A method for optimizing the mix ratio of high-strength thin-walled lining concrete for temperature control and crack prevention
By optimizing the concrete mix ratio, increasing fly ash and slag powder, adjusting the water-adhesive ratio and using high-performance water reducing agents, the problem of temperature crack prevention and control of prestressed concrete lining in tunnels is solved, and the insulation temperature rise and the durability are achieved. effect.
Patent Information
- Application Number
- CN202310610165.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-25
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2043-05-25
AI Technical Summary
The temperature crack prevention and control effect of prestressed concrete lining in the tunnel is poor, mainly due to the temperature stress caused by the internal and external temperature difference caused by the cement hydration heat. It is difficult for the prior art to effectively reduce the adiabatic temperature rise and improve durability.
By optimizing the concrete mix ratio, increasing the amount of fly ash and slag powder, adjusting the gel material and water cement ratio, reducing the amount of cement, combining high-performance polycarboxylic acid water reducing agent, designing C50W12F50-grade inner lining concrete, adopting double- The cement hydration heat and adiabatic temperature rise are calculated exponentially, and the maximum admixture dosage is optimized to not exceed 45% to reduce the early adiabatic temperature rise and improve the later strength.
It effectively reduces the adiabatic temperature rise of the tunnel lining concrete, improves compressive strength and durability, reduces early crack risks, meets the temperature control and crack prevention and construction requirements, and meets the maximum dosage requirements of the specifications.
Smart Images

Figure CN117756464B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of concrete mix ratio, and in particular to a method for optimizing the mix ratio of high-strength thin-wall lining concrete for temperature control and crack prevention. Background Art
[0002] Prestressed concrete lining generates prestress in the lining by tensioning the annular anchor cables in the concrete lining, which can effectively make up for the shortcomings of low tensile strength and low ductility of concrete, reduce the thickness of the lining, save materials and excavation, and significantly reduce the project cost. The double-layer composite lining structure is a new type of tunnel lining structure. Its outer lining bears external water and soil pressure, and the inner lining bears internal water pressure, which embodies the new water supply tunnel design concept of "structural integration and functional independence". The outer lining is precast concrete segments, and the inner lining is cast-in-place concrete. The causes of cracks in tunnel lining concrete are relatively complex, and are usually the result of the combined action of multiple unfavorable factors. The crack formation mechanism is mainly that after the lining concrete is poured, due to the heat of cement hydration, the internal temperature of the concrete rises rapidly, forming a large temperature difference between the inside and the outside. During the cooling process of the concrete, the volume shrinkage is constrained by the outer lining segments (or bedrock), resulting in large temperature stress. When the local stress concentration exceeds the instantaneous tensile strength of the concrete at the weak strength domain, it will crack and extend to form cracks. The magnitude of temperature stress is proportional to the temperature difference. The greater the temperature difference between the inside and outside of the concrete, the higher the elastic modulus of the outer lining segment (or bedrock), and the thinner the lining thickness, the easier it is to produce cracks. Therefore, it is a huge challenge to prevent and control temperature cracks in prestressed concrete linings in tunnels. It is necessary to design a concrete mix optimization method to solve the problem of poor temperature control and crack prevention effects. Summary of the invention
[0003] In view of the problems existing in the prior art, the present invention provides a method for optimizing the mix ratio of high-strength thin-wall lining concrete for temperature control and crack prevention.
[0004] To achieve the above purpose, the technical solution adopted by the present invention is as follows:
[0005] A method for optimizing the mix ratio of high-strength thin-wall lining concrete for temperature control and crack prevention comprises the following steps:
[0006] Step 1: Select concrete performance indicators and raw materials; the concrete performance indicators at least include lining concrete working performance, durability and thermal insulation temperature rise sensitivity; the raw materials at least include cement, fly ash, slag powder, admixtures, fine aggregate and coarse aggregate;
[0007] Step 2: Based on the raw materials, the working performance, durability and thermal insulation temperature rise sensitivity of the lining concrete are studied;
[0008] Step 3: According to the research results and the performance of fly ash and slag powder, adjust the amount of gel material and water-binder ratio to achieve the optimal mix ratio.
[0009] Based on the above technical solution, further, the raw materials in step 1 at least include cement, fly ash, slag powder, admixtures, fine aggregate and coarse aggregate.
[0010] Based on the above technical solution, further, the cement is P.O52.5 cement with a specific surface area of 355m 2 / kg, chloride ion content is 0.024%, alkali content is 0.51%, flexural strength at 3d is 5.8MPa, flexural strength at 28d is 8.1MPa, compressive strength at 3d is 32.5MP, and compressive strength at 28d is 58.8MPa.
[0011] Based on the above technical solution, further, the fly ash adopts Class F II, with an activity index of 78%, a chloride ion content of 0.009%, and an alkali content of 0.84%.
[0012] Based on the above technical solution, further, the slag powder is selected from two batches, and the first batch of slag powder has a specific surface area of 519m 2 / kg, S95 grade, chloride ion content is 0.03%, alkali content is 0.30%, 28d activity index is 96%; the second batch of slag powder has a specific surface area of 412m 2 / kg, S95 grade, 28d activity index is 95%.
[0013] Based on the above technical solution, further, the admixture adopts B0Z-300 high-performance polycarboxylic acid water-reducing agent (slow-setting type), with a water reduction rate of 27%, a chloride ion content of 0.02%, an alkali content of 1.64%, and a 28d compressive strength ratio of 159%.
[0014] Based on the above technical solution, further, the fine aggregate is natural river sand with a fineness modulus of 2.9, belonging to zone II medium sand, a chloride ion content of 0.00%, and a non-alkali active aggregate; the coarse aggregate is 5-20 mm artificial crushed stone with a crushing index of 6.2%, and is a non-alkali active aggregate.
[0015] Based on the above technical solution, further, in step 2, the study on working performance and durability is to set the conditions to be met:
[0016] (1) The concrete working performance meets the following conditions: the design slump is 170mm-230mm;
[0017] (2) Durability of concrete structure meets the following conditions: Total alkali content of concrete is less than 2.5 kg / m 3, the maximum chloride ion content is less than 0.06%, the water-binder ratio is not more than 0.40, and the chloride ion diffusion coefficient of the standard 28d concrete specimen is ≤7.0×10 -12 m 2 / s.
[0018] Based on the above technical solution, further, in step 2, the process of studying the thermal insulation temperature rise sensitivity of the lining concrete includes the following steps:
[0019] Step 11: Calculate the cement hydration heat using the double exponential formula, where the calculation formula is:
[0020] Q(τ)=Q 0 (1-exp(-aτ b )); where Q(τ) is the heat of hydration of cement at age τ, in kJ / kg; Q 0 is the final hydration heat of cement, in kJ / kg; a and b are both unknown constants;
[0021] Step 12: Calculate the adiabatic temperature rise of concrete based on the heat of cement hydration; the calculation formula is:
[0022] Where θ(τ) is the adiabatic temperature rise of concrete at age τ, c is the specific heat of concrete, ρ is the density of concrete, W is the amount of cement, F is the amount of admixture, and k is the reduction factor, which is taken as 0.25.
[0023] Based on the above technical solution, further, in step 3, the maximum admixture amount of the optimized composite fly ash and slag powder does not exceed 45%, among which the maximum admixture amount of single fly ash does not exceed 30%, and the maximum admixture amount of single slag powder does not exceed 45%.
[0024] Based on the above technical solution, further, the design performance grade of the tunnel lining concrete is C50W12F50.
[0025] Compared with the prior art, the present invention has the following beneficial effects:
[0026] The present invention can reduce the early concrete insulation temperature rise by optimizing the prestressed concrete mix ratio, adding a certain amount of fly ash and slag powder, and reducing the amount of cement, and is beneficial to the durability of the lined prestressed concrete structure in a humid environment for a long time. When it exceeds a certain range, it is advisable to use the 56d or 90d age strength for design to fully utilize the later strength of the concrete with mineral admixtures. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1 is a flow chart of the method of the present invention;
[0028] Figure 2Schematic diagram of thermal insulation temperature rise of concrete with different admixture dosages in Example 1 of the present invention;
[0029] Figure 3 This is a schematic diagram of adiabatic temperature rise of concrete with different slag powder finenesses according to Example 1 of the present invention;
[0030] Figure 4 This is a schematic diagram comparing the adiabatic temperature rise test value and the fitting value of Example 1 numbered B3-1 of the present invention;
[0031] Figure 5 This is a schematic diagram comparing the adiabatic temperature rise test value and the fitting value of Example 1 numbered B3-2 of the present invention;
[0032] Figure 6 This is a schematic diagram comparing the adiabatic temperature rise test value and the fitting value numbered B3-3 of Example 1 of the present invention;
[0033] Figure 7 This is a schematic diagram comparing the adiabatic temperature rise test value and the fitting value numbered B3-4 of Example 1 of the present invention;
[0034] Figure 8 This is a schematic diagram of the predicted adiabatic temperature rise in the first 60 days according to the fitting formula numbered B3-1 in Example 1 of the present invention;
[0035] Fig. 9 This is a schematic diagram of the predicted adiabatic temperature rise in the first 60 days according to the fitting formula numbered B3-2 in Example 1 of the present invention;
[0036] Fig.10 This is a schematic diagram of the predicted adiabatic temperature rise in the first 60 days according to the fitting formula numbered B3-3 in Example 1 of the present invention;
[0037] Fig.11 This is a schematic diagram of the predicted values of adiabatic temperature rise in the first 60 days according to the fitting formula numbered B3-4 in Example 1 of the present invention. DETAILED DESCRIPTION
[0038] It is worth noting that the raw materials used in the present invention are all common commercially available products, and their sources are not specifically limited.
[0039] The following sources of raw materials are provided for illustrative purposes:
[0040] Example 1
[0041] like Figure 1 As shown, a method for optimizing the mix ratio of high-strength thin-walled lining concrete for temperature control and crack prevention comprises the following steps:
[0042] Step 1: Set concrete performance indicators and raw materials; the concrete performance indicators at least include lining concrete working performance, mechanical properties, durability and thermal insulation temperature rise sensitivity; the tunnel lining concrete design performance grade is C50W12F50;
[0043] Specifically, the raw materials include at least cement, fly ash, slag powder, admixtures, fine aggregate and coarse aggregate. Among them, the cement is P.O52.5 cement with a specific surface area of 355m 2 / kg, chloride ion content of 0.024%, alkali content of 0.51%, 3d flexural strength of 5.8MPa, 28d flexural strength of 8.1MPa, 3d compressive strength of 32.5MP, 28d compressive strength of 58.8MPa. The fly ash is of Class F II, with an activity index of 78%, chloride ion content of 0.009%, and alkali content of 0.84%. The slag powder is selected from two batches, and the specific surface area of the first batch of slag powder is 519m 2 / kg, S95 grade, chloride ion content is 0.03%, alkali content is 0.30%, 28d activity index is 96%; the second batch of slag powder has a specific surface area of 412m 2 / kg, S95 grade, 28d activity index is 95%. The admixture adopts B0Z-300 high-performance polycarboxylate water reducer (slow setting type), with a water reduction rate of 27%, a chloride ion content of 0.02%, an alkali content of 1.64%, and a 28d compressive strength ratio of 159%. The fine aggregate adopts natural river sand, such as the sand in Table 1, with a fineness modulus of 2.9, belonging to the medium sand in Zone II, a chloride ion content of 0.00%, and a non-alkali active aggregate; the coarse aggregate adopts 5-20mm artificial crushed stone, such as the small stone in Table 1, with a crushing index of 6.2%, and a non-alkali active aggregate. Among them, 3d, 28d, etc. correspond to 3 days, 28 days, etc.
[0044] Step 2: Based on the raw materials, the working performance, durability and thermal insulation temperature rise sensitivity of the lining concrete are studied;
[0045] Specifically, when prestressed concrete (water-cement ratio ≤ 0.40) is prepared with ordinary Portland cement, the maximum dosage of fly ash alone shall not exceed 30%, the maximum dosage of slag powder alone shall not exceed 45%, and the maximum dosage of composite admixtures shall not exceed 45%.
[0046] Step 3: According to the research results and the performance of fly ash and slag powder, adjust the amount of gel material and water-binder ratio to achieve the optimal mix ratio.
[0047] Specifically, (1) the concrete working performance meets the conditions: the design slump is 170mm-230mm; (2) the concrete structure durability meets the conditions: the total alkali content of the concrete is less than 2.5kg / m 3, the maximum chloride ion content is less than 0.06%, the maximum water-binder ratio is not more than 0.40, and the chloride ion diffusion coefficient of the standard 28d concrete specimen is ≤7.0×10 -12 m 2 / s.
[0048] Among them, the hydration heat of cement is an important factor affecting the temperature stress of concrete. In fact, there are two main methods for the adiabatic temperature rise of concrete in the temperature field simulation analysis: direct method and indirect method. Among them, the direct method is to directly measure the adiabatic temperature rise using the adiabatic temperature rise test equipment; the indirect method is to first measure the hydration heat of cement, and then calculate the adiabatic temperature rise based on the hydration heat and the specific heat, bulk density and cement dosage of concrete. This method is based on the mix ratio, cement hydration heat, specific heat and bulk density of each component of concrete, and uses the indirect method to calculate the adiabatic temperature rise of concrete of each mix ratio. The sensitivity study process of the adiabatic temperature rise of lining concrete includes the following steps:
[0049] Step 11: Calculate the cement hydration heat using the double exponential formula, where the calculation formula is:
[0050] Q(τ)=Q 0 (1-exp(-aτ b )); where Q(τ) is the heat of hydration of cement at age τ, in kJ / kg; Q 0 is the final hydration heat of cement, in kJ / kg; a and b are both unknown constants, which can be obtained by fitting the test data;
[0051] Step 12: Calculate the adiabatic temperature rise of concrete based on the heat of cement hydration; the calculation formula is:
[0052] Where θ(τ) is the adiabatic temperature rise of concrete at age τ, c is the specific heat of concrete, ρ is the density of concrete, W is the amount of cement, F is the amount of admixture, and k is the reduction factor, which is taken as 0.25.
[0053] Based on the optimization method, four different admixture schemes, B3-1, B3-2, B3-3, and B3-4, were designed (see Table 1 for the test mix ratio). Among them, the fly ash of B3-1, B3-2, B3-3, and B3-4 was 15%, 15%, 20%, and 20% respectively, and the slag powder was 0%, 15%, 20%, and 25% respectively. The total admixture content was within the range of 15%-45, meeting the requirement that the maximum admixture content of the specification should not exceed 45%. By studying the influence of different admixture contents on the performance indicators of concrete insulation temperature rise, mechanical properties, and durability, the mix ratio of the lining prestressed concrete that can meet the design and construction requirements and effectively reduce the insulation temperature rise is selected. In order to study the influence of slag powder fineness on the insulation temperature rise of concrete, two slag powders with different finenesses were selected for the same mix ratio comparison test, see mix ratios B3-3 and B3-3 (A), and the admixture content was adjusted according to workability.
[0054] In order to reduce the hydration heat and adiabatic temperature rise of concrete as much as possible, the concrete cementitious materials are reduced as much as possible on the basis of meeting the working performance and design performance index requirements of pumped concrete. In order to ensure that the compressive strength and working performance of concrete meet the design index and pumping construction requirements, during the mix optimization test, according to the performance characteristics of fly ash and slag powder, the amount of cementitious materials and water-cement ratio are fine-tuned to ensure that the compressive strength of concrete meets the design requirements (concrete mix strength 59.0MPa); by adjusting the amount of admixtures, the slump of concrete is controlled to be basically consistent to meet the pumping construction requirements.
[0055] Table 1 Mix ratio of C50W12F50 prestressed concrete for tunnel lining
[0056]
[0057] Among them, B3-0 is the original design mix ratio, and the test raw materials are not from the same batch as other mix ratios; B3-1, B3-2, B3-3, B3-4 and B3-3 (A) are tested with raw materials from the same batch. Compared with B3-0, the retarding component of the admixture is adjusted, such as adding the water reducer in Table 1; B3-2, B3-3, B3-4 use the measured specific surface area value of 519m 2 / kg of slag powder; B3-3 (A) uses a specific surface area of 412m 2 / kg slag powder.
[0058] The working performance of the tunnel lining C50W12F50 prestressed concrete is shown in Table 2. All concrete mix ratios meet the requirements of pumping construction performance. From the comparison in Table 2, it can be seen that as the total amount of cementitious materials decreases, the water-cement ratio needs to be increased and the amount of admixtures needs to be greatly increased to ensure that the concrete working performance meets the requirements; this also shows that the concrete cementitious material 454kg / m 3When the cementitious material of a single cubic meter of concrete is close to the critical point required for the working performance of pumped concrete, the cementitious material is reduced to 438kg / m 3 The lack of sufficient slurry filling and lubrication between concrete aggregates will not meet the pumping requirements. Comparing B3-3 and B3-3 (A), it can be seen that when the mix ratio is the same, reducing the specific surface area of slag powder will reduce the amount of water reducer required for concrete to achieve workability (slump).
[0059] Table 2 Concrete working performance
[0060]
[0061] The compressive strength, splitting tensile strength and static elastic modulus of C50W12F50 prestressed concrete in the tunnel lining are shown in Table 3.
[0062] Table 3 Mechanical properties of concrete
[0063]
[0064] It can be seen from Table 3 that the compressive strength, splitting tensile strength and static elastic modulus of concrete all show a downward trend with the increase of the total amount of composite admixtures and the decrease of cement content. The downward trend is more obvious at the early age (7d), and the downward trend of 28d, 56d and 90d strength slows down; the law between the compressive strength of concrete is basically consistent with the law of splitting tensile strength and static elastic modulus; generally speaking, it has little effect on the later strength.
[0065] Compared with B3-1 with 15% fly ash alone, the cement content in B3-2, B3-3 and B3-4 gradually decreases, and the admixture content gradually increases. Even if the water-binder ratio is slightly reduced, the compressive strength at the early age still decreases, by about 3.3%-6.3%. This is because the 28d activity of slag powder and fly ash is usually lower than that of cement. However, the gap between the later compressive strength of B3-2, B3-3, B3-4 and B3-1 gradually narrows, and even exceeds B3-1 at 90d. This is because the fine particles in fly ash and slag powder can fully fill part of the pores in the cement and aggregate accumulation system, and the active silica and alumina in fly ash and slag powder react with calcium silicate and calcium hydroxide in cement hydration products to form calcium silicate, calcium sulfoaluminate, etc., which further fill the remaining pores in the concrete to increase the density and improve the pore structure, thus ensuring the development of the later strength of the concrete. The 28d compressive strength of B3-1 and B3-2 concretes can reach the prepared strength, the 56d compressive strength of B3-3 concrete can reach the prepared strength, and the B3-4 concrete can reach the prepared strength at the age of 60d-90d. When the admixture in the concrete exceeds a certain range, it is advisable to use the 56d or 90d strength for design, so as to make full use of the later strength of the concrete with mineral admixtures.
[0066] Comparing B3-3 and B3-3(A), we can see that the specific surface area of slag powder increases from 519m 2 / kg reduced to 412m 2 / kg, the early age (7d) compressive strength of concrete decreased by 10.8%, and the compressive strength from 28d to 90d was not much different.
[0067] The results of durability-related performance indicators such as impermeability grade, frost resistance grade, chloride ion diffusion coefficient, concrete alkali content, chloride ion content, etc. of the tunnel lining C50W12F50 prestressed concrete are shown in Table 4.
[0068] Table 4 Concrete durability related indicators
[0069]
[0070] Among them, the total alkali content and total chloride ion content of concrete in Table 4 are calculated based on the concrete mix ratio and raw material test indicators. It can be seen from Table 4 that the 28d and 56d impermeability grades and 28d frost resistance grades of each mix ratio have reached the design performance index requirements of C50W12F50 prestressed concrete. Among them, the average seepage heights of B3-1, B3-2, B3-3, and B3-4 after the 56d impermeability test are 17mm, 17mm, 18mm, and 16mm respectively. The alkali content of concrete is less than 2.5kg / m 3 , the total chloride ion content is less than 0.06% (design life 100 years), which meets the design requirements.
[0071] The chloride ion diffusion coefficient of B3-0, B3-2 and B3-3 concrete at 28 days (RCM method) is ≤7.0×10 - 12 m 2 / s, all meet the design requirements. By comparison, compared with the original mix ratio B3-0, the chloride ion diffusion coefficient of B3-2 and B3-3 concretes with appropriate amount of fly ash and slag powder is significantly reduced. This is because fly ash and slag powder play a filling role and secondary hydration role in concrete, which can reduce the porosity of concrete, improve the pore structure, effectively improve the density of concrete, and thus improve the durability of concrete. The chloride ion diffusion coefficient is one of the important indicators of concrete durability. The significant reduction of the chloride ion diffusion coefficient of concrete can reflect the improvement of the concrete's anti-permeability performance from the side.
[0072] In addition, adding a certain amount of fly ash and slag powder into the concrete can reduce the amount of cement used, and the total alkali content and chloride ion content of the concrete can be reduced, which is beneficial to the durability of the lined prestressed concrete structure that is in a humid environment for a long time.
[0073] The adiabatic temperature rise test results corresponding to each mix ratio of C50W12F50 prestressed concrete for tunnel lining are shown in Table 5. The adiabatic temperature rise test results are fitted according to the adiabatic temperature rise hyperbolic formula using the least squares method. The hyperbolic expression of the adiabatic temperature rise θ is: θ(τ)=θ0·τ / (n+τ), where θ0 is the final adiabatic temperature rise of concrete, τ is the concrete age, and n is a constant to be determined. The fitting results are shown in Table 5. It can be seen that the goodness of fit (R2) result is very close to 1, and the calculation results of the hyperbolic formula are in good agreement with the experimental values.
[0074] Table 5 Prestressed C50W12F50 concrete insulation temperature rise test results
[0075]
[0076] It can be seen from Table 5 that compared with the original design mix B3-0 with only 15% fly ash, the 1d adiabatic temperature rise of concrete B3-1, B3-2, B3-3, B3-4 and B3-3 (A) are significantly reduced, which may be related to the adjustment of the retarding component of the concrete admixture. Some retarding components of the admixture can prolong the hydration induction period, inhibit the early hydration of cement, prolong the initial setting time of the concrete, and reduce the early hydration heat.
[0077] From Table 5, Figure 2 From the adiabatic temperature rise test results of B3-1, B3-2, B3-3 and B3-4, it can be seen that under the premise of a slight increase or no change in the total amount of cementitious materials, as the total amount of admixtures increases (15%, 30%, 40%, 45%), the amount of cement decreases, and the adiabatic temperature rise of concrete shows a downward trend. The adiabatic temperature rise of B3-4 concrete is the lowest; the early adiabatic temperature rise value decreases significantly, while the later adiabatic temperature rise decreases gradually. Compared with B3-1, the adiabatic temperature rise test values of B3-4 corresponding to the 1d and 10d age concrete are reduced by 5.2℃ and 3.6℃, and the final value of the adiabatic temperature rise fitting is reduced by about 1.7℃. This shows that the use of fly ash and slag powder as an admixture instead of cement can reduce the adiabatic temperature rise of concrete to a certain extent, but has little effect on the later adiabatic temperature rise.
[0078] From Table 5, Figure 3 The adiabatic temperature rise test results of B3-3 and B3-3(A) show that the specific surface area of slag powder increases from about 520m 2 / kg down to about 410m 2 / kg, the adiabatic temperature rise of concrete at 1d and 10d decreased by 1.1℃ and 0.8℃, and the final value of fitting decreased by about 0.5℃, indicating that reducing the specific surface area of slag powder has a certain effect on reducing the early adiabatic temperature rise. Considering that the specific surface area decreases, the activity of slag powder decreases; the mechanical properties of concrete such as compressive strength decrease, and the increase of specific surface area will also increase the early self-shrinkage of concrete. Therefore, considering the pros and cons of slag powder fineness, the fineness of slag powder should be controlled at (450±30)m in actual engineering application. 2 / kg, which is beneficial to reducing the early hydration heat of concrete and making full use of the later strength of mineral admixtures.
[0079] That is, the test results show that with the increase of the amount of fly ash and slag powder added and the decrease of cement content, the early adiabatic temperature rise of concrete and mechanical properties such as compressive strength and splitting tensile strength all show a downward trend. Although the difference between the adiabatic temperature rise and mechanical properties of concrete in the later period is narrowed, given that the reduction of early splitting tensile strength is not conducive to the prevention and control of early cracks in concrete, and the cracking of prestressed concrete in tunnel lining mainly occurs in the early stage, it is necessary to comprehensively consider the influence of early strength and concrete adiabatic temperature rise on temperature control and crack prevention.
[0080] The 28d compressive strength of B3-2 concrete meets the prepared strength, and the 56d compressive strength of B3-3 concrete meets the prepared strength. The concrete working performance and durability meet the design requirements. Considering the design age, mechanical properties, durability, thermal insulation temperature rise and economy of concrete, B3-2 and B3-3 are preliminarily determined as the best mix ratios. The simulation analysis results of temperature control and crack prevention show that the concrete mix ratio of B3-2 or B3-3 is adopted, and the concrete pouring temperature is controlled to be less than 27℃, the water spraying curing is not less than 28d (the curing water temperature is controlled in a step-by-step manner at 40℃-32℃), the hand hole is sealed below the waistline of the tunnel, and the geotextile is laid to reduce the constraints. The concrete crack resistance coefficient has a certain surplus and meets the temperature control and crack prevention requirements.
[0081] Although the dosage of mineral admixtures in B3-2 and B3-3 complies with the provisions of "Ordinary Concrete Mix Design Code" JGJ55-2011, the "Technical Specifications for Fly Ash in Hydraulic Concrete" (DL / T5055-2007) stipulates that when prestressed concrete is prepared with ordinary Portland cement, the maximum dosage of Class F fly ash shall not exceed 15%; the simulation calculation and analysis results of B3-2 and B3-3 under the preliminary temperature control and crack prevention scheme show that compared with B3-3, B3-2 has higher early strength and lower early cracking risk. Therefore, it is recommended to use B3-2 with 15% fly ash and slag powder as the recommended concrete mix.
[0082] When conducting a theoretical analysis of the sensitivity of concrete to adiabatic temperature rise, in order to estimate the adiabatic temperature rise of concrete, the specific heat of concrete is first estimated based on the specific heat of various raw materials and mix ratio. Assume that the specific heat of various raw materials is C i , the mass of various raw materials in unit volume of concrete is W i , then the specific heat of concrete is:
[0083]
[0084] In order to carry out sensitivity analysis of concrete insulation temperature rise parameters, mechanical and thermal performance tests were conducted on four concrete mixes with different proportions. The density and specific heat of various raw materials in concrete are shown in Table 6.
[0085] Table 6 Density and specific heat of raw materials
[0086] Material parameters water cement Fly ash Mineral powder sand stone <![CDATA[Density (kg / m 3 )]]> 1000 3090 2600 2860 2640 2860 Specific heat (kJ / (kg·℃)) 4.187 0.536 0.754 0.84 0.745 0.785
[0087] The concrete mix proportions and properties are shown in Tables 7, 8 and 9.
[0088] Table 7 Prestressed C50W12F50 first-grade concrete mix ratio
[0089]
[0090] Table 8 Concrete durability test results
[0091]
[0092] Table 9 Concrete mechanical properties test results
[0093]
[0094] Using Table 6 and Table 7, according to the formula and The specific heat and final adiabatic temperature rise values of concrete under various mix ratios are calculated and shown in Table 10.
[0095] Table 10 Specific heat and maximum adiabatic temperature rise of prestressed C50 concrete
[0096] Mix ratio number Specific heat (kJ / (kg·℃)) Final adiabatic temperature rise (℃) B3-1 0.957 57.5 B3-2 0.969 52.6 B3-3 0.978 49.7 B3-4 0.983 47.4
[0097] As can be seen from the table, with the reduction of cement dosage and the increase of fly ash and mineral powder, the final adiabatic temperature rise of concrete decreases accordingly. Therefore, in this project, the adiabatic temperature rise of concrete can be reduced by reducing the cement dosage and increasing the fly ash and mineral powder dosage, thereby reducing the concrete temperature stress and avoiding temperature cracks. Since the actual hydration heat parameters of the cement used in the project are not used in the theoretical analysis, the theoretical analysis results may not be consistent with the measured data, but the rules obtained by the theoretical analysis are reasonable and can be used to guide the project.
[0098] The adiabatic temperature rise of concrete can be fitted by hyperbolic, double exponential and composite exponential formulas according to the test data. This section uses the hyperbolic formula to fit the adiabatic temperature rise results obtained from the test to compare with the theoretical analysis. The hyperbolic expression of the adiabatic temperature rise θ is as follows:
[0099] In the formula, θ 0 is the final adiabatic temperature rise of concrete, τ is the age of concrete, and n is an undetermined constant that can be obtained by fitting the experimental data.
[0100] According to the preliminary test results, the adiabatic temperature rise test results of four concrete mix ratios in the first 10 days are shown in Table 11.
[0101] Table 11 Prestressed C50 concrete insulation temperature rise test results
[0102]
[0103] Utilization The least squares method was used to fit the test results in Table 9, and the results are shown in Table 12. As can be seen from the table, with the reduction of cement dosage, the final adiabatic temperature rise of concrete shows a downward trend, which is consistent with the results of theoretical analysis. From the above test results, it can be found that the effect of adding fly ash and mineral powder on reducing the adiabatic temperature rise of early-age concrete in the 0d-3d period is obvious, which is also the key technical problem of controlling early cracks in concrete that must be solved in this test study.
[0104] After 3 days, there is a certain deviation between the adiabatic temperature rise test value and the theoretical calculation value. The effect of fly ash and mineral powder added in the test value on reducing the adiabatic temperature rise of concrete is not obvious. The main reason is that the fineness of the mineral powder used in the test is too large (519m 2 / kg), the fine powder has a certain amount of hydration heat and a fast initial hydration rate, which is quite different from the hydration performance of fly ash. In actual engineering applications, the fineness of the powder can be controlled at 450±30m 2 / kg, which not only reduces the early hydration heat of concrete but also helps to make full use of the later strength of mineral admixtures.
[0105] Table 12 Hyperbolic parameter fitting results of adiabatic temperature rise of prestressed C50 concrete
[0106] serial number <![CDATA[Final adiabatic temperature rise θ 0 (°C)]]> Parameter n B3-1 59.9 0.245 B3-2 59.0 0.306 B3-3 58.6 0.294 B3-4 58.2 0.333
[0107] Comparison of experimental and fitted values of adiabatic temperature rise of concrete with four different mix ratios Figure 4-7 As shown in the figure, it can be seen that the hyperbolic calculation results are in good agreement with the experimental values.
[0108] When the above fitting results are used to predict the adiabatic temperature rise of the four mix proportions in the first 60 days, the results are as follows: Figure 8-11 As shown in the results, it can be seen that at the 60th day, the predicted values of adiabatic temperature rise of the four mix proportions are 59.6℃, 58.7℃, 58.3℃ and 56.9℃ respectively, which is consistent with the change law of the final adiabatic temperature rise, that is, as the amount of cement decreases, the value of adiabatic temperature rise decreases.
[0109] Finally, it should be noted that the above content is only used to illustrate the technical solution of the present invention, rather than to limit the scope of protection of the present invention. Simple modifications or equivalent substitutions of the technical solution of the present invention by ordinary technicians in this field do not deviate from the essence and scope of the technical solution of the present invention.
Claims
1. A method for optimizing the mix ratio of high-strength thin-walled lining concrete for temperature control and crack prevention, characterized in that: The following steps are involved: Step 1: Select concrete performance indicators and raw materials; the concrete performance indicators at least include the working performance, durability and thermal insulation temperature rise sensitivity of the lining concrete; the raw materials at least include water-cement ratio, cement, fly ash, slag powder, admixtures, fine aggregate and coarse aggregate; cement, slag powder and fly ash are used as cementitious materials; The cement is P.O52.5 cement with a specific surface area of 355m 2 / kg, chloride ion content is 0.024%, alkali content is 0.51%, 3d flexural strength is 5.8MPa, 28d flexural strength is 8.1MPa, 3d compressive strength is 32.5MPa, 28d compressive strength is 58.8MPa; The fly ash is of Class F II, with an activity index of 78%, a chloride ion content of 0.009%, and an alkali content of 0.84%; The admixture is a B0Z-300 high-performance polycarboxylate water reducer with a water reduction rate of 27%, a chloride ion content of 0.02%, an alkali content of 1.64%, and a 28d compressive strength ratio of 159%; The slag powder is selected from two batches, and the first batch of slag powder has a specific surface area of 519m 2 / kg, S95 grade, chloride ion content is 0.03%, alkali content is 0.30%, 28d activity index is 96%; the second batch of slag powder has a specific surface area of 412m 2 / kg, S95 grade, 28d activity index is 95%; Step 2: Based on the raw materials, the working performance, durability and thermal insulation temperature rise sensitivity of the lining concrete are studied; Among them, the research on working performance and durability is to set the conditions to meet: (1) The concrete working performance meets the following conditions: the design slump is 170mm-230mm; (2) Durability of concrete structure meets the following conditions: Total alkali content of concrete is less than 2.5 kg / m 3 , the maximum chloride ion content is less than 0.06%, the water-binder ratio is not more than 0.40, and the chloride ion diffusion coefficient of the standard 28d concrete specimen is ≤7.0×10 -12 m 2 / s; Among them, in step 2, the process of studying the sensitivity of lining concrete insulation temperature rise includes the following steps: Step 11: Calculate the cement hydration heat using the double exponential formula, where the calculation formula is: ; In the formula, Cement at the age Heat of hydration at , in kJ / kg; is the final hydration heat of cement, in kJ / kg; a and b are both unknown constants; Step 12: Calculate the adiabatic temperature rise of concrete based on the heat of cement hydration; the calculation formula is: ; In the formula, For concrete at age The adiabatic temperature rise is, c is the specific heat of concrete, is the density of concrete, W is the amount of cement, F is the amount of admixture, k is the reduction coefficient, and ; Step 3: According to the research results and the performance of fly ash and slag powder, adjust the amount of cementitious materials and water-binder ratio to achieve the optimization of the mix ratio; The optimized concrete mix ratio in step 3 is: water-binder ratio is 0.35, fly ash content is 20%, slag powder content is 20%, water reducer content is 1.8%, and water content is 159 kg / m 3 , cement consumption 272kg / m 3 , the amount of fly ash and slag powder is 91kg / m 3 ,Sand dosage: 770kg / m 3 ,Small stone dosage 1024kg / m 3 , water reducing agent dosage 8.17kg / m 3 , the specific surface area of slag powder is 519m 2 / kg, the diffusion of concrete is 525mm, the impermeability grade of 28d and 56d is ≥W12, the frost resistance grade is ≥F50, and the total alkali content is 1.82kg / m 3 , total chloride ion content 0.02%; The concrete pouring temperature is controlled below 27℃, and the water spraying curing is carried out for no less than 28 days. The curing water temperature is controlled in a step-by-step manner between 40℃ and 32℃ to meet the temperature control and crack prevention requirements.
2. The method for optimizing the mix ratio of high-strength thin-walled lining concrete for temperature control and crack prevention according to claim 1 is characterized in that: The fine aggregate is natural river sand with a fineness modulus of 2.9, belonging to zone II medium sand, a chloride ion content of 0.00%, and a non-alkali active aggregate.
3. The method for optimizing the mix ratio of high-strength thin-walled lining concrete for temperature control and crack prevention according to claim 1 is characterized in that: The coarse aggregate is 5-20 mm artificial crushed stone with a crushing index of 6.2%, and is a non-alkali active aggregate.