Lightweight sound insulation mortar and preparation method thereof

By using the formula of porous allophane, sand and inorganic cementitious materials, the problem of insufficient strength of cork particles in existing sound insulation mortar is solved, the sound insulation effect and hardness are improved, the construction needs are met, and the cost is reduced.

CN117800663BActive Publication Date: 2024-10-01中桔(广东)建材科技有限公司
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202311856426.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-12-29
Publication Date
2024-10-01
Estimated Expiration
2043-12-29

AI Technical Summary

Technical Problem

The cork particles used in existing sound insulation mortar have low particle strength and poor sound absorption, and their performance decreases after mixing, making it difficult to meet construction needs.

Method used

Using a formula of porous allophane with sand and inorganic cementitious materials, the porous allophane is prepared and combined with latex powder, maleic anhydride, ethylene acetate, acrylic acid, emulsifiers and moisturizing thickeners to form a lightweight High-quality soundproof mortar to improve soundproofing and maintain hardness.

Benefits of technology

The sound insulation effect and hardness of the sound insulation mortar are improved to meet the construction needs, and due to the wide source of porous materials, the cost is reduced and good sound absorption and storage properties are achieved.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The present application provides a lightweight sound insulation mortar, which comprises, by weight, 40 to 60 parts of porous allophane, 50 to 55 parts of sand, 42 to 45 parts of inorganic gelling materials, 3 to 4 parts of redispersible latex powder, 3.5 to 4.5 parts of maleic anhydride, 41 to 45 parts of vinyl acetate, 4 to 6 parts of acrylic acid, 1 to 3 parts of emulsifier, and 0.6 to 0.7 parts of moisturizing thickener. The preparation method of the porous allophane is to bake the allophane at 800 to 900°C for 2 to 3 hours, then add the above product to a sodium silicate solution and stir for 2 to 3 hours, make holes in the slurry at 200 to 220°C for 50 to 55 hours, and continuously pass nitrogen into the slurry. After the reaction is completed, filter to obtain porous allophane. The lightweight sound insulation mortar of the present application not only improves the sound insulation effect of the sound insulation mortar, but also maintains a good hardness range to meet actual construction needs.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application belongs to the technical field of mortar, and specifically relates to a lightweight sound-insulating mortar and a preparation method thereof. Background Art

[0002] Mortar is a bonding material used for bricklaying in buildings. It is made of a certain proportion of sand and binder (cement, lime paste, clay, etc.) and water. It is also called mortar or mortar. Common mortars include cement mortar, mixed mortar (or cement lime mortar), lime mortar and clay mortar. In recent years, compared with ordinary mortar, modified mortar has the functions of light weight, heat preservation, sound insulation, etc., and has value in energy saving, noise reduction and environmental protection, so that modified mortar has been widely developed as a new green building material. In modified mortar, perlite and vitrified microspheres are often used as modified aggregates to give mortar functions such as heat preservation and sound insulation; but as the construction mortar industry tends to enhance environmental protection, a plan to use solid waste to replace functional aggregates has been proposed. Among them, cork particles are round particles made from wood waste debris, which can be used to replace functional aggregates. However, the cork particles currently used for sound insulation mortar have low particle strength. Although they have a certain effect in increasing absorption, their wood particles have a low hardness, and after stirring, the particles are crushed, resulting in poor absorption effect and reduced mortar performance.

[0003] To this end, we propose a lightweight sound insulation mortar and a preparation method thereof to solve the above problems. Summary of the invention

[0004] The present application provides a lightweight sound insulation mortar, which not only improves the sound insulation effect of the sound insulation mortar, but also maintains a good hardness range to meet actual construction needs.

[0005] The present application provides a lightweight sound-insulating mortar, which comprises, by weight, 40 to 60 parts of porous allophane, 50 to 55 parts of sand, 42 to 45 parts of inorganic gelling materials, 3 to 4 parts of redispersible latex powder, 3.5 to 4.5 parts of maleic anhydride, 41 to 45 parts of vinyl acetate, 4 to 6 parts of acrylic acid, 1 to 3 parts of emulsifier, and 0.6 to 0.7 parts of moisturizing thickener.

[0006] In some embodiments, the preparation method of the porous allophane is to calcine the allophane at 800-900°C for 2-3 hours, then add the above product to a sodium silicate solution and stir for 2-3 hours, make pores in the slurry at 200-220°C for 50-55 hours, and continuously introduce nitrogen into the slurry. After the reaction is completed, filter it to obtain the porous allophane.

[0007] In some embodiments, the chemical formula of the allophane is Al2O3·SiO2·2.5H2O.

[0008] In some embodiments, the circularity of the porous allophane is 0.6-0.8, the circularity of the porous allophane is 0.6-0.8, and the porosity of the porous allophane is 70-80%.

[0009] In some embodiments, the circularity of the porous allophane is 0.7-0.8.

[0010] In some embodiments, the mass ratio of the porous allophane to the sand is 1-1.2.

[0011] A method for preparing a lightweight sound insulation mortar comprises the following steps: Step 1: mixing porous allophane, sand and an inorganic gelling material, then adding deionized water to dilute the mixture into a solution, and drying the mixture at 125° C. to obtain a porous allophane composite slurry;

[0012] Step 2: adding redispersible latex powder, maleic anhydride, vinyl acetate, acrylic acid, emulsifier and moisturizing thickener to the porous allophane composite slurry.

[0013] In some embodiments, the composition includes, by weight, 40 to 60 parts of porous allophane, 50 to 55 parts of sand, 42 to 45 parts of inorganic gelling material, 3 to 4 parts of redispersible latex powder, 3.5 to 4.5 parts of maleic anhydride, 41 to 45 parts of vinyl acetate, 4 to 6 parts of acrylic acid, 1 to 3 parts of emulsifier, and 0.6 to 0.7 parts of moisturizing thickener.

[0014] In some embodiments, the preparation method of the porous allophane is to calcine the allophane at 800-900°C for 2-3 hours, then add the above product to a sodium silicate solution and stir for 2-3 hours, make pores in the slurry at 200-220°C for 50-55 hours, and continuously introduce nitrogen into the slurry. After the reaction is completed, filter it to obtain the porous allophane.

[0015] The lightweight sound insulation mortar provided by the present application not only improves the sound insulation effect of the sound insulation mortar, but also maintains a good hardness range to meet the actual construction needs. Through the voids of the porous allophane, the slurry is effectively filled, the design of the voids is combined with the optimization of the formula of the porous allophane, sand and inorganic gelling materials, not only the void material plays a filling effect, but also because the above-mentioned porous material has a wide source and lower cost, it has a better sound insulation effect. DETAILED DESCRIPTION

[0016] The following will be combined with the specific embodiments of the present application to clearly and completely describe the technical solutions in the embodiments of the present application. Obviously, the described embodiments are only part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of this application.

[0017] The terms used in this application are for the purpose of describing specific embodiments only and are not intended to limit this application. The singular forms of "a", "said" and "the" used in this application and the appended claims are also intended to include plural forms unless the context clearly indicates other meanings. It should also be understood that the term "and / or" used herein refers to and includes any or all possible combinations of one or more associated listed items.

[0018] The present application provides a lightweight sound-insulating mortar, which comprises, by weight, 40 to 60 parts of porous allophane, 50 to 55 parts of sand, 42 to 45 parts of inorganic gelling materials, 3 to 4 parts of redispersible latex powder, 3.5 to 4.5 parts of maleic anhydride, 41 to 45 parts of vinyl acetate, 4 to 6 parts of acrylic acid, 1 to 3 parts of emulsifier, and 0.6 to 0.7 parts of moisturizing thickener.

[0019] In some embodiments, the preparation method of the porous allophane is to calcine the allophane at 800-900°C for 2-3 hours, then add the above product to a sodium silicate solution and stir for 2-3 hours, make pores in the slurry at 200-220°C for 50-55 hours, and continuously introduce nitrogen into the slurry. After the reaction is completed, filter it to obtain the porous allophane.

[0020] In some embodiments, the chemical formula of the allophane is Al2O3·SiO2·2.5H2O.

[0021] In some embodiments, the circularity of the porous allophane is 0.6-0.8.

[0022] In some embodiments, the circularity of the porous allophane is 0.7-0.8.

[0023] In some embodiments, the mass ratio of the porous allophane to the sand is 1-1.2.

[0024] A method for preparing a lightweight sound insulation mortar comprises the following steps: Step 1: mixing porous allophane, sand and an inorganic gelling material, then adding deionized water to dilute the mixture into a solution, and drying the mixture at 125° C. to obtain a porous allophane composite slurry;

[0025] Step 2: adding redispersible latex powder, maleic anhydride, vinyl acetate, acrylic acid, emulsifier and moisturizing thickener to the porous allophane composite slurry.

[0026] In some embodiments, the composition includes, by weight, 40 to 60 parts of porous allophane, 50 to 55 parts of sand, 42 to 45 parts of inorganic gelling material, 3 to 4 parts of redispersible latex powder, 3.5 to 4.5 parts of maleic anhydride, 41 to 45 parts of vinyl acetate, 4 to 6 parts of acrylic acid, 1 to 3 parts of emulsifier, and 0.6 to 0.7 parts of moisturizing thickener.

[0027] In some embodiments, the preparation method of the porous allophane is to calcine the allophane at 800-900°C for 2-3 hours, then add the above product to a sodium silicate solution and stir for 2-3 hours, make pores in the slurry at 200-220°C for 50-55 hours, and continuously introduce nitrogen into the slurry. After the reaction is completed, filter it to obtain the porous allophane.

[0028] The lightweight sound insulation mortar provided by the present application not only improves the sound insulation effect of the sound insulation mortar, but also maintains a good hardness range to meet the actual construction needs. Through the voids of the porous allophane, the slurry is effectively filled, the design of the voids is combined with the optimization of the formula of the porous allophane, sand and inorganic gelling materials, not only the void material plays a filling effect, but also because the above-mentioned porous material has a wide source and lower cost, it has a better sound insulation effect.

[0029] 40-60 parts of porous allophane, 50-55 parts of sand, 42-45 parts of inorganic gelling material, 3-4 parts of redispersible latex powder, 3.5-4.5 parts of maleic anhydride, 41-45 parts of vinyl acetate, 4-6 parts of acrylic acid, 1-3 parts of emulsifier, 0.6-0.7 parts of moisturizing thickener.

[0030] Example 1: 50 parts of porous allophane, 50 parts of sand, 42 parts of inorganic gelling material, 3 parts of redispersible latex powder, 3.5 parts of maleic anhydride, 41 parts of vinyl acetate, 4 parts of acrylic acid, 1 part of emulsifier, 0.6 parts of moisturizing thickener, the preparation method comprises the following steps:

[0031] Step 1: Mix porous allophane, sand and inorganic gelling material, then add deionized water to dilute into a solution, and dry at 125° C. to obtain porous allophane composite slurry;

[0032] Step 2: adding redispersible latex powder, maleic anhydride, vinyl acetate, acrylic acid, emulsifier and moisturizing thickener to the porous allophane composite slurry.

[0033] Example 2: 50 parts of porous allophane, 51 parts of sand, 42 parts of inorganic gelling material, 3 parts of redispersible latex powder, 3.5 parts of maleic anhydride, 41 parts of vinyl acetate, 4 parts of acrylic acid, 1 part of emulsifier, 0.6 parts of moisturizing thickener, the preparation method comprises the following steps:

[0034] Step 1: Mix porous allophane, sand and inorganic gelling material, then add deionized water to dilute into a solution, and dry at 125° C. to obtain porous allophane composite slurry;

[0035] Step 2: adding redispersible latex powder, maleic anhydride, vinyl acetate, acrylic acid, emulsifier and moisturizing thickener to the porous allophane composite slurry.

[0036] Example 3: 50 parts of porous allophane, 52 parts of sand, 42 parts of inorganic gelling material, 3 parts of redispersible latex powder, 3.5 parts of maleic anhydride, 41 parts of vinyl acetate, 4 parts of acrylic acid, 1 part of emulsifier, 0.6 parts of moisturizing thickener, the preparation method comprises the following steps:

[0037] Step 1: Mix porous allophane, sand and inorganic gelling material, then add deionized water to dilute into a solution, and dry at 125° C. to obtain porous allophane composite slurry;

[0038] Step 2: adding redispersible latex powder, maleic anhydride, vinyl acetate, acrylic acid, emulsifier and moisturizing thickener to the porous allophane composite slurry.

[0039] Example 4: 50 parts of porous allophane, 53 parts of sand, 42 parts of inorganic gelling material, 3 parts of redispersible latex powder, 3.5 parts of maleic anhydride, 41 parts of vinyl acetate, 4 parts of acrylic acid, 1 part of emulsifier, 0.6 parts of moisturizing thickener, the preparation method comprises the following steps:

[0040] Step 1: Mix porous allophane, sand and inorganic gelling material, then add deionized water to dilute into a solution, and dry at 125° C. to obtain porous allophane composite slurry;

[0041] Step 2: adding redispersible latex powder, maleic anhydride, vinyl acetate, acrylic acid, emulsifier and moisturizing thickener to the porous allophane composite slurry.

[0042] Example 5: 50 parts of porous allophane, 54 parts of sand, 42 parts of inorganic gelling material, 3 parts of redispersible latex powder, 3.5 parts of maleic anhydride, 41 parts of vinyl acetate, 4 parts of acrylic acid, 1 part of emulsifier, 0.6 parts of moisturizing thickener, the preparation method comprises the following steps:

[0043] Step 1: Mix porous allophane, sand and inorganic gelling material, then add deionized water to dilute into a solution, and dry at 125° C. to obtain porous allophane composite slurry;

[0044] Step 2: adding redispersible latex powder, maleic anhydride, vinyl acetate, acrylic acid, emulsifier and moisturizing thickener to the porous allophane composite slurry.

[0045] Example 6: 50 parts of porous allophane, 60 parts of sand, 42 parts of inorganic gelling material, 3 parts of redispersible latex powder, 3.5 parts of maleic anhydride, 41 parts of vinyl acetate, 4 parts of acrylic acid, 1 part of emulsifier, 0.6 parts of moisturizing thickener, the preparation method comprises the following steps:

[0046] Step 1: Mix porous allophane, sand and inorganic gelling material, then add deionized water to dilute into a solution, and dry at 125° C. to obtain porous allophane composite slurry;

[0047] Step 2: adding redispersible latex powder, maleic anhydride, vinyl acetate, acrylic acid, emulsifier and moisturizing thickener to the porous allophane composite slurry.

[0048] Example 7: 50 parts of porous allophane, 60 parts of sand, 42 parts of inorganic gelling material, 3 parts of redispersible latex powder, 3.5 parts of maleic anhydride, 41 parts of vinyl acetate, 4 parts of acrylic acid, 1 part of emulsifier, 0.6 parts of moisturizing thickener, the preparation method comprises the following steps:

[0049] Step 1: Mix porous allophane, sand and inorganic gelling material, then add deionized water to dilute into a solution, and dry at 125° C. to obtain porous allophane composite slurry;

[0050] Step 2: adding redispersible latex powder, maleic anhydride, vinyl acetate, acrylic acid, emulsifier and moisturizing thickener to the porous allophane composite slurry.

[0051] Comparative Example 1: 50 parts of porous allophane, 49 parts of sand, 42 parts of inorganic gelling material, 3 parts of redispersible latex powder, 3.5 parts of maleic anhydride, 41 parts of vinyl acetate, 4 parts of acrylic acid, 1 part of emulsifier, 0.6 parts of moisturizing thickener, the preparation method comprises the following steps:

[0052] Step 1: Mix porous allophane, sand and inorganic gelling material, then add deionized water to dilute into a solution, and dry at 125° C. to obtain porous allophane composite slurry;

[0053] Step 2: adding redispersible latex powder, maleic anhydride, vinyl acetate, acrylic acid, emulsifier and moisturizing thickener to the porous allophane composite slurry.

[0054] Comparative Example 2: 35 parts of porous allophane, 50 parts of sand, 42 parts of inorganic gelling material, 3 parts of redispersible latex powder, 3.5 parts of maleic anhydride, 41 parts of vinyl acetate, 4 parts of acrylic acid, 1 part of emulsifier, 0.6 parts of moisturizing thickener, the preparation method comprises the following steps:

[0055] Step 1: Mix porous allophane, sand and inorganic gelling material, then add deionized water to dilute into a solution, and dry at 125° C. to obtain porous allophane composite slurry;

[0056] Step 2: adding redispersible latex powder, maleic anhydride, vinyl acetate, acrylic acid, emulsifier and moisturizing thickener to the porous allophane composite slurry.

[0057] The porosity of the porous allophane in Examples 1 to 7 and Comparative Examples 1 and 2 is 70%. The porosity is calculated by N2 adsorption to obtain the void ratio.

[0058] Using a standing sound wave sound absorption meter, the sound absorption coefficient of a sample of 100mm×900mm×50mm is measured: the obtained data are as follows:

[0059] Example Compressive strengthMpa Sound absorption coefficient Example 1 11.0 0.40 Example 2 11.1 0.41 Example 3 11.2 0.42 Example 4 11.3 0.45 Example 5 11.7 0.44 Example 6 11.3 0.43 Example 7 11.4 0.42 Comparative Example 1 10.4 0.38 Comparative Example 2 10.1 0.32

[0060] The present application provides a lightweight sound insulation mortar, which comprises 40 to 60 parts of porous allophane, 50 to 55 parts of sand, 42 to 45 parts of inorganic gelling materials, 3 to 4 parts of redispersible latex powder, 3.5 to 4.5 parts of maleic anhydride, 41 to 45 parts of vinyl acetate, 4 to 6 parts of acrylic acid, 1 to 3 parts of emulsifier, and 0.6 to 0.7 parts of moisturizing thickener by weight. The above-mentioned slurry formula is set in a suitable range so that the sound absorption coefficient is in a suitable range and has good compressive strength. This may be because the void design of the porous allophane is matched with other compositions of the formula so that its voids are filled, and it has good sound absorption and storage, and better performance. The preparation method of the porous allophane using the present application is to bake the allophane at 800-900°C for 2-3h, then add the above product to a sodium silicate solution and stir for 2-3h, make pores in the slurry at 200-220°C for 50-55h, and continuously introduce nitrogen into the slurry. After the reaction is completed, filter and obtain porous allophane. The structure has a better pore design and the pores are in a suitable range, so that the combined formula has a better use effect.

[0061] Example 8: 50 parts of porous allophane, 60 parts of sand, 42 parts of inorganic gelling material, 3 parts of redispersible latex powder, 3.5 parts of maleic anhydride, 41 parts of vinyl acetate, 4 parts of acrylic acid, 1 part of emulsifier, 0.6 parts of moisturizing thickener, the preparation method comprises the following steps:

[0062] Step 1: Mix porous allophane, sand and inorganic gelling material, then add deionized water to dilute into a solution, and dry at 125° C. to obtain porous allophane composite slurry;

[0063] Step 2: adding redispersible latex powder, maleic anhydride, vinyl acetate, acrylic acid, emulsifier and moisturizing thickener to the porous allophane composite slurry.

[0064] The porosity of porous allophane is 72%.

[0065] Example 9: 50 parts of porous allophane, 60 parts of sand, 42 parts of inorganic gelling material, 3 parts of redispersible latex powder, 3.5 parts of maleic anhydride, 41 parts of vinyl acetate, 4 parts of acrylic acid, 1 part of emulsifier, 0.6 parts of moisturizing thickener, the preparation method comprises the following steps:

[0066] Step 1: Mix porous allophane, sand and inorganic gelling material, then add deionized water to dilute into a solution, and dry at 125° C. to obtain porous allophane composite slurry;

[0067] Step 2: adding redispersible latex powder, maleic anhydride, vinyl acetate, acrylic acid, emulsifier and moisturizing thickener to the porous allophane composite slurry.

[0068] The porosity of porous allophane is 75%.

[0069] Example 10: 50 parts of porous allophane, 60 parts of sand, 42 parts of inorganic gelling material, 3 parts of redispersible latex powder, 3.5 parts of maleic anhydride, 41 parts of vinyl acetate, 4 parts of acrylic acid, 1 part of emulsifier, 0.6 parts of moisturizing thickener, the preparation method comprises the following steps:

[0070] Step 1: Mix porous allophane, sand and inorganic gelling material, then add deionized water to dilute into a solution, and dry at 125° C. to obtain porous allophane composite slurry;

[0071] Step 2: adding redispersible latex powder, maleic anhydride, vinyl acetate, acrylic acid, emulsifier and moisturizing thickener to the porous allophane composite slurry.

[0072] The porosity of porous allophane is 80%.

[0073] Example Compressive strengthMpa Sound absorption coefficient Example 8 11.9 0.45 Example 9 11.8 0.44 Example 10 12.1 0.46

[0074] In some embodiments, the porosity of the porous allophane can be selected to be 70-80%. By optimizing the porosity of the porous allophane to be 72-80%, it is found that it has better compressive strength and sound absorption coefficient. This is because the voids are controlled within a suitable range and the filling effect is better. However, the porosity greater than 80% is difficult to achieve due to the difficulty of preparation and is not economical. Therefore, selecting the porosity of the porous allophane to be 72-80% has a better effect.

[0075] Through the optimization of this application, not only the sound insulation effect of the sound insulation mortar is improved, but also a good hardness range is maintained to meet the actual construction needs. Through the voids of porous allophane, the slurry is effectively filled, the design of the voids is combined with the optimization of the formula of porous allophane, sand and inorganic gelling materials, not only the void material plays a filling effect, but also because the above-mentioned porous material has a wide source and lower cost, it has a better sound insulation effect.

[0076] It should be noted that, in this article, relational terms such as "first" and "second" are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. The terms "include", "comprises" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device. In the absence of further restrictions, the elements defined by the sentence "comprises a ..." do not exclude the presence of other identical elements in the process, method, article or device including the elements.

[0077] The above description is only a preferred embodiment of the present application and does not constitute any form of limitation to the present application. Any technician familiar with the profession can make some changes or modify the technical contents disclosed above into equivalent embodiments with equivalent changes without departing from the scope of the technical solution of the present application. However, any simple modification, equivalent change and modification made to the above embodiments based on the technical essence of the present application without departing from the content of the technical solution of the present application still falls within the scope of the technical solution of the present application.

Claims

1. A lightweight sound insulation mortar, characterized in that: According to the mass ratio, 40-60 parts of porous allophane, 50-55 parts of sand material, 42-45 parts of inorganic gelling material, 3-4 parts of redispersible latex powder, 3.5-4.5 parts of maleic anhydride, 41-45 parts of vinyl acetate, 4-6 parts of acrylic acid, 1-3 parts of emulsifier, 0.6-0.7 parts of moisturizing thickener; The preparation method of the porous allophane comprises the following steps: calcining the allophane at 800-900° C. for 2-3 hours, adding the above product to a sodium silicate solution and stirring for 2-3 hours, forming pores in the slurry at 200-220° C. for 50-55 hours, and continuously introducing nitrogen into the slurry. After the reaction is completed, filtering is performed to obtain the porous allophane. The chemical formula of the allophane is Al2O3·SiO2·2.5H2O, the circularity of the porous allophane is 0.7-0.8, the porosity of the porous allophane is 70-80%, and the mass ratio of the porous allophane to the sand is 1-1.2; The preparation method of the lightweight sound insulation mortar comprises the following steps: Step 1: Mix porous allophane, sand and inorganic gelling material, then add deionized water to dilute into a solution, and dry at 125° C. to obtain porous allophane composite slurry; Step 2: adding redispersible latex powder, maleic anhydride, vinyl acetate, acrylic acid, emulsifier and moisturizing thickener to the porous allophane composite slurry; The compressive strength of this lightweight sound insulation mortar is 11.0Mpa.