative electrode material.
[0089] In the preparation method of the present application, m Ca / m Mg Specifically, it can be 0.01, 0.02, 0.03, 0.04, 0.05, 0.06, 0.07, 0.08, 0.09, 0.099, etc. Of course, it can also be other values within the above range, which are not limited here. Ca / m Mg The value of is limited to the above range, and the size of silicon microcrystals generated by silicon oxide reaction can be controlled within 15nm or less; when m Ca / m Mg When the value is too large, the reaction between Ca and silicon oxide will be more violent, and a large amount of heat will be released during the reaction, which will cause the generated Si grains to be larger, thereby resulting in poor cycle performance of the negative electrode material.
[0090] In the preparation method of the present application, m Cu / m MgSpecifically, it can be 0.001, 0.002, 0.003, 0.004, 0.005, 0.006, 0.007, 0.008, 0.009, 0.0099, etc. Of course, it can also be other values within the above range, which are not limited here. When the mass content ratio of the Cu element to the Mg element is too large, the amount of copper silicide generated will be too much, and too much copper silicide will cause the capacity of the material to decrease.
[0091] In some embodiments, the mass ratio of the metal doping source of the M element to the raw material of the silicon-based active particles is (1-35):100, specifically 1:100, 10:100, 20:100, 30:100, 35:100, etc., and of course it can also be other values within the above range, which is not limited here.
[0092] In some embodiments, the metal doping source includes at least one of a simple substance of metal M and a compound containing metal M.
[0093] In some embodiments, the metal doping source includes a mixture of an oxide containing a metal M and / or a salt containing a metal M and a reducing substance.
[0094] In some embodiments, the reducing salt containing metal M includes at least one of copper, magnesium, or aluminum.
[0095] In some embodiments, the reducing salt containing metal M includes at least one of MgCO3, MgCl2, CaCO3, dolomite, and copper-dyed dolomite.
[0096] In some embodiments, the raw material of the silicon-based active particles includes at least one of Si, a mixture of SiOy and SiO2, a mixture of SiOy and Si, and a mixture of Si and SiO2, wherein 0<y<2.
[0097] In some embodiments, the molar amount of the M element in the metal doping source is n M , 0<n Ca / n Mg <1.8,0<n Cu / n Mg By limiting the molar content ratio of calcium and copper to magnesium in the metal doping source to the above range, it is possible to ensure that the mass content ratio of calcium and copper to magnesium in the active material in the prepared negative electrode material satisfies: 0 < m Ca / m Mg <0.1,0<m Cu / m Mg <0.01.
[0098] In some embodiments, the molar amount of the M element in the metal doping source is n MThe molar amount of Si in the raw material of the silicon-based active particles is n Si , and n M :n Si =(0.02-0.62):1, specifically 0.02:1, 0.1:1, 0.2:1, 0.4:1, 0.62:1 or any ratio therebetween; by limiting the molar ratio of the M element in the metal doping source to the silicon element in the raw material of the silicon-based active particles within the above range, the first coulombic efficiency, electrical conductivity and cycle performance of the prepared negative electrode material can be comprehensively improved to the greatest extent.
[0099] In some embodiments, the heat treatment includes heating and keeping the mixture of the raw material of the silicon-based active particles and the metal doping source in a negative pressure environment.
[0100] In some embodiments, the vacuum degree of the negative pressure environment is 0.001 Pa-100 Pa, specifically 0.001, 10, 40, 60, 80, 100 or any value therebetween.
[0101] In some embodiments, the heating temperature is 1100° C.-1600° C., specifically 1100° C., 1200° C., 1300° C., 1400° C., 1500° C. or any value therebetween.
[0102] In some embodiments, the insulation time is 4 h-30 h, specifically 4 h, 12 h, 20 h, 25 h, 30 h or any value therebetween.
[0103] In some embodiments, the cooling temperature is ≤ 100°C.
[0104] In some embodiments, the method further comprises pulverizing and / or classifying the active material obtained by cooling.
[0105] In some embodiments, the pulverization process is carried out by a method of ball milling, air flow pulverization, crushing or spheroidization.
[0106] In some embodiments, during the classification process, materials having an average particle size D50 of 1 to 100 μm and a specific surface area of 1 to 120 m 2 / g are selected.
[0107] In some embodiments, the active material obtained by cooling is firstly pulverized and then classified.
[0108] In some embodiments, the method further comprises: performing carbon coating treatment on the active material obtained by cooling to obtain a negative electrode material.
[0109] In some embodiments, the active material obtained by cooling is subjected to pulverization, classification and coating treatments in sequence.
[0110] In some embodiments, the carbon coating process includes any one of a gas phase carbon coating process, a liquid phase carbon coating process, or a solid phase carbon coating process.
[0111] In some embodiments, the coating material used in the carbon coating treatment is a carbon material, and the carbon material includes at least one of graphite, graphene, amorphous carbon, diamond-like carbon, carbon nanotubes and carbon fibers.
[0112] In some embodiments, the coating thickness of the carbon coating treatment is 50 nm-200 nm, specifically 50 nm, 100 nm, 150 nm, 200 nm or any value therebetween.
[0113] In some embodiments, the mass content ratio of carbon material to active substance is (1-20):(80-99), specifically 1:99, 1:80, 5:80, 10:80, 15:80, 20:80 or any ratio therebetween.
[0114] In a third aspect, the present application also proposes a lithium-ion battery, which includes the negative electrode material as described above, or the lithium-ion battery includes the negative electrode material prepared by the preparation method as described above. The lithium-ion battery proposed in the present application has the characteristics of high first coulombic efficiency, high conductivity and excellent cycle performance.
[0115] The following is a further description of the embodiments of the present application in multiple embodiments. The embodiments of the present application are not limited to the following specific embodiments. Within the scope of the unchanged main rights, appropriate changes can be made to the implementation.
[0116] Example 1
[0117] Preparation of negative electrode materials
[0118] (1) Preparation of active material: 5 kg SiO, 0.48 kg Mg, 0.2 kg Ca and 0.01 kg Cu were mixed for 30 min and then put into a vacuum furnace. The mixture was heated to 1350°C under vacuum conditions to generate SiO vapor, Mg vapor, Ca vapor and Cu vapor in the furnace. The vapors were mixed evenly and condensed to obtain 4 kg active material.
[0119] (2) Powdering: 3 kg of the active material obtained in the above (1) was crushed, ball-milled, classified, etc., and its average particle size D50 was controlled to be about 4 μm.
[0120] (3) Carbon coating treatment: The active material after the powderization treatment in the above (2) is placed in a CVD furnace, argon gas is introduced as a protective gas from the outside, and acetylene gas is introduced as a carbon source from the inside. The mixture is heated to 800°C to decompose acetylene, and 5% carbon is coated on the surface of the active material to obtain a negative electrode material.
[0121] The negative electrode material prepared in Example 1 was subjected to elemental quantitative analysis using an inductively coupled plasma emission spectrometer. The test results and m calculated based on the test results were Ca / m Mg and m Cu / m Mg As shown in Table 1.
[0122] Furthermore, the electrochemical performance of the negative electrode material prepared in Example 1 was tested. Please refer to Tables 2 and 3 for the test results.
[0123] Example 2
[0124] Preparation of negative electrode materials
[0125] (1) Preparation of active material: 3 kg of silicon powder, 6 kg of SiO2, 6 kg of calcined copper-dyed dolomite and 3 kg of Mg were mixed for 30 min and then put into a vacuum furnace; the mixture was heated to 1350°C under vacuum conditions to generate SiO vapor, Mg vapor, Ca vapor and Cu vapor in the furnace. After the vapors were evenly mixed, they were condensed to obtain 4 kg of active material.
[0126] (2) Powdering: 3 kg of the active material obtained in the above (1) was crushed, ball-milled, classified, etc., and its average particle size D50 was controlled to be about 4 μm.
[0127] (3) Carbon coating treatment: The active material after the powderization treatment in the above (2) is placed in a CVD furnace, argon gas is introduced as a protective gas from the outside, and acetylene gas is introduced as a carbon source from the inside. The mixture is heated to 800°C to decompose acetylene, and 5% carbon is coated on the surface of the active material to obtain a negative electrode material.
[0128] The negative electrode material prepared in Example 2 was subjected to elemental quantitative analysis using an inductively coupled plasma emission spectrometer. The test results and m calculated based on the test results were Ca / m Mg and m Cu / m Mg As shown in Table 1.
[0129] Furthermore, the electrochemical performance of the negative electrode material prepared in Example 2 was tested. Please refer to Table 2 and Table 3 for the test results.
[0130] Example 3
[0131] Preparation of negative electrode materials
[0132] (1) Preparation of active material: 5 kg SiO, 0.5 kg Mg, 0.8 kg Ca and 0.1 kg Cu were mixed for 30 min and then put into a vacuum furnace. The mixture was heated to 1350°C under vacuum conditions to generate SiO vapor, Mg vapor, Ca vapor and Cu vapor in the furnace. After the vapors were evenly mixed, they were condensed to obtain 4 kg of active material.
[0133] (2) Powdering: 3 kg of the active material obtained in the above (1) was crushed, ball-milled, classified, etc., and its average particle size D50 was controlled to be about 4 μm.
[0134] (3) Carbon coating treatment: The active material after the powderization treatment in the above (2) is placed in a CVD furnace, argon gas is introduced as a protective gas from the outside, and acetylene gas is introduced as a carbon source from the inside. The mixture is heated to 800°C to decompose acetylene, and 5% carbon is coated on the surface of the active material to obtain a negative electrode material.
[0135] The negative electrode material prepared in Example 3 was subjected to elemental quantitative analysis using an inductively coupled plasma emission spectrometer. The test results and m calculated based on the test results were Ca / m Mg and m Cu / m Mg As shown in Table 1.
[0136] Furthermore, the electrochemical performance of the negative electrode material prepared in Example 3 was tested. Please refer to Tables 2 and 3 for the test results.
[0137] Example 4
[0138] Preparation of negative electrode materials
[0139] (1) Preparation of active material: 5 kg SiO, 0.5 kg Mg, 0.7 kg Ca and 0.01 kg Cu were mixed for 30 min and then put into a vacuum furnace. The mixture was heated to 1350°C under vacuum conditions to generate SiO vapor, Mg vapor, Ca vapor and Cu vapor in the furnace. After the vapors were evenly mixed, they were condensed to obtain 4 kg of active material.
[0140] (2) Powdering: 3 kg of the active material obtained in the above (1) was crushed, ball-milled, classified, etc., and its average particle size D50 was controlled to be about 4 μm.
[0141] (3) Carbon coating treatment: The active material after the powderization treatment in the above (2) is placed in a CVD furnace, argon gas is introduced as a protective gas from the outside, and acetylene gas is introduced as a carbon source from the inside. The mixture is heated to 800°C to decompose acetylene, and 5% carbon is coated on the surface of the active material to obtain a negative electrode material.
[0142] The negative electrode material prepared in Example 4 was subjected to elemental quantitative analysis using an inductively coupled plasma emission spectrometer. The test results and m calculated based on the test results were Ca / m Mg and m Cu / m Mg As shown in Table 1.
[0143] Furthermore, the electrochemical performance of the negative electrode material prepared in Example 3 was tested. Please refer to Tables 2 and 3 for the test results.
[0144] Example 5
[0145] Preparation of negative electrode materials
[0146] (1) Preparation of active material: 5 kg SiO, 0.5 kg Mg, 1.5 kg Ca and 0.06 kg Cu were mixed for 30 min and then put into a vacuum furnace. The mixture was heated to 1350°C under vacuum conditions to generate SiO vapor, Mg vapor, Ca vapor and Cu vapor in the furnace. The vapors were mixed evenly and condensed to obtain 4 kg active material.
[0147] (2) Powdering: 3 kg of the active material obtained in the above (1) was crushed, ball-milled, classified, etc., and its average particle size D50 was controlled to be about 4 μm.
[0148] (3) Carbon coating treatment: The active material after the powderization treatment in the above (2) is placed in a CVD furnace, argon gas is introduced as a protective gas from the outside, and acetylene gas is introduced as a carbon source from the inside. The mixture is heated to 800°C to decompose acetylene, and 5% carbon is coated on the surface of the active material to obtain a negative electrode material.
[0149] The negative electrode material prepared in Example 5 was subjected to elemental quantitative analysis using an inductively coupled plasma emission spectrometer. The test results and m calculated based on the test results were Ca / m Mg and m Cu / m Mg As shown in Table 1.
[0150] Furthermore, the electrochemical performance of the negative electrode material prepared in Example 5 was tested. Please refer to Table 2 and Table 3 for the test results.
[0151] Example 6
[0152] Preparation of negative electrode materials
[0153] (1) Preparation of active material: 5 kg SiO, 0.48 kg Mg, 0.8 kg Ca and 0.4 kg Cu were mixed for 30 min and then put into a vacuum furnace. The mixture was heated to 1350°C under vacuum conditions to generate SiO vapor, Mg vapor, Ca vapor and Cu vapor in the furnace. After the vapors were evenly mixed, they were condensed to obtain 4 kg of active material.
[0154] The active material prepared in (1) was subjected to elemental quantitative analysis using an inductively coupled plasma emission spectrometer. The test results and m calculated based on the test results were Ca / m Mg and m Cu / m Mg For example, as shown in Table 1.
[0155] (2) Powdering: 3 kg of the active material obtained in the above (1) was crushed, ball-milled, classified, etc., and its average particle size D50 was controlled to be about 4 μm.
[0156] (3) Carbon coating treatment: The active material after the powderization treatment in the above (2) is placed in a CVD furnace, argon gas is introduced as a protective gas from the outside, and acetylene gas is introduced as a carbon source from the inside. The mixture is heated to 800°C to decompose acetylene, and 5% carbon is coated on the surface of the active material to obtain a negative electrode material.
[0157] The negative electrode material prepared in Example 6 was subjected to elemental quantitative analysis using an inductively coupled plasma emission spectrometer. The test results and m calculated based on the test results were Ca / m Mg and m Cu / m Mg As shown in Table 1.
[0158] Furthermore, the electrochemical performance of the negative electrode material prepared in Example 6 was tested. Please refer to Tables 2 and 3 for the test results.
[0159] Comparative Example 1
[0160] The difference from Example 1 is that the raw materials added in step (1) are 5 kg SiO and 0.5 kg Mg.
[0161] Comparative Example 2
[0162] The difference from Example 1 is that the raw materials added in step (1) are 5 kg SiO, 0.5 kg Mg and 0.2 kg Ca.
[0163] Comparative Example 3
[0164] The difference from Example 1 is that the raw materials added in step (1) are 5 kg SiO, 0.5 kg Mg, 0.2 kg Ca and 0.2 kg Cu.
[0165] Comparative Example 4
[0166] The difference from Example 1 is that the raw materials added in step (1) are 5 kg SiO, 0.5 kg Mg, 0.8 kg Ca and 0.01 kg Cu.
[0167] Comparative Example 5
[0168] The difference from Example 1 is that the raw materials added in step (1) are 5 kg SiO, 0.5 kg Mg and 0.6 kg Cu.
[0169] Test method:
[0170] 1. Element content: Use inductively coupled plasma emission spectrometer and oxygen, nitrogen and hydrogen tester to carry out quantitative element analysis of negative electrode materials.
[0171] 2. Powder conductivity: The volume resistivity of the negative electrode material powder is tested by the four-probe method. The resistance of the powder under five pressure points of 4KN, 8KN, 12KN, 16KN and 20KN is tested respectively by the instrument, and then the conductivity and resistivity of the negative electrode material powder are automatically calculated by the computer. The data in Appendix 3 are the conductivity under the pressure of 20KN.
[0172] 3. Electrical performance test:
[0173] Referring to BTRTC / ZY / 01-020 "Button Cell Method Operation Instructions", button cells were assembled; wherein, metal lithium sheets were used as electrodes, and the separator was a PP-PE-PP composite film with a diameter of 19.2 mm; the electrolyte component ratio was EC / EMC / DMC=1 / 1 / 1, and the lithium salt (LiPF6) concentration was 1.05 mol / L.
[0174] (1) Lithium insertion capacity: Under normal temperature conditions, 0.1C constant current charging, the charging voltage is limited to 0.005V~1.5V, and the corresponding capacity is the lithium insertion capacity.
[0175] (2) Lithium removal capacity: Under normal temperature conditions, 0.1C constant current discharge, the discharge voltage is limited to 1.5V ~ 0.005V, and the corresponding capacity is the lithium removal capacity.
[0176] (3) First coulombic efficiency: the ratio of the lithium insertion capacity obtained by the first charge to the lithium removal capacity obtained by the first discharge × 100%.
[0177] (4) Cycle performance: The negative electrode materials prepared in the examples and comparative examples were prepared into batteries and tested using a button battery charging and discharging device. In the first week, the battery was discharged at 0.1C to 0.01V, then discharged at 0.01C in arithmetic descending order to 0.01V, then discharged at 0.01C to 0.005V, and then charged at 0.1C to 1.5V. In the second week, the battery was discharged at 0.2C to 0.01V, then discharged at 0.02C in arithmetic descending order to 0.01V, then discharged at 0.02C to 0.005V, and then charged at 0.2C to 1.5V. In the third week, the battery was discharged at 0.1C to 0.01V, then discharged at 0.01C in arithmetic descending order to 0.01V, then discharged at 0.02C to 0.005V, and then charged at 0.2C to 1.5V. In the first week, the battery was discharged at 0.5C to 0.01V, discharged at 0.05C in an arithmetic decreasing manner to 0.01V, discharged at 0.05C to 0.005V and charged at 0.5C to 1.5V; from the 4th to the 50th week, the battery was discharged at 1C to 0.01V, discharged at 0.1C in an arithmetic decreasing manner to 0.01V, discharged at 0.1C to 0.005V and charged at 1C to 1.5V; in the 51st week, the battery was discharged at 0.1C to 0.01V, discharged at 0.01C in an arithmetic decreasing manner to 0.01V and discharged at 0.01C to 0.005V.
[0178] Test Results
[0179] The element content test results of the negative electrode materials prepared in Examples 1-6 and Comparative Examples 1-5 are shown in Table 1 below:
[0180]
[0181] The electrical performance test results of the negative electrode materials prepared in Examples 1-6 and Comparative Examples 1-5 are shown in Table 2 below:
[0182]
[0183]
[0184] The test results of the conductivity and cycle expansion performance of the negative electrode materials prepared in Examples 1-6 and Comparative Examples 1-5 are shown in Table 3 below:
[0185]
[0186] Combined analysis of Table 1, Table 2 and Table 3:
[0187] By comparing Comparative Examples 1, 2 and 5 with Example 1, it can be seen that, compared with the negative electrode material whose active material contains only one or two of the elements Ca, Mg and Cu, the active material of the negative electrode material of the present application contains three elements of Ca, Mg and Cu at the same time, which is beneficial to reduce the volume expansion rate of the material and improve the ratio of lithium removal capacity to lithium insertion capacity, and can comprehensively improve the first coulomb efficiency, conductivity and cycle performance of the material. Among them, compared with Example 1, although the conductivity of Comparative Example 5 is higher, its cycle expansion rate is also significantly increased, and the application of the negative electrode material is greatly limited. The specific reason is that in Comparative Example 5, mCu / m Mg The increase in the content of copper silicide in the negative electrode material is large, which increases the conductivity of the negative electrode material. Ca / m Mg The decrease makes the ratio of magnesium silicate and calcium silicate in the negative electrode material unbalanced, reduces the structural stability of the negative electrode material, and leads to a significant decrease in the cycle performance of the negative electrode material.
[0188] By comparing Comparative Examples 3-4 with Examples 1-4, it can be seen that when the mass content ratios of calcium element and copper element to magnesium element in the prepared negative electrode material respectively meet the following conditions: 0<m Ca / m Mg <0.1, and 0<m Cu / m Mg When m is less than 0.01, the volume expansion rate of the negative electrode material and the ratio of lithium removal capacity to lithium insertion capacity can be improved, and the initial coulombic efficiency, conductivity and cycle performance of the material can be comprehensively improved, without the situation where one or more of the performances are reduced due to the imbalance of element distribution. Among them, compared with Examples 1-4, although the conductivity of Comparative Example 3 is higher, its cycle expansion rate is also significantly increased, and the application of the negative electrode material is greatly limited. The reason is that in Comparative Example 3, m Cu / m Mg A large increase occurs, which increases the content of copper silicide in the negative electrode material, thereby improving the conductivity of the negative electrode material. However, the lack of calcium element significantly reduces the structural stability of the negative electrode material and significantly increases the cycle expansion rate.
[0189] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the scope of protection of the present invention.
Claims
1. A negative electrode material, characterized in that: The negative electrode material includes an active substance, the active substance includes Si element, O element and metal M element, the metal M includes Mg, Ca and Cu, wherein the Mg element exists in the form of magnesium silicate, and the Ca and Cu exist in the form of metal compounds, and the metal compound includes at least one of metal silicate, metal oxide and silicide; The negative electrode material is tested by inductively coupled plasma emission spectrometry. In the negative electrode material, the mass content of Mg element is m Mg , the mass content of Ca element m Ca , the mass content of Cu element is m Cu , 0<m Ca / m Mg <0.1,0<m Cu / m Mg <0.
01.
2. The negative electrode material according to claim 1, characterized in that The negative electrode material has at least one of the following characteristics (1)-(9): (1) In the active material, Mg, Ca and Cu are uniformly distributed; (2)0<m Mg <25%; (3)0<m Ca <10%; (4)0<m Cu <0.5%; (5) The mass content of silicon in the negative electrode material is 24% to 36%; (6) The mass content of oxygen in the negative electrode material is 44% to 59%; (7) In the active material, the Si element exists in the form of silicon element and / or silicon oxide, and the Si crystallite size in the silicon element and / or silicon oxide is ≤15 nm; (8) In the active material, the Si element exists in the form of at least one of amorphous silicon, crystalline silicon, silicon oxide, silicon alloy, and a composite of crystalline silicon and amorphous silicon; (9) The active material includes silicon oxide, and the general formula of the silicon oxide is SiOx, 0<x≤2.
3. The negative electrode material according to claim 1 or 2, characterized in that: The negative electrode material has at least one of the following characteristics (1)-(8): (1) The negative electrode material further comprises a carbon material, and the carbon material is located on at least a portion of the surface of the active material; (2) The negative electrode material further comprises a carbon material, wherein the carbon material comprises at least one of graphite, graphene, amorphous carbon, diamond-like carbon, carbon nanotubes and carbon fibers; (3) The negative electrode material further includes a carbon material, and the carbon material forms a carbon layer on the surface of the active material; (4) The negative electrode material further includes a carbon material, wherein the carbon material forms a carbon layer on the surface of the active material, and the thickness of the carbon layer is 50 nm to 200 nm; (5) The negative electrode material further comprises a carbon material, and the mass content of carbon in the negative electrode material is 1% to 20%; (6) The pH value of the negative electrode material is 8 to 10; (7) The average particle size D50 of the negative electrode material is 1 μm to 100 μm; (8) The specific surface area of the negative electrode material is 1 m 2 / g~120m 2 / g.
4. A method for preparing a negative electrode material according to any one of claims 1 to 3, characterized in that: The preparation method comprises the following steps: The raw material of silicon-based active particles is mixed with a metal doping source containing an M element and subjected to heat treatment. The generated steam is mixed and then cooled to obtain an active material. The negative electrode material includes the active material.
5. The preparation method according to claim 4, characterized in that: The preparation method comprises at least one of the following features (1)-(5): (1) The mass ratio of the metal doping source to the raw material of the silicon-based active particles is (1-35):100; (2) The metal doping source includes at least one of a simple substance of metal M and a compound containing metal M; (3) The raw material of the silicon-based active particles includes at least one of Si, a mixture of SiOy and SiO2, a mixture of SiOy and Si, and a mixture of Si and SiO2, wherein 0<y<2; (4) The molar amount of the M element in the metal doping source is n M The molar amount of Si in the raw material of the silicon-based active particles is n Si , and n M :n Si = (0.02~0.62): 1; (5) The molar amount of the M element in the metal doping source is n M , 0<n Ca / n Mg <1.8,0<n Cu / n Mg <0.
3.
6. The preparation method according to claim 4, characterized in that: The preparation method has at least one of the following characteristics: (1) The heat treatment comprises placing a mixture of the raw material of the silicon-based active particles and the metal doping source in a negative pressure environment, heating and keeping the mixture warm; (2) The heat treatment comprises placing a mixture of the raw material of the silicon-based active particles and the metal doping source in a negative pressure environment, heating and keeping the mixture warm, wherein the vacuum degree of the negative pressure environment is 0.001 Pa-100 Pa; (3) The heat treatment includes heating and keeping the mixture of the raw material of the silicon-based active particles and the metal doping source in a negative pressure environment, and the heating temperature is 1100° C.-1600° C.; (4) The heat treatment comprises heating and keeping the mixture of the raw material of the silicon-based active particles and the metal doping source in a negative pressure environment, and the keeping time is 4 hours to 30 hours; (5) The cooling temperature is below 100°C.
7. The preparation method according to claim 4, characterized in that: The method further comprises: performing carbon coating treatment on the active material obtained by cooling to obtain a negative electrode material.
8. The preparation method according to claim 7, characterized in that: The preparation method has at least one of the following characteristics (1) to (4): (1) The carbon coating treatment includes any one of a gas phase carbon coating treatment, a liquid phase carbon coating treatment or a solid phase carbon coating treatment; (2) The coating material used in the carbon coating treatment is a carbon material, and the carbon material includes at least one of graphite, graphene, amorphous carbon, diamond-like carbon, carbon nanotubes and carbon fibers; (3) The coating thickness of the carbon coating treatment is 50nm-200nm; (4) The coating material used in the carbon coating treatment is a carbon material, and the mass content ratio of the carbon material to the active substance is (1-20): (80-99).
9. The preparation method according to claim 4, characterized in that: The preparation method further comprises at least one of the following steps: (1) pulverizing and / or classifying the active material obtained by cooling; (2) pulverizing and / or classifying the active material obtained by cooling, wherein the pulverizing method is a combination of at least one of ball milling, air flow pulverization, crushing or spheroidization; (3) The cooled active material is subjected to a pulverization treatment and / or a classification treatment, wherein in the classification treatment, particles having an average particle size D50 of 1 μm to 100 μm and a specific surface area of 1 m 2 / g~120m 2 / g of material; (4) The active material obtained by cooling is subjected to pulverization and classification treatments in sequence.
10. A lithium ion battery, characterized in that: The negative electrode material comprises the negative electrode material as described in any one of claims 1 to 3, or comprises the negative electrode material prepared by the preparation method as described in any one of claims 4 to 9.