LED structure, manufacturing method thereof and corresponding LED chip

By doping high-concentration Te in the n-type expansion layer of red LED and adopting a high-temperature diffusion process, the problem of excessive current expansion layer is solved, and efficient light extraction and cost reduction of red LED are achieved, and the quality of material growth is improved .

CN117810330BActive Publication Date: 2024-11-26DR TECH CO LTD YIXING JIANGSU
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202311851323.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-12-29
Publication Date
2024-11-26
Estimated Expiration
2043-12-29

AI Technical Summary

Technical Problem

The current expansion layer of existing red LEDs is too thick, resulting in poor light extraction effect, high cost, long growth time, and may affect internal quantum efficiency, and the materials used are expensive.

Method used

By doping high-concentration Te in the n-type expansion layer and using a high-temperature diffusion process, Te is diffused to the n-type expansion layer, thinning the current expansion layer, and reducing the doping concentration of Si, forming an LED structure and manufacturing method to achieve the same 的横向导电能力。

Benefits of technology

Without reducing the n-side expansion effect, the thickness of the n-type expansion layer is thinned, the epitaxial time and cost are reduced, the material growth quality is improved, the conductive ability is enhanced, and the impact on the active region is reduced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117810330B_ABST
    Figure CN117810330B_ABST
Patent Text Reader

Abstract

The present invention discloses an LED structure, a manufacturing method thereof and a corresponding LED chip. The LED structure includes an epitaxial stack and metal electrode layers located on both sides of the epitaxial stack, the epitaxial stack includes an n-type extension layer, an n-type restriction layer, an active layer, a p-type restriction layer and a p-type conductive layer stacked in sequence along the growth direction, the n-type extension layer is an n-type AlInP layer or an n-type AlGaInP layer and high-concentration Te doping is achieved through a high-temperature diffusion process. The present invention does not need to set up an independent n-type conductive layer, and can reduce the epitaxial thickness of the n-type extension layer, reduce the epitaxial time, improve the quality of material growth, and reduce the epitaxial cost while achieving the same or higher lateral conductivity.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of semiconductor technology, and in particular to an LED structure and a manufacturing method thereof, and a related LED chip. Background Art

[0002] As an electroluminescent light source, light emitting diode (LED) is energy-saving and environmentally friendly, and has a series of excellent properties such as high light efficiency, high brightness, low power consumption, and long life, and is widely used. Since the first appearance of red light emitting diodes, with the advancement of material growth technology and the development of device process technology, the luminous efficiency of red light LEDs has been continuously improved.

[0003] In the existing red LED epitaxial structure, a current expansion layer is designed to expand the light-emitting area and improve the external quantum efficiency of the diode. The current expansion layer must grow to a certain thickness to effectively expand the current. If the current expansion layer is not grown or the thickness is not enough, the light emitted by the diode is mainly concentrated under the electrode. Since the electrodes are all non-transparent metal materials, the emitted light will be reflected back and cannot be effectively extracted, resulting in poor light extraction. Growing a current expansion layer of a certain thickness can spread the current to the entire diode chip, allowing the chip to emit light as evenly as possible and improve the light extraction efficiency. Therefore, in the current red LED, in order to achieve effective lateral expansion of the current, the current expansion layer is relatively thick. However, a current expansion layer that is too thick has several disadvantages: ① A too thick expansion layer will spread the current to the edge of the LED chip, which will increase surface recombination and reduce efficiency; ② The absorption of light below the band gap of this layer of material increases with the increase of thickness; ③ The growth time is long, which may cause the doping source to diffuse into the active area and reduce the internal quantum efficiency. ④ The growth time is long, which may affect the growth quality of this layer and the active area. In addition, the raw materials of the LED n-side expansion layer, Al, In, and P, are relatively expensive, especially In and P. Growing AlInP:Si with a thickness that can achieve the n-expansion effect is very costly.

[0004] Therefore, it is necessary to provide a method for thinning the current spreading layer without reducing the n-side spreading effect. Summary of the invention

[0005] 1. Technical issues to be resolved

[0006] The purpose of the present invention is to provide an LED structure and a preparation method, which can reduce the thickness of the current spreading layer of the LED and solve the problem of thick current spreading layer of the flip-chip red LED in the prior art without reducing the n-side spreading effect.

[0007] (II) Technical solution

[0008] In order to achieve the above-mentioned purpose, one aspect of the present invention proposes an LED structure, including an epitaxial stack and metal electrode layers located on both sides of the epitaxial stack, the epitaxial stack includes an n-type extension layer, an n-type confinement layer, an active layer, a p-type confinement layer and a p-type conductive layer stacked along a growth direction; the n-type extension layer is an n-type AlInP layer or an n-type AlGaInP layer; the n-type extension layer is doped with Te.

[0009] As a preferred embodiment of the present invention, the n-type extension layer is doped with high concentration of Te.

[0010] As a preferred embodiment of the present invention, the metal electrode layer includes an n-side metal electrode layer directly disposed on the surface of the n-type extension layer.

[0011] As a preferred embodiment of the present invention, the concentration of Te doped in the n-type extension layer is greater than or equal to 1×10 19 / cm 3 .

[0012] As a preferred embodiment of the present invention, the high-concentration Te doping is performed by non-in-situ high-temperature diffusion.

[0013] As a preferred embodiment of the present invention, the n-type extension layer is doped with Si, and the doping concentration of Si is between 0.5×10 17 / cm 3 and 5×10 17 / cm 3 between.

[0014] As a preferred embodiment of the present invention, the thickness of the n-type extension layer is between 400 nm and 2000 nm.

[0015] Another aspect of the present invention provides a method for manufacturing an LED structure, comprising the following steps: manufacturing an epitaxial stack by an epitaxial growth process, the epitaxial stack comprising an n-type extension layer, an n-type restriction layer, an active layer, a p-type restriction layer and a p-type conductive layer stacked in sequence along a growth direction, wherein the n-type extension layer is an n-type AlInP layer or an n-type AlGaInP layer; forming a Te-containing thin film layer on the n-type extension layer, and performing ex-situ growth on the Te-containing thin film layer so that Te in the Te-containing thin film layer enters the n-type extension layer; and forming metal electrode layers on both sides of the epitaxial stack.

[0016] As a preferred embodiment of the present invention, an n-side metal electrode layer is directly formed on the surface of the n-type extension layer.

[0017] As a preferred embodiment of the present invention, the step of diffusing Te in the Te-containing thin film layer into the n-type extension layer is performed by high temperature diffusion.

[0018] As a preferred embodiment of the present invention, after the Te thin film layer is annealed, residual Te-containing components on the n-type extension layer are removed.

[0019] As a preferred embodiment of the present invention, potassium hydroxide or nitric acid is used to clean the residual Te-containing component.

[0020] As a preferred embodiment of the present invention, the Te-containing thin film layer is a Te thin film layer or a CdTe thin film layer.

[0021] As a preferred embodiment of the present invention, in the step of forming a Te-containing thin film layer on the n-type extension layer: when the Te-containing thin film layer is a Te thin film layer, the thickness of the Te thin film layer is at least 0.03% of the thickness of the n-type extension layer; when the Te-containing thin film layer is a CdTe thin film layer, the thickness of the CdTe thin film layer is at least 0.07% of the thickness of the n-type extension layer.

[0022] As a preferred embodiment of the present invention, the temperature of the high temperature diffusion is 300° C. to 500° C., and the time is 1 min to 10 min.

[0023] As a preferred embodiment of the present invention, the material of the metal electrode layer formed on the n-type extension layer side is Au.

[0024] A third aspect of the present invention provides an LED chip, comprising the LED structure provided above.

[0025] A fourth aspect of the present invention provides an LED chip, comprising an LED structure manufactured by the above-mentioned method for manufacturing an LED structure.

[0026] (III) Beneficial effects

[0027] Under the condition of achieving the same lateral conductivity, the present invention can reduce the epitaxial thickness of the n-type extension layer, shorten the epitaxial time, improve the quality of material growth, and reduce the epitaxial cost. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 It is a schematic diagram of the structure of the epitaxial stack generated in the manufacturing method of the LED structure of the comparative example.

[0029] Figure 2 It is a schematic structural diagram of forming a p-side gold electrode layer on the epitaxial stack in the manufacturing method of the LED structure of the comparative embodiment.

[0030] Figure 3 It is a schematic structural diagram of forming a metal electrode layer on the n-type extension layer side in the manufacturing method of the LED structure of the comparative embodiment.

[0031] Figure 4It is a schematic diagram of the structure of the epitaxial stack generated in the method for manufacturing the LED structure of Example 1 of the present invention.

[0032] Figure 5 It is a structural schematic diagram of forming a p-side gold electrode layer on the epitaxial stack in the method for manufacturing the LED structure of Example 1 of the present invention.

[0033] Figure 6 It is a schematic diagram of the structure of doping Te in the n-type extension layer in the method for manufacturing the LED structure of Example 1 of the present invention.

[0034] Figure 7 It is a structural schematic diagram of forming a metal electrode layer on the n-type extension layer side in the method for manufacturing the LED structure of embodiment 1 of the present invention. DETAILED DESCRIPTION

[0035] As mentioned above, in order to achieve effective lateral expansion of current in red LEDs, the current expansion layer is relatively thick. The purpose of the present invention is to provide an LED structure and a preparation method, which can reduce the thickness of the current expansion layer and solve the above problems in the prior art without reducing the n-side expansion effect.

[0036] Under the premise of not reducing the n-side expansion effect, thinning the n-side current expansion layer needs to consider the conductivity of this surface. According to the resistance formula R = ρL / S (R: resistance; ρ: resistivity; L: current diffusion length; S is the cross-sectional area through which the current passes). Without considering the change of L, there are two ways to reduce resistance: ① reduce the resistivity ρ; ② increase the cross-sectional area S through which the current passes.

[0037] In method ②, increasing the cross-sectional area S through which the current passes requires increasing the thickness of the n-side current spreading layer, which does not meet the purpose of thinning. In method ①, according to the formula ρ = 1 / nqμ n (n: carrier concentration, q: unit charge, μ n : Mobility), generally the mobility changes little, and the resistivity can be reduced by increasing the doping concentration.

[0038] The n-side extension layer material of the LED structure is generally Si-doped Al(Ga)InP (expressed as AlInP:Si or AlGaInP:Si). The doping concentration of Si in Al(Ga)InP is low, so the doping source can be replaced to achieve the purpose of high doping and reducing resistance. Te can reach a higher doping concentration in Al(Ga)InP, which meets the requirements. There are also two methods for doping Te in Al(Ga)InP:

[0039] The first is in-situ doping, which is to directly dope and grow Te during the epitaxial growth of Al(Ga)InP. However, this method has two limitations or disadvantages. First, it is difficult to epitaxially grow high-quality high-Te-doped AlInP materials using the MOCVD method, and the quality of material growth is difficult to guarantee, which may affect the subsequent growth quality of the active area. Second, the diffusion coefficient of Te in III-V semiconductor materials such as Al(Ga)InP is very high. Under high-temperature growth conditions with high doping concentrations, or when the subsequent chip works at high temperatures for a long time, Te atoms may diffuse into the active area, thereby reducing the internal quantum efficiency and affecting chip performance.

[0040] The second method is non-in-situ doping. During the chip process, a layer of Te is evaporated on the low-Si-doped Al(Ga)InP. Through RTP annealing, Te is thermally diffused into Al(Ga)InP:Si to increase the doping concentration, reduce the resistance of the n-side extension layer, and thin the n-side extension layer.

[0041] According to literature reports, high Si doping will affect the growth quality of Al(Ga)InP materials. This subsequent Te diffusion has another benefit, which is that when MOCVD epitaxially grows Si-doped Al(Ga)InP material layers, the Si doping concentration can be reduced, and the growth quality of the layer can be improved, thereby improving or ensuring the material quality of the subsequent active area. At the same time, this method can also control the diffusion depth of Te so that it does not diffuse into the active area and does not affect the internal quantum efficiency.

[0042] In order to achieve the above object, the technical solution adopted by the present invention is as follows:

[0043] The LED structure includes an epitaxial stack and metal electrode layers located on both sides of the epitaxial stack, the epitaxial stack at least includes an n-type extension layer, an n-type confinement layer, an active layer, a p-type confinement layer and a p-type conductive layer stacked in sequence along a growth direction, wherein the n-type extension layer is an n-type AlInP layer or an n-type AlGaInP layer, and Te is doped in the n-type extension layer.

[0044] The Te doped in the n-type extension layer is diffused into the n-type extension layer by the high temperature diffusion process of the present invention, and the concentration of Te in the n-type extension layer can be made greater than or equal to 1×10 19 / cm 3 At the same time, in order to improve the growth quality of the n-type AlInP layer or the n-type AlGaInP layer, the present invention can reduce the doping concentration of Si in the n-type AlInP layer or the n-type AlGaInP layer. For example, the present invention can make it within 0.5×10 17 / cm 3 and 5×10 17 / cm 3It is much lower than the doping concentration of Te.

[0045] The high temperature diffusion process includes an annealing process.

[0046] After adopting the above scheme, a high doping concentration of the n-type diffusion layer is achieved, thereby reducing the resistance. Therefore, while achieving the same lateral conductivity, the thickness of the n-type diffusion layer can be reduced, while improving the growth quality of the n-type layer, reducing the epitaxial time and cost. Optionally, the n-type extension layer can be thinned to 1 / 4 to 1 / 6 of the n-type extension layer when Te is not doped, for example, 1 / 5 of the original.

[0047] The present invention does not strictly limit the composition of the epitaxial stack, but generally speaking, the epitaxial stack structure of the LED includes an n-type extension layer, an n-type confinement layer, an active layer, a p-type confinement layer, and a p-type conductive layer stacked in sequence along the growth direction. However, it should be noted that other layers may also appear in the epitaxial stack, such as an ohmic contact layer, which should all be considered to be within the scope of protection of the present invention. In addition, temporary structures may also appear in the formation process of the epitaxial stack, such as a temporary substrate and a temporary functional layer, including a buffer layer, a corrosion layer, etc.

[0048] However, since GaAs has a relatively small band gap, it can absorb part of the light emitted by the active layer, which will reduce the external quantum efficiency of the LED. Considering this, the present invention preferably does not provide an n-type GaAs ohmic contact layer.

[0049] As a specific implementation, the temporary substrate may be a GaAs substrate. For example, one implementation is to grow an epitaxial stack on a GaAs substrate, wherein the epitaxial stack includes an n-type buffer layer, an n-type corrosion layer, an n-type extension layer, an n-type confinement layer, an active layer, a p-type confinement layer, and a p-type conductive layer sequentially stacked along a growth direction.

[0050] As a specific implementation, in order to dope Te in the n-type extension layer, in the manufacturing process of the present invention, a Te thin film layer or a CdTe thin film layer is evaporated on the n-type extension layer.

[0051] The thickness of the Te thin film layer or the CdTe thin film layer is determined according to the thickness of the n-type extension layer. According to the simulation and actual measurement of the present invention, the thickness of the Te thin film layer is preferably greater than or equal to 0.03% of the thickness of the n-type extension layer, and the thickness of the CdTe thin film layer is preferably greater than or equal to 0.07% of the thickness of the n-type extension layer; further, nitric acid or potassium hydroxide can be used to clean the residual Te thin film layer or the CdTe thin film layer.

[0052] Te is introduced into the n-type extension layer through a high temperature diffusion process, and the RTP annealing temperature is between 300°C and 500°C to achieve high doping of the n-type extension layer, and the process time is 1 minute to 10 minutes. An optional process is the RTP annealing process.

[0053] According to the present invention, the doping concentration of the n-type extension layer can be increased to 1×10 19 / cm 3 At the same time, compared with the conventional Si doping concentration of 10 18 / cm 3 Compared with the expansion layer of an order of magnitude, the present invention can reduce the Si doping concentration to 10 17 / cm 3 As a specific embodiment, the metal electrode layer of the present invention preferably adopts an n-metal semiconductor contact structure, such as an n-type AlInP:Si layer / n-metal structure, wherein the n-metal is preferably Au.

[0054] It can be seen that the present invention forms a Te / CdTe thin film layer and anneals it in the manufacturing process, thereby achieving a high doping concentration of the n-type extension layer, thereby reducing the resistance. While achieving the same lateral conductivity, the thickness of the n-type extension layer can be reduced, the growth quality of the n-type extension layer can be improved, and the epitaxial time and cost can be reduced.

[0055] In order to make the objectives, technical solutions and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with specific embodiments and with reference to the accompanying drawings.

[0056] In order to reflect the characteristics and advantages of the present invention over the prior art, a comparative example is first described herein for comparison. The comparative example adopts a conventional LED structure, that is, Te is not doped in the n-type extension layer.

[0057] Figure 1 FIG. 1 is a schematic diagram of the structure of the epitaxial stack generated in the manufacturing method of the LED structure of the comparative embodiment. Figure 1 As shown, the comparative embodiment adopts metal organic vapor phase epitaxy to sequentially grow an n-type GaAs:Si buffer layer 2 (200nm), an n-type GaInP:Si etching layer 3 (150nm), an n-type AlInP:Si extension layer 4 (3μm), an n-type AlInP:Si confinement layer 5 (500nm), an active layer 6 (AlInP:Si confinement layer 7 (AlInP:Si confinement layer 8 (AlInP:Si confinement layer 9 (AlInP:Si confinement layer 10 (AlInP:Si confinement layer 11 (AlInP:Si confinement layer 12 (AlInP:Si confinement layer 13 (AlInP:Si confinement layer 14 (AlInP:Si confinement layer 15 (AlInP:Si confinement layer 16 (AlInP:Si confinement layer 17 (AlInP:Si confinement layer 18 (Al 0.6 GaInP barrier layer, GaInP, Al 0.55 GaInP、Al 0.6 GaInP barrier layer), p-type AlInP:Mg confinement layer 7 (500nm and p-type GaP:Mg conductive layer 8 (3μm).

[0058] The thickness of the n-type AlInP:Si extension layer 4 is 3 μm, and the Si doping concentration is 2×10 18 / cm 3 .

[0059] Figure 2 It is a schematic structural diagram of forming a p-side gold electrode layer on the epitaxial stack in the manufacturing method of the LED structure of the comparative embodiment. Figure 2 The direction is Figure 1 The direction after flipping upside down, such as Figure 2 As shown, after forming the epitaxial stack, a p-side metal electrode layer 9 is grown on one side of the p-type conductive layer 8. Furthermore, the GaAs substrate 1, GaAs:Si buffer layer 2, and n-type GaInP:Si etching layer 3 are removed by etching to expose the n-type AlInP:Si extension layer 4.

[0060] Figure 3 FIG. 1 is a schematic diagram of a structure in which a metal electrode layer is formed on one side of an n-type extension layer in a method for manufacturing an LED structure of a comparative embodiment. Figure 3 As shown, in this comparative embodiment, an evaporation process of an n-side metal electrode layer 10 is performed on the n-type AlInP:Si extension layer 4, and Au is used here.

[0061] Embodiment 1 of the present invention:

[0062] Figure 4 FIG. 1 is a schematic diagram of the structure of the epitaxial stack generated in the method for manufacturing the LED structure of Example 1 of the present invention. Figure 4 As shown in the figure, the comparative embodiment of the present invention embodiment 1 has a similar structure to the comparative embodiment described above, and it also adopts metal organic vapor phase epitaxy to sequentially grow an n-type GaAs:Si buffer layer 2, an n-type GaInP:Si etching layer 3, an n-type AlInP:Si extension layer 4, an n-type AlInP:Si restriction layer 5, an active layer 6 (AlInP:Si is sequentially grown) from bottom to top on a GaAs substrate 1. 0.6 GaInP barrier layer, GaInP, Al 0.55 GaInP、Al 0.6 GaInP barrier layer), p-type AlInP:Mg confinement layer 7 and p-type GaP:Mg conductive layer 8.

[0063] However, unlike the comparative example, the thickness of the n-type AlInP:Si extension layer in the practical example 1 of the present invention can be reduced to 400nm-2000nm, for example, 600nm. At the same time, the doping concentration of Si can be reduced to 0.5x10 17 / cm 3 ~5ⅹ10 17 / cm 3 , for example 1 x 10 17 / cm 3 1 x 10 17 / cm 3 .

[0064] Figure 5 FIG. 1 is a schematic diagram of a structure in which a p-side gold electrode layer is formed on an epitaxial stack in a method for manufacturing an LED structure according to Embodiment 1 of the present invention. Figure 5 As shown, similar to the comparative embodiment, after the epitaxial stack is formed, a p-side metal electrode layer 9 is grown on one side of the p-type conductive layer 8. Furthermore, the GaAs substrate 1, the GaAs:Si buffer layer 2, and the n-type GaInP:Si etching layer 3 are removed by etching to expose the n-type AlInP:Si extension layer 4.

[0065] Figure 6 FIG. 1 is a schematic diagram of a method for manufacturing an LED structure according to Embodiment 1 of the present invention, in which Te is doped in an n-type extension layer and a metal electrode layer is formed on the side. Figure 6 As shown, a Te film 41 with a thickness of 1 nm is evaporated on the n-type AlInP:Si extension layer 4, and then RTP annealing at 400°C for 1 min is performed to allow Te to enter the n-type AlInP:Si extension layer 4 (in the direction of the arrow in the figure), thereby achieving high doping of the n-type AlInP:Si extension layer 4, and then the residual Te film 41 is cleaned with potassium hydroxide.

[0066] Figure 7 1 is a schematic diagram of a structure in which a metal electrode layer is formed on the n-type extension layer side in the method for manufacturing the LED structure of Example 1 of the present invention. Similar to the comparative example, an evaporation process of an n-side metal electrode layer 10 is performed on the n-type AlInP:Si extension layer 4, and Au is used here.

[0067] Embodiment 2:

[0068] Example 2 is similar to Example 1, except that the Te thin film layer used in Example 1 is replaced by a CdTe thin film layer. Since the Te content in the CdTe thin film layer is less than that in the Te thin film layer, a thicker CdTe thin film layer is required to achieve the same Te doping concentration.

[0069] In Example 2, similarly, first, an n-type GaAs:Si buffer layer 2, an n-type GaInP:Si etching layer 3, an n-type AlInP:Si extension layer 4, an n-type AlInP:Si restriction layer 5, and an active layer 6 (AlInP:Si is grown in sequence) are grown on a GaAs substrate 1 from bottom to top by using a metal organic vapor phase epitaxy method. 0.6 GaInP barrier layer, GaInP, Al 0.55 GaInP、Al 0.6GaInP barrier layer), p-type AlInP:Mg restriction layer 7, p-type GaP:Mg conductive layer 8. Next, grow p-side metal electrode layer 9, etch GaAs substrate 1, GaAs:Si buffer layer 2, n-type GaInP:Si etching layer 3. Then, evaporate a layer of CdTe film 41 with a thickness of 2nm on the n-type AlInP:Si extension layer 4, and then perform 400℃RTP annealing for 1min to allow Te to enter the n-type AlInP:Si extension layer 4, thereby achieving high Te doping of the n-type AlInP:Si extension layer 4. Then use nitric acid to clean the remaining CdTe film, and then perform the evaporation process of the n-side metal electrode layer 9, in which Au is used.

[0070] In this embodiment 2, similarly, the thickness of the n-type AlInP:Si extension layer 4 can be 400nm to 2000nm, for example, 600nm, and the doping concentration of Si is reduced to 0.5x10 17 / cm 3 ~5ⅹ10 17 / cm 3 , for example 1 x 10 17 / cm 3 .

[0071] In the above-mentioned Embodiment 1 and Embodiment 2, the n-type AlInP:Si extension layer may be replaced by an n-type AlGaInP:Si extension layer.

[0072] The LED structure proposed in the present invention and the LED structure manufactured by the manufacturing method can be manufactured into an LED chip by a flip-chip packaging process.

[0073] In summary, in the above-mentioned Embodiment 1 and Embodiment 2, since Te is doped in the n-type extension layer through the annealing process, the conductivity of the n-type extension layer is enhanced. Therefore, compared with the prior art, the thickness of the n-type extension layer can be reduced and the epitaxial time can be reduced while achieving the same lateral conductivity. At the same time, since the doping concentration of Si in the n-type extension layer can be reduced, the present invention is also conducive to improving the growth quality of the extension layer material and reducing the epitaxial cost.

[0074] The specific embodiments described above further illustrate the objectives, technical solutions and beneficial effects of the present invention in detail. It should be understood that the above description is only a specific embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the scope of protection of the present invention.

Claims

1. An LED structure, comprising an epitaxial stack and metal electrode layers located on both sides of the epitaxial stack, wherein: The epitaxial stack includes an n-type extension layer, an n-type confinement layer, an active layer, a p-type confinement layer and a p-type conductive layer stacked along a growth direction; The n-type extension layer is an n-type AlInP layer or an n-type AlGaInP layer; The n-type extension layer is doped with high concentration of Te; The metal electrode layer comprises an n-side metal electrode layer directly disposed on the surface of the n-type extension layer; The Te doping concentration in the n-type extension layer is greater than 1×10 19 / cm 3 , Te doping is carried out by non-in-situ high-temperature diffusion; The n-type extension layer is doped with Si, and the doping concentration of Si is 0.5×10 17 / cm 3 and 5×10 17 / cm 3 between.

2. The LED structure according to claim 1, characterized in that: The thickness of the n-type extension layer is between 400 nm and 2000 nm.

3. A method for manufacturing an LED structure, characterized in that: The steps include: An epitaxial stack is produced by an epitaxial growth process, wherein the epitaxial stack comprises an n-type extension layer, an n-type confinement layer, an active layer, a p-type confinement layer and a p-type conductive layer sequentially stacked along a growth direction, wherein the n-type extension layer is an n-type AlInP layer or an n-type AlGaInP layer; forming a Te-containing thin film layer on the n-type extension layer, and performing ex-situ growth on the Te-containing thin film layer so that Te in the Te-containing thin film layer diffuses into the n-type extension layer; directly forming an n-side metal electrode layer on the surface of the n-type extension layer; Wherein, the Te doping concentration in the n-type extension layer is greater than 1×10 19 / cm 3 ; The n-type extension layer is doped with Si, and the doping concentration of Si is 0.5×10 17 / cm 3 and 5×10 17 / cm 3 between.

4. The method for manufacturing an LED structure according to claim 3, characterized in that: The step of diffusing Te in the Te-containing thin film layer into the n-type extension layer is performed by high-temperature diffusion.

5. The method for manufacturing an LED structure according to claim 3, wherein: After Te in the Te-containing thin film layer is diffused into the n-type extension layer, residual Te-containing components on the n-type extension layer are removed.

6. The method for manufacturing an LED structure according to claim 3, wherein: The Te-containing thin film layer is a Te thin film layer or a CdTe thin film layer.

7. The method for manufacturing an LED structure according to claim 6, wherein: In the step of forming a Te-containing thin film layer on the n-type extension layer: when the Te-containing thin film layer is a Te thin film layer, the thickness of the Te thin film layer is at least 0.03% of the thickness of the n-type extension layer; when the Te-containing thin film layer is a CdTe thin film layer, the thickness of the CdTe thin film layer is at least 0.07% of the thickness of the n-type extension layer.

8. The method for manufacturing an LED structure according to claim 4, wherein: The high temperature diffusion temperature is 300° C. to 500° C., and the time is 1 min to 10 min.

9. An LED chip, characterized in that: The LED structure comprises the LED structure according to any one of claims 1 to 2.

10. An LED chip, characterized in that: The invention comprises an LED structure manufactured by the method for manufacturing an LED structure according to any one of claims 3 to 8.

Citation Information

Patent Citations

  • Light-emitting diode with modulation-doped current expansion layer

    CN102664226A

  • High concentration Te doped light emitting diode epitaxial structure

    CN104332537A

  • Optoelectronic semiconductor chip and a method for producing optoelectronic semiconductor chips

    CN104813487A

  • Semiconductor luminous equipment

    CN1099521A

  • Micron-sized light emitting diode designs

    CN112088431A