A glassy carbon microneedle patch and preparation method thereof

Through the centralized heat preservation method of gridded precursors, the process complexity and defect problems existing in the preparation of glassy carbon microneedle patches are solved, high-quality, low-cost product preparation is achieved, and the process flow is simplified.

CN117815529BActive Publication Date: 2024-10-11HUAHANGMICROCREATETECHNOLOGYCO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202311717078.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-12-14
Publication Date
2024-10-11
Estimated Expiration
2043-12-14

AI Technical Summary

Technical Problem

The preparation process of existing glassy carbon microneedle patches is complex, which makes the product prone to defects such as degeneration, foaming, and cracking. It is difficult to avoid morphological and performance problems, and the process is time-consuming and costly.

Method used

The gridded precursor is used for pyrolysis treatment through a centralized heat preservation method, including two stages of stress relief and pyrolysis carbonization. The gridded arrangement is used to uniformly discharge impurities, reduce the dependence on high-temperature heat preservation, and use rapid temperature rise to complete material conversion.

Benefits of technology

The quality of the glassy carbon microneedle patch is improved, the defect area is reduced, the preparation cost is reduced, the form and performance of the product are improved, and the process flow is simplified.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117815529B_ABST
    Figure CN117815529B_ABST
Patent Text Reader

Abstract

The present invention relates to the field of glassy carbon preparation, specifically to a glassy carbon microneedle patch and a preparation method thereof, wherein the glassy carbon microneedle patch is prepared by a centralized heat preservation method based on a gridded precursor, and the method comprises the steps of: using a gridded preparation process to obtain a gridded precursor for preparing the glassy carbon microneedle patch, and the precursor comprises a plurality of grid holes arranged at intervals to form a gridded arrangement, and a microneedle structure to be formed is arranged at the edge of the grid hole; placing the gridded precursor in a heating box, and performing a key gradient heat preservation on the gridded precursor in a lower temperature range, and then using a rapid heating process to complete the final glassy carbon material conversion. The centralized heat preservation method based on a gridded design proposed by the present invention can effectively avoid defects such as foaming, deformation, and breakage of the glassy carbon microneedle patch, and optimize the performance of the glassy carbon product.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of glassy carbon preparation, in particular to a glassy carbon microneedle patch and a preparation method thereof. Background Art

[0002] Microneedle patches are composed of multiple tiny needle tips connected to a base in an array, and are widely used in disease prevention, diagnosis and treatment, rehabilitation, medical aesthetics and other fields.

[0003] Glassy carbon (also known as glassy carbon) is a type of amorphous carbon with good mechanical properties, electrical conductivity, biocompatibility, and chemical stability. Compared with commonly used polymers, metals, ceramics and other materials for preparing microneedle patches, it has some unique properties. Microneedle patches based on glassy carbon have unique applications in medicine, electronics, chemical industry and other fields. The development of microneedle patches based on glassy carbon is of great significance.

[0004] Glassy carbon is usually obtained by gradient pyrolysis of polymer precursors. The process is complicated, and the pyrolysis process will cause a large volume shrinkage, causing large product defects, such as: denaturation, foaming, cracking, breakage, etc., and it is very difficult to develop high-quality glassy carbon microneedle patches. For example, CN109627003A discloses a method for preparing a new glassy carbon material with furfural furfuryl alcohol modified resin. For another example, CN105819859A discloses a method for preparing a glassy carbon material based on a polymer prepolymer precursor. However, this process is relatively complicated in terms of heating procedures, especially the need to perform several insulation treatments relatively frequently at various temperature points (which will also involve multi-stage temperature control, and the process implementation cost and monitoring difficulty are relatively large), and the process is relatively time-consuming; second, when preparing glassy carbon microneedle products with tiny morphology, it is extremely difficult to avoid large product defects, which will also seriously affect the morphology and performance of glassy carbon.

[0005] At present, research has achieved the preparation of glassy carbon microneedles; however, microneedles often need to be made into microneedle patches to be convenient to use and exert their effects, especially the conductivity and other effects of glassy carbon microneedles are very dependent on the performance of the microneedle base. However, due to the fine and complex structure of microneedle patches, the pyrolysis process in the preparation of glassy carbon will cause serious deformation defects in conventional microneedle patches, and the development of high-quality glassy carbon microneedle patches faces huge challenges.

[0006] Therefore, the development of a new type of glassy carbon microneedle patch and an efficient preparation method has important scientific significance and great application value. At present, there is an urgent need for a preparation method that can improve the morphology, performance and other properties of glassy carbon microneedle patch products and can control the implementation cost. Summary of the invention

[0007] The object of the present invention is to provide a method for preparing a glassy carbon microneedle patch, which partially solves or alleviates the above-mentioned deficiencies in the prior art, can improve the preparation quality of the microneedle patch, and reduce the preparation cost.

[0008] In order to solve the above-mentioned technical problems, the present invention specifically adopts the following technical solutions:

[0009] The first aspect of the present invention is to provide a glassy carbon microneedle patch, comprising: a main body, and a hollow area that can be arranged in the main body; the main body comprises: a gridded substrate, a plurality of grid holes are arranged at intervals on the gridded substrate, and a plurality of microneedles or microneedle-like structures are arranged on the edges of the grid holes; wherein the glassy carbon microneedle patch is prepared by subjecting a gridded precursor to centralized heat-insulating pyrolysis treatment, and the gridded precursor is prepared from a carbon-based polymer.

[0010] In some embodiments, the line width L1 of the grid holes in the gridded precursor is less than or equal to 2 mm, and the radius L2 of the body is less than or equal to 100 mm.

[0011] In some embodiments, the body may be in one or more of the following shapes: circular, annular, elliptical, or rounded rectangular.

[0012] In some embodiments, the base of the microneedle-like structure may be in one or more of the following shapes: circular, rectangular, cross-shaped, or 'P'-shaped.

[0013] The present invention also provides a method for preparing a glassy carbon microneedle patch, wherein the centralized heat preservation step comprises: S20 placing the gridded precursor in a heating box and starting the centralized heat preservation method; and S20 comprises:

[0014] S21 selects a stress relief temperature to perform insulation treatment on the gridded precursor in the first heating stage to relieve stress on the gridded precursor; wherein the stress relief temperature is selected by a first selection rule; and the first selection rule is: selecting the stress relief temperature from the weight loss rate fluctuation temperature; and the weight loss rate fluctuation temperature corresponds to the temperature value corresponding to the data point with the largest curvature change in the thermogravimetric differential curve within a range less than the pyrolysis carbonization temperature.

[0015] In some embodiments, S20 further includes:

[0016] S22 heats up and enters the second heating stage, and in the second heating stage, the pyrolysis carbonization temperature is selected to perform insulation treatment on the grid precursor again to make the grid precursor undergo pyrolysis carbonization. At this time, the microneedles or microneedle-like structures to be formed on the grid precursor and the grid holes shrink in proportion during the pyrolysis carbonization process, and the impurities generated can be evenly discharged outward using a grid arrangement; wherein, the pyrolysis carbonization temperature is selected by a second selection rule; the second selection rule is: the pyrolysis carbonization temperature is selected from the weight loss fluctuation temperature; wherein, the weight loss fluctuation temperature corresponds to the temperature value corresponding to the curve segment with the largest curvature change in the interval where the slope of the thermogravimetric analysis curve gradually decreases.

[0017] In some embodiments, it also includes:

[0018] S30 In the subsequent third heating stage, the temperature is continuously raised from the pyrolysis carbonization temperature to the target heating temperature; and finally the grid precursor prepared from the carbon-based polymer is converted into a glassy carbon microneedle patch.

[0019] In some embodiments, it also includes:

[0020] During the heating stage of the gridded precursor, an inert gas is introduced into the heating box to protect the precursor and discharge the impurities;

[0021] The concentration index of the impurities is collected through a gas monitoring device.

[0022] In some embodiments, it also includes:

[0023] In the third heating stage, when the concentration index of the impurity is monitored to be lower than the set concentration range, a switching time is selected according to the current time, wherein the difference between the switching time and the current time is less than the set difference range;

[0024] At the conversion moment, the current first heating rate is increased to the second heating rate, and the temperature is continuously increased to the target heating temperature.

[0025] In some embodiments, the carbon-based polymer includes: a carbon-rich polymer, wherein the carbon-rich polymer includes one or more of the following: polyurethane, epoxy resin, phenolic resin, polyacrylonitrile, polyimide, polystyrene, polytetrafluoroethylene, polyethylene, polyaniline, or a product obtained by further modification of the carbon-rich polymer;

[0026] And / or, the preparation method of the gridded precursor includes: mold forming, and / or 3D printing.

[0027] Another aspect of the present invention provides a method for preparing a glassy carbon microneedle patch, wherein the glassy carbon is prepared by a centralized heat preservation method based on a gridded precursor, and accordingly, the method comprises the steps of:

[0028] S10: preparing a grid precursor using a carbon polymer raw material, wherein the grid precursor comprises a plurality of grid holes arranged at intervals, the grid holes intersect each other to form a grid arrangement, and microneedles or microneedle-like structures to be formed are arranged at the edges of the grid holes;

[0029] S20 places the gridded precursor in a heating box and starts a centralized heat preservation method, S20 includes:

[0030] S21: in the first heating stage, a stress relief temperature is selected to perform a heat preservation treatment on the gridded precursor to relieve stress on the gridded precursor; wherein the stress relief temperature is selected by a first selection rule;

[0031] S22: The temperature is raised to enter the second heating stage, and the pyrolysis carbonization temperature is selected in the second heating stage to perform heat preservation treatment on the grid precursor again, so that the grid precursor is pyrolyzed and carbonized. At this time, the target to be formed on the grid precursor and the grid holes shrink in proportion during the pyrolysis and carbonization process, and the impurities generated can be uniformly discharged outward by using the grid arrangement; wherein the pyrolysis and carbonization temperature is selected by the second selection rule;

[0032] S30: in the subsequent third heating stage, the temperature is continuously raised from the pyrolysis carbonization temperature to the target heating temperature; finally, the carbon polymer is converted into glassy carbon;

[0033] Among them, the first selection rule is: select the stress relief temperature from the weight loss rate fluctuation temperature; and the weight loss rate fluctuation temperature corresponds to the temperature value corresponding to the data point with the largest curvature change in the interval less than the pyrolysis and carbonization temperature in the thermogravimetric differential curve; the second selection rule is: select the pyrolysis and carbonization temperature from the weight loss fluctuation temperature; wherein the weight loss fluctuation temperature corresponds to the temperature value corresponding to the curve segment with the largest curvature change in the interval where the slope of the thermogravimetric analysis curve gradually decreases.

[0034] In some embodiments, when there is a first number of weight loss rate fluctuation temperatures, and the first number is greater than or equal to 2, the S21 includes the steps of:

[0035] A second number of weight loss rate fluctuation temperatures are selected from the first number of weight loss rate fluctuation temperatures at intervals, and a second number of stress relief temperatures are correspondingly acquired, wherein the second number is less than or equal to the first number, and the stress relief temperatures at least include: a first stress relief temperature and a second stress relief temperature;

[0036] In the first heating stage, a first stress relief temperature is used for heat preservation treatment, so as to perform a first stress relief on the gridded precursor;

[0037] The temperature is continuously raised from the first stress relief temperature to the second stress relief temperature for heat preservation, so as to perform a second stress relief on the gridded precursor.

[0038] In some embodiments, the steps include:

[0039] During the heating stage of the gridded precursor, an inert gas is introduced into the heating box to discharge the impurities out of the heating box through an exhaust pipe;

[0040] The concentration index of the impurities is collected through a gas monitoring device connected to the exhaust pipe.

[0041] In some embodiments, the steps include:

[0042] In the third heating stage, when the concentration index of the impurity is monitored to be lower than the set concentration range, a switching time is selected according to the current time, wherein the difference between the switching time and the current time is less than the set difference range;

[0043] At the conversion moment, the current first heating rate is increased to the second heating rate, and the temperature is continuously increased to the target heating temperature.

[0044] In some embodiments, the gridded precursor includes: a main body, and a hollow area arranged in the middle of the main body, and the main body is evenly arranged around the edge of the hollow area, and a plurality of grid holes are arranged at intervals on the main body.

[0045] In some embodiments, the line width L1 of the grid holes is less than 2 mm, and the radius L2 of the body is less than 100 mm; and / or,

[0046] The body may be in one or more of the following shapes: circular, oval, or rounded rectangular.

[0047] In some embodiments, the base of the object to be formed may be in one or more of the following shapes: circular, square, cross, or '-shaped; and / or, the object to be formed is a microneedle.

[0048] In some embodiments, S10 includes:

[0049] Providing a carbon-rich photopolymer material as a raw material, and obtaining process parameters for preparing the gridded precursor according to the photopolymer material, wherein the process parameters include one or more of the following: the line width of the grid holes, the radius of the main body, the size of the target to be formed, and the thickness of the gridded precursor;

[0050] The process parameters are input into a 3D printing system based on photopolymerization, and the photopolymerization material is discretized and stacked by the 3D printing system to prepare a corresponding gridded precursor. BRIEF DESCRIPTION OF THE DRAWINGS

[0051] In order to more clearly illustrate the technical solutions in the embodiments of the present invention or the prior art, the drawings required for use in the embodiments or the prior art descriptions are briefly introduced below. In all the drawings, similar elements or parts are generally identified by similar reference numerals. In the drawings, each element or part is not necessarily drawn according to the actual scale. Obviously, the drawings described below are some embodiments of the present invention. For those of ordinary skill in the art, other drawings can also be obtained based on these drawings without paying creative labor.

[0052] Figure 1 It is a schematic flow chart of a centralized heat preservation method in an exemplary embodiment of the present invention;

[0053] Figure 2a A schematic diagram of temperature design of a centralized heat preservation method in an exemplary embodiment of the present invention;

[0054] Figure 2b A schematic diagram of temperature design of a centralized heat preservation method in another exemplary embodiment of the present invention;

[0055] Figure 3 A schematic diagram of a thermogravimetric curve of a meshed precursor in an exemplary embodiment of the present invention;

[0056] Figure 4 is a schematic diagram of the structure of a gridded microneedle in an exemplary embodiment of the present invention;

[0057] Figure 5 It is a schematic diagram of the surface morphology of a grid-shaped precursor after being pyrolyzed by a centralized heat preservation method in an exemplary embodiment of the present invention;

[0058] Figure 6 is a schematic structural diagram of a gridded precursor in an exemplary embodiment of the present invention;

[0059] Figure 7 Schematic diagram of the effect of different heating temperatures on the conductive properties of meshed microneedles;

[0060] Figure 8 This is a schematic diagram of a failed product;

[0061] Fig. 9 It is a module diagram of a monitoring system in an exemplary embodiment of the present invention.

[0062] Reference numerals:

[0063] 01 is the main body, 011 is the microneedle, 012 is the grid hole, and 02 is the hollow area. DETAILED DESCRIPTION

[0064] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.

[0065] Herein, suffixes such as "module", "component" or "unit" used to represent elements are only used to facilitate the description of the present invention, and have no specific meanings by themselves. Therefore, "module", "component" or "unit" can be used mixedly.

[0066] In this document, the terms "upper", "lower", "inner", "outer", "front", "back", "one end", "the other end" and the like indicate positions or positional relationships based on the positions or positional relationships shown in the drawings, and are only for the convenience of describing the present invention and simplifying the description, and do not indicate or imply that the devices or elements referred to must have a specific orientation, be constructed and operate in a specific orientation, and therefore cannot be understood as limiting the present invention. In addition, the terms "first" and "second" are used for descriptive purposes only and cannot be understood as indicating or implying relative importance.

[0067] In this document, unless otherwise clearly specified and limited, the terms "installed", "provided with", "connected", etc. should be understood in a broad sense. For example, "connected" can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection, a direct connection, or an indirect connection through an intermediate medium, or it can be the internal communication of two components. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.

[0068] Herein "and / or" includes any and all combinations of one or more of the associated listed items.

[0069] Herein, "plurality" means two or more than two, ie, it includes two, three, four, five, etc.

[0070] It should be noted that, in this article, the terms "include", "comprises" or any other variations thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device. In the absence of further restrictions, an element defined by the sentence "comprises a ..." does not exclude the existence of other identical elements in the process, method, article or device including the element.

[0071] As used in this specification, the term "about" typically means + / - 5% of the stated value, more typically + / - 4% of the stated value, more typically + / - 3% of the stated value, more typically + / - 2% of the stated value, even more typically + / - 1% of the stated value, and even more typically + / - 0.5% of the stated value.

[0072] In this specification, some embodiments may be disclosed in a format of being within a certain range. It should be understood that such description of "being within a certain range" is only for convenience and brevity, and should not be interpreted as a rigid limitation on the disclosed range. Therefore, the description of the range should be considered to have specifically disclosed all possible sub-ranges and independent numerical values ​​within this range. For example, the range The description of should be considered to have specifically disclosed sub-ranges such as from 1 to 3, from 1 to 4, from 1 to 5, from 2 to 4, from 2 to 6, from 3 to 6, etc., as well as individual numbers within this range, such as 1, 2, 3, 4, 5 and 6. Regardless of the breadth of the range, the above rules apply. As used herein, "data point" may refer to a piece of data corresponding to one or more temperature points.

[0073] Herein, "carbon-based polymer" generally refers to a carbon-rich polymer, for example, it can be a photocurable polymer material such as polyurethane, epoxy resin, or a polymer such as acrylonitrile resin, phenolic resin or polyimide.

[0074] Herein, "concentration index" refers to an index that can be used to characterize the quantity / concentration of a substance (such as an impurity). For example, in some embodiments, the concentration index can be characterized by the impurity flow rate per unit time; or, in other embodiments, the concentration index can also be characterized by the amount of impurities discharged per unit time; or, in yet other embodiments, the concentration index can also be characterized by the impurity concentration per unit gas.

[0075] Herein, "grid material" is also referred to as "grid precursor", which refers to a material having multiple grid holes (or openings) distributed on the material plane, and a target to be formed (such as a microneedle) is arranged at the edge of the grid hole. Such grid holes can be arranged on the material plane to form a regular grid distribution. Among them, the preparation method that can form grid holes on the precursor is called a grid preparation method, and the grid preparation method in this article is preferably a 3D printing method.

[0076] Glassy carbon materials usually use a high-temperature sintering process with full-process gradient insulation (for example, it is often necessary to heat to a high temperature of about 1,000 degrees for insulation, such as a temperature of about 1000°C, etc.). In this article, the "centralized insulation process", also known as the low-temperature gradient insulation process, refers to the relatively concentrated insulation treatment of the key processes of the gridded material (such as stress elimination and pyrolysis carbonization). And in the centralized treatment link, the insulation treatment is directly guided by the technical results. That is, with stress elimination and pyrolysis carbonization as the goal, targeted insulation treatment is used to directly achieve the purpose of stress elimination and pyrolysis carbonization. Thereby reducing the influence of the heating rate on the deformation of the precursor in the subsequent heating stage, so that the subsequent heating stage (such as the third heating stage) can be heated to the target heating temperature as soon as possible without relying on insulation treatment, thereby simplifying the heating process.

[0077] In other words, the centralized heat preservation method based on the grid precursor provided by the present invention is different from the procedure of setting the heat preservation treatment in the low temperature range and the high temperature range in a dispersed manner. It directly aims at eliminating stress and pyrolysis carbonization, and specifically achieves the treatment requirements in the low temperature range through a limited number of heat preservation treatments (even two or three heat preservation treatments can achieve the purpose). And this centralized heat preservation treatment design in the low temperature range also unexpectedly makes the glassy carbon preparation get rid of the dependence on high temperature heat preservation treatment.

[0078] Moreover, it has been verified through experiments that the glassy carbon products obtained by the centralized heat preservation method can still obtain good quality (ie, defects such as foaming, breakage, and deformation are effectively controlled).

[0079] In this article, Figure 2b As shown in the figure, the "rapid heating process" means that for the third heating stage (i.e., after the heat preservation treatment of pyrolysis carbonization), a continuous and rapid heating method (for example, no need to perform heat preservation treatment again at multiple high temperature intervals such as 600°C and 1000°C) can be used to complete the final material property transformation and prepare high-purity glassy carbon. For example, the rapid heating rate can be greater than or equal to about 0.5°C / min, and even after the speed change, it can reach a heating rate of about 2°C / min.

[0080] Microneedles (MN) are a new type of physical penetration-promoting technology. For example, it can be composed of a plurality of micron-sized fine needle tips connected in an array on a base. Specifically, the shape of the "microneedles" on the microneedle patch is usually conical, and the top of the cone is the needle tip, and it can pierce the skin to a certain extent (for example, pierce the stratum corneum). The "microneedle-like structure" refers to other similar morphological designs that also have needle tips that can pierce the skin. For example, the bottom of the microneedle-like structure can be a variety of designs such as round, square, cross, and rice, and a needle tip is formed at its top.

[0081] Herein, a glassy carbon microneedle patch is provided, which includes: a main body, and a hollow area that can be arranged in the main body; the main body includes: a gridded substrate, a plurality of grid holes are arranged at intervals on the gridded substrate, and a plurality of microneedles or microneedle-like structures are arranged at the edges of the grid holes; wherein the glassy carbon microneedle patch is prepared by subjecting a gridded precursor to centralized heat-insulating pyrolysis treatment, and the gridded precursor is prepared from a carbon-based polymer.

[0082] Embodiment 1

[0083] like Figure 1-Figure 7 As shown, in order to reduce the defects such as foaming caused by the sintering process of glassy carbon products (such as microneedle structures), the present invention provides a method for preparing glassy carbon, wherein the glassy carbon is prepared by a centralized heat preservation method based on a gridded precursor, and accordingly, the method comprises the steps of:

[0084] S10: preparing a grid precursor using a carbon-based polymer raw material, wherein the grid precursor comprises a plurality of grid holes arranged at intervals, wherein the grid holes form a grid arrangement, wherein a plurality of objects to be formed are arranged at the edges of the grid holes.

[0085] For example, in some embodiments, the target to be formed is arranged at the intersection of the grid holes.

[0086] For another example, in some embodiments, the objects to be formed may also be arranged at intervals along the edges of the grid holes.

[0087] S20 places the gridded precursor in a heating box and starts the centralized heat preservation method, S20 includes:

[0088] S21: in the first heating stage, a stress relief temperature is selected to perform a heat preservation treatment on the gridded precursor to relieve stress on the gridded precursor; wherein the stress relief temperature is selected by a first selection rule;

[0089] S22: The temperature is raised to enter the second heating stage, and the pyrolysis carbonization temperature is selected in the second heating stage to perform heat preservation treatment on the grid precursor again, so that the grid precursor is pyrolyzed and carbonized. At this time, the target to be formed on the grid precursor and the grid holes shrink and deform during the pyrolysis and carbonization process, and the impurities generated during the process can be uniformly discharged outward by using the grid arrangement; the temperature of the second heating stage is higher than the temperature of the first heating stage; wherein the pyrolysis and carbonization temperature is selected by the second selection rule;

[0090] S30 In the subsequent third heating stage, the temperature is continuously raised from the pyrolysis temperature to the target heating temperature; and finally the carbon polymer is converted into glassy carbon.

[0091] In some embodiments, the first selection rule is:

[0092] The stress relief temperature is selected from the weight loss rate fluctuation temperature (equivalent to the recommended temperature); wherein the weight loss rate fluctuation temperature corresponds to the thermogravimetric differential curve (for example, DTG curve, see Figure 3 The thermogravimetric differential curve represents a curve showing the change in weight rate with temperature.

[0093] For example, taking the DTG curve as an example, the exemplary selection rule of the stress relief temperature is explained:

[0094] A DTG curve of the precursor is obtained, wherein the DTG curve is considered to be composed of multiple curve segments. At this time, the curvature change value of each curve segment before the pyrolysis temperature (for example, before about 350°C in this example) can be calculated (for example, when a curve segment involves multiple data points, the average curvature change of each data point can be calculated), and then the temperature value corresponding to the curve segment with the largest curvature change is selected as the weight loss rate fluctuation temperature.

[0095] Alternatively, in other embodiments, the user may pre-set a screening threshold, from which a finite number (e.g., 1, 2, etc.) of curve segments are screened out, and a finite number of optional weight loss rate fluctuation temperatures are correspondingly provided, wherein the curvature change value of the selected curve segment falls within the screening threshold.

[0096] In some embodiments, if there are multiple weight loss rate fluctuation temperatures, it is preferred to use two heat preservation treatments for stress relief. For example, if there are multiple weight loss rate fluctuation temperatures, two (or more) stress relief temperatures can be selected from the multiple weight loss rate fluctuation temperatures at intervals to avoid frequent heat preservation treatments in a single temperature interval.

[0097] The second selection rule for selecting the pyrolysis temperature is:

[0098] The pyrolysis temperature is selected from the weight loss fluctuation temperature (equivalent to the recommended temperature); wherein the weight loss fluctuation temperature corresponds to one or more temperature values ​​corresponding to the curve segment with the largest curvature change in the interval where the slope of the thermogravimetric analysis curve (e.g., TGA curve) gradually decreases. The thermogravimetric analysis curve is used to represent the relationship between weight change and temperature, and is also called a thermal weight loss curve.

[0099] For example, taking the TGA curve (as shown in the first curve) as an example, the selection of the pyrolysis temperature is exemplified as follows:

[0100] The TGA curve can also be considered as consisting of several curve segments. In the interval where its slope gradually decreases (for example, the interval before approximately 425°C), the curve segment with the largest slope change is selected, and the corresponding temperature is the weight loss fluctuation temperature. The pyrolysis temperature thus selected is approximately 350°C.

[0101] For example, in some embodiments, the temperature corresponding to a data point with the largest curvature change in the thermogravimetric analysis curve (i.e., the slope difference between the current data point and the previous data point is the largest compared to the slope difference between any two adjacent data points in the curve) can also be selected as the weight loss fluctuation temperature.

[0102] In this embodiment, only one insulation treatment for stress relief can be used in combination with one insulation treatment for pyrolysis and carbonization, so that the precursor can undergo relatively concentrated deformation at a relatively low pyrolysis and carbonization temperature (for example, insulation treatment is only performed within 350°C in Verification Example 1), thereby reducing the influence of the heating rate in the third heating stage on the deformation of the precursor.

[0103] Of course, in other embodiments, in order to achieve more uniform stress relief and avoid improper deformation under stress relief, when there is a first number of weight loss rate fluctuation temperatures, and the first number is greater than or equal to 2, the S21 includes the steps of:

[0104] A second number of weight loss rate fluctuation temperatures are selected from the first number of weight loss rate fluctuation temperatures at intervals, and a second number of stress relief temperatures are correspondingly obtained (for example, a stress relief temperature is correspondingly set for each weight loss rate fluctuation temperature), wherein the second number is less than or equal to the first number, and the stress relief temperatures at least include: a first stress relief temperature and a second stress relief temperature;

[0105] In the first heating stage, a first stress relief temperature is used for heat preservation treatment, so as to perform a first stress relief on the gridded precursor;

[0106] The temperature is continuously raised from the first stress relief temperature to the second stress relief temperature for heat preservation, so as to perform a second stress relief on the gridded precursor.

[0107] Therefore, in this embodiment, in the case where stress elimination is difficult, multiple heat preservation treatments can be used to eliminate stress.

[0108] Furthermore, it is understandable that the stress relief temperature (or pyrolysis carbonization) of the material is not a single temperature value, and as the material type changes or external processing conditions change, those skilled in the art can flexibly adjust the actual stress relief temperature or pyrolysis carbonization temperature according to the weight loss rate fluctuation temperature or the weight loss fluctuation temperature based on actual conditions.

[0109] For example, in some embodiments, the stress relief temperature has a certain deviation from the given weight loss rate fluctuation temperature (eg, the deviation is ±1° C., ±5° C., ±10° C., ±15° C., etc.).

[0110] Of course, in actual application, the weight loss rate fluctuation temperature or the weight loss fluctuation temperature can also be obtained from the existing thermogravimetric analysis related data, as long as the purpose of eliminating stress and pyrolysis and carbonization is achieved.

[0111] In some embodiments, S30 includes the steps of:

[0112] S31: obtaining conversion information for converting the heating rate, wherein the conversion information includes: a conversion temperature C4, and / or a conversion time;

[0113] S32 When the temperature is increased from the pyrolysis temperature C2 to the switching temperature C4 according to the first setting sub-speed VIII-1, or when the heating time is at the switching moment, the heating speed is converted from the first setting sub-speed VIII-1 to the second setting sub-speed VIII-2.

[0114] S33: The temperature is raised to the target heating temperature C5 according to the second setting sub-speed VIII-2; wherein the second setting sub-speed VIII-2 is greater than the first setting sub-speed VIII-1.

[0115] In some embodiments, the setting range of the first setting sub-speed VIII-1 is approximately 0.1-1°C / min, and the setting range of the second setting sub-speed VIII-2 is approximately 1-3°C / min.

[0116] In order to improve the quality of glassy carbon (such as reducing defect area and improving strength), the present invention proposes a centralized heat preservation method based on a gridded precursor. Different from the existing full-process gradient heat preservation process, the present invention designs the following preparation stages for glassy carbon preparation:

[0117] (1) Grid preparation stage; (2) Based on the technical results, concentrated stress relief and pyrolysis carbonization are directly carried out in the low temperature area; (3) Continuous heating method is directly adopted to increase the temperature to the target heating temperature.

[0118] The present invention adopts the cooperation of stages (1) to (3), which can not only effectively improve the uniformity of the stress relief process of the precursor during the heating stage (avoiding cracks or adverse deformation caused by stress), but also alleviate the surface damage that may be caused by major deformation processes such as pyrolysis and carbonization of the material and continuous heating.

[0119] In addition, the present invention reduces the deformation effect of the heating method (such as speed) on the precursor in the high temperature stage to a certain extent by combining the grid design with the centralized heat preservation method. This eliminates the dependence on high temperature heat preservation treatment and reduces the process cost. And it has been verified by experiments, for example Figure 5 As shown, there are very few defects such as blistering, deformation or breakage on the surface of the microneedle patch.

[0120] Furthermore, in order to facilitate the industrial application of the centralized insulation method, the temperatures of each insulation treatment for the low-temperature insulation of the gridded precursor can be directly obtained from the relevant data of thermogravimetric analysis to assist users in quickly exploring the preparation conditions for low-temperature gradient insulation.

[0121] It is understandable that in order to improve the accuracy and reliability of temperature selection, the head interval of the thermal decomposition curve (such as TGA or DTG) is usually discarded (for example, depending on the type of material or the difference in thermal decomposition analysis instruments, the curve segment with a temperature below about 50°C may be discarded), and then the effective interval of the curve is analyzed.

[0122] In some embodiments, the set curve segment may be the length of one data point or multiple data points.

[0123] The following provides a verification example 1 to illustrate the exemplary preparation steps of the glassy carbon microneedle patch of the present invention:

[0124] The 3D printing technology based on the principle of photopolymerization is used to prepare the photosensitive resin as the raw material, and the grid precursor is printed. Among them, the line width of the grid hole of the grid precursor (that is, the edge width of the grid hole, or the width L1 of the edge side wall of the grid hole) is 0.6mm, the size of the grid hole (equivalent to the line spacing) is 1mm, and the radius of the body (that is, the radius size of the edge of the precursor) is 10mm.

[0125] The grid precursor is heated in a heating box (such as a high temperature furnace) to convert the photosensitive resin into glassy carbon. The heating process mainly includes the following three stages:

[0126] First heating stage: step 1) heating to a first stress relief temperature C1 at a first set speed VI (1.5°C / min), and keeping at the first stress relief temperature C1 for a first time period T1 (30 min). At this time, the first stress relief temperature selected by the first selection rule is 150°C;

[0127] Second heating stage: step 2) heating to the pyrolysis temperature C2 at the second set speed VII (1°C / min), and maintaining the temperature at the pyrolysis temperature C2 for a second time T2 (120 min), wherein the pyrolysis temperature C2 obtained by the second selection rule is 350°C; the meshed precursor can shrink and deform relatively uniformly during this process;

[0128] The third heating stage: Step 3) After the two insulation treatments in the low-temperature zone are completed, the third heating stage of continuous heating is entered; specifically, the temperature is directly increased to the target heating temperature C5 (1000°C) according to the third set speed VIII (0.5°C / min), so that the grid precursor is converted from a carbon polymer to a glassy carbon material.

[0129] In this verification example 1, a grid design is adopted for the precursor, and only two key insulations are carried out in the low temperature range, which specifically achieves the purposes of stress elimination, pyrolysis carbonization, etc., eliminating the high-temperature insulation process. And the defect area (or defect generation rate) of the prepared grid microneedle can also be effectively controlled within 1% (the product quality is excellent). That is, the surface of the grid microneedle has good continuity, without defects such as foaming, cracks, deformation, etc., and because it also has high strength, it is suitable for actual industrial application needs.

[0130] It should be noted that the defect area (i.e., the percentage of defect area to the total surface area of ​​the meshed microneedles) was used in this experiment to evaluate the product quality of the meshed microneedles. When the defect area is 0-5%, the product quality is excellent; when the defect area is 5-15%, the product quality is good; when the defect area exceeds 15%, the product quality is poor.

[0131] For another example, in some embodiments, since the present invention reduces the dependence of the third heating stage on the heating rate, variable speed heating can be performed in the third heating stage.

[0132] The recommended speed change point (equivalent to the recommended temperature) for the temperature rise rate conversion can be the temperature corresponding to the data point where the slope of the thermogravimetric analysis curve is 0 or approximately 0 (e.g., within about ±0.001) during the process of gradually increasing the slope, such as Figure 3The recommended speed change point obtained in is about 600° C. Moreover, the actual speed change point selected is preferably not lower than the recommended speed change point (or generally only within 1° C., 5° C., 10° C., etc. below the recommended speed change point).

[0133] The speed-changing heating effect is verified by verification example 2 and comparative example 1:

[0134] In this verification example 2, the same gridded precursor as in verification example 1 is selected for centralized heat preservation treatment. The centralized heat preservation treatment includes:

[0135] The first heating stage: the temperature is raised to the first stress relief temperature C1 (150°C) at the first set speed VI (1.5°C / min), and kept at the first stress relief temperature for 30 minutes; the temperature is raised to the second stress relief temperature C3 (250°C) at the fourth set speed VIV (1°C / min), and kept at the second stress relief temperature for 60 minutes;

[0136] The second heating stage: heating from 250°C to 350°C at a heating rate of 1°C / min and keeping the temperature for 120 minutes;

[0137] The third heating stage: the temperature is increased from 350°C at a rate of 0.5°C / min, and then increased from 600°C to 1000°C at a rate of 2°C / min.

[0138] The surface state of the product prepared in Verification Example 2 can also be found in Figure 5 As shown. It can be seen that the gridded microneedles prepared by the present invention still have a good surface morphology even at a microscopic angle.

[0139] Comparative Example 1

[0140] The difference between the comparative example 1 and the verification example 2 in the preparation process is shown in Table 1:

[0141] Table 1

[0142]

[0143] In some embodiments, the method further comprises the steps of:

[0144] S200 When the glassy carbon preparation enters the concentrated heat preservation method stage (preferably the second heating stage or the third heating stage), the concentration index of impurities discharged through the exhaust duct of the heating box is monitored; wherein the impurities include: first-class impurities, and the first-class impurities include one or more of the following: carbon monoxide, carbon dioxide, nitric oxide, nitrogen dioxide and nitrogen;

[0145] S201 automatically adjusts the centralized heat preservation method according to the concentration index and the current state of the centralized heat preservation method; wherein the concentration index includes: a first concentration index for characterizing the concentration of the first type of impurities; accordingly, S201 includes the steps of:

[0146] S11: when the centralized heat preservation method enters the pyrolysis temperature and reaches the first set time but does not reach the second time length T2, and the first concentration index belongs to the first concentration threshold range X1, a first time reduction signal is sent to the gradient control module (or control unit) of the heating box, wherein the gradient control unit can reduce the second time length T2 in response to the first time reduction signal;

[0147] S12 When the centralized insulation method enters the pyrolysis temperature and reaches or exceeds the second time length T2, and the first concentration index belongs to the corresponding second concentration threshold range X2, a first delay signal is sent to the control unit, wherein the control unit can extend the second time length T2 in response to the first delay signal.

[0148] As a preferred embodiment, the present invention selects the concentration of nitrogen (or a gas containing nitrogen) as the first concentration indicator.

[0149] In some embodiments, the second type of impurities includes: tar.

[0150] In the centralized insulation method, the second type of impurities discharged from the heating box can also be monitored to obtain a second concentration index of the second type of impurities, and the second concentration index, the first concentration index and the current process status can be used to monitor and adjust parameters.

[0151] It is understood that the temperature of the heat preservation treatment is not only directly determined by the thermogravimetric analysis results of the meshed precursor (such as Figure 3 It can also be obtained by analyzing the empirical value collected by engineers after process debugging.

[0152] In this embodiment, it is preferred to use finite factors such as nitrogen and second-class impurities to monitor and automatically adjust the centralized heat preservation method. This automated adjustment process based on finite factors can also reduce the accuracy requirements of users in setting process parameters in the early stage to a certain extent.

[0153] For example, at the beginning of preparation, only a rough insulation treatment temperature can be selected based on the pyrolysis data (or the insulation temperature can be preliminarily selected based on the engineer's experience), and then the insulation treatment temperature can be relatively accurately adjusted according to the actual processing status through the automated adjustment process, thereby assisting engineers to quickly explore the preparation conditions and reduce the process application cost to a certain extent.

[0154] In some embodiments, the steps include:

[0155] During the heating stage of the gridded precursor, an inert gas is introduced into the heating box to exhaust the impurities out of the heating box through the exhaust pipe. The introduction rate of the inert gas is about 10-60 cm 3 / min;

[0156] The concentration index of the impurities is collected through a gas monitoring device connected to the exhaust pipe.

[0157] In order to reduce the influence of stress elimination and rapid deformation of the grid precursor during pyrolysis and carbonization during the centralized heat preservation method, the grid precursor is symmetrically designed. For example, in some embodiments, the grid precursor includes: a main body, and a hollow area arranged in the middle of the main body, and the main body is evenly arranged around the edge of the hollow area. Among them, the evenly arranged grid holes are matched with the hollow area arranged along the middle, so that an impurity discharge space is formed on the grid precursor, which is conducive to the uniform discharge of impurities.

[0158] For example, in some embodiments, the edge of the body may be in one or more of the following shapes: circular, oval, or rounded rectangular.

[0159] For example, in some embodiments, the base of the object to be formed may be in one or more of the following shapes: circular, square, cross, or cross.

[0160] In some embodiments, the steps include:

[0161] Providing a carbon-rich photopolymer material as a raw material, and obtaining process parameters for preparing the gridded precursor according to the photopolymer material, wherein the process parameters include one or more of the following: grid hole size, size of a target to be formed, and thickness of the gridded precursor;

[0162] The process parameters are input into a 3D printing system based on photopolymerization, and the photopolymerization material is discretized and stacked by the 3D printing system to prepare a corresponding gridded precursor.

[0163] For example, a grid precursor can be prepared by 3D printing technology based on the principle of photopolymerization and photocuring technology based on micro-template technology. Among them, 3D printing technology based on photopolymerization is used to prepare microneedles, including laser stereolithography (SLA), two-photon polymerization (TPP), digital light processing (DLP), liquid crystal display (LCD) polymerization, continuous liquid interface manufacturing (CLIP), static light projection printing (SOPL) and one or more. This type of technology is based on digital models and manufactures three-dimensional entities in a discrete and stacked manner by regulating the light source.

[0164] For another example, a polymer microneedle precursor can be prepared by photocuring molding technology based on a micro-template process. A mold can be pre-made by etching, 3D printing, etc., and then a microneedle structure can be obtained by filling a photopolymer material, exposing and curing, and demolding.

[0165] The gridded microneedle product prepared in this application using 3D printing technology, precursor optimization design and centralized insulation method has good continuity on the product surface (almost no obvious defects, uniform mechanical properties), improved strength and conductivity, and improved reliability and service life in actual application.

[0166] In this embodiment, a 3D printing process is introduced for the preparation of precursors to facilitate the customized production of microneedle products. And through experimental verification, the grid design used in this application is combined with the low-temperature gradient insulation process to effectively alleviate or reduce the defects that may occur in the sintering process of the precursor obtained by 3D printing.

[0167] Of course, in other embodiments, the mold method can also be used to manufacture the precursor of the microneedle.

[0168] Further, in order to improve the synergy between the grid design and the low temperature gradient insulation process, when the grid precursor adopts a circular ring or rounded corner design, and the edge width L1 of the grid hole of the precursor is less than or equal to about 2 mm, and the radius L2 of the main body is less than or equal to about 100 mm, the overall morphology of the grid precursor remains good after the low temperature gradient insulation process, without obvious defects. The verification results are shown in Table 2.

[0169] Table 2

[0170]

[0171] Note: The other preparation processes of the gridded precursor in Table 2 are the same as those in Verification Example 1;

[0172] The experimental data in Table 2 further show that the gridding process design provided by the embodiment of the present invention can achieve uniform stress elimination and proportional shrinkage deformation (eg, the shrinkage rate of each local area is about 25%), and the defect area of ​​the final product is significantly reduced.

[0173] On the contrary, see Figure 8 As shown, a preparation process similar to that of Verification Example 1 was used to perform low-temperature gradient processing on a circle with a radius of 8 mm and a rectangle with a length of 8 mm (which did not adopt a grid design). The prepared microneedles were severely deformed and could not meet the needs of actual applications.

[0174] Therefore, based on the grid process design proposed in this embodiment, when it needs to be applied to different process applications, users can also adjust the product shape and size relatively flexibly in terms of morphological design, grid distribution, etc. according to actual product requirements (such as preparing medical devices, sensors and other components of different sizes and performances) to ensure the reliability of the final molded product.

[0175] In the present invention, the grid design is used to facilitate the formation of uniform stress distribution on the precursor structure and the formation of space for uniform impurity discharge; at the same time, the corresponding centralized thermal insulation treatment is coordinated with the uniform stress distribution and the uniform impurity discharge space, which can successively and stage-by-stage realize the core processes such as uniform and stable stress elimination and pyrolysis carbonization.

[0176] In addition, the present invention utilizes the spatial design for uniform impurity discharge in conjunction with centralized heat preservation treatment, which can concentrate the main stages of pyrolysis and carbonization (first, concentration in terms of time and temperature range, and second, relatively concentrated exhaust from the exhaust perspective), so that users can more easily achieve centralized monitoring of the pyrolysis and carbonization process during the production process.

[0177] Embodiment 2

[0178] The centralized heat preservation method in the present invention is to select centralized gradient heat preservation in the low temperature area and to quickly heat up in the subsequent high temperature stage. In addition, in order to accelerate the process in the high temperature stage, the present invention also provides a preparation method introducing a variable speed adjustment process, and the preparation method may include the same or similar steps as in Example 1.

[0179] In some embodiments, the preparation method further comprises the steps of:

[0180] Monitor and collect impurity concentration indicators;

[0181] When the concentration index is lower than a set first threshold range A, a first speed change signal is sent to the heating box (with a gradient control unit);

[0182] The heating box converts the current first setting sub-speed (ie, the first heating speed) to the second setting sub-speed (ie, the second heating speed) in response to the first speed change signal.

[0183] For example, in some embodiments, the first setting sub-speed is approximately 0.5° C. / min, and the second setting sub-speed is approximately 2° C. / min.

[0184] In this embodiment, the concentration index can be used to control the variable speed heating process in real time.

[0185] It is worth noting that, unlike the glassy carbon preparation process of the prior art, the present invention focuses on the glassy carbon preparation of microneedle-shaped products. For microneedle products with small sizes, they are prone to produce adverse deformation due to excessive shrinkage speed during the actual sintering process, which in turn affects the surface morphology and strength of the final microneedle, making it difficult to apply in practice.

[0186] However, the present invention reduces the influence of the heating rate on the third heating stage to a certain extent by proposing a precursor grid design and centralized heat preservation treatment, and accordingly, this also reduces the volatility of the discharged impurity content in the third heating stage to a certain extent. Therefore, in this embodiment, by combining the monitoring of key impurity parameters in the third heating stage with centralized heat preservation, the reliability and stability of the monitoring results can be guaranteed, thereby effectively optimizing product quality.

[0187] Embodiment 3

[0188] In order to improve the reliability of the centralized insulation method (i.e., the low-temperature gradient insulation process) and reduce the labor cost in the preparation process to a certain extent, the present invention also provides an automated monitoring system for glassy carbon preparation, such as Fig. 9 As shown, including:

[0189] A gradient control module 10 (or control unit) for controlling the heating process of the heating box;

[0190] Low temperature gradient process monitoring subsystem (also known as centralized insulation monitoring subsystem), which includes:

[0191] The impurity monitoring module 20 is connected to the exhaust pipe of the heating box and is configured to monitor the concentration index of impurities discharged through the exhaust pipe; wherein the impurities include: first-class impurities, and the first-class impurities include one or more of the following: carbon monoxide, carbon dioxide, nitric oxide, nitrogen dioxide and nitrogen;

[0192] The signal adjustment module 21 is configured to automatically adjust the centralized heat preservation method according to the concentration index and the current state of the centralized heat preservation method; wherein the concentration index includes: a first concentration index for characterizing the concentration of the first type of impurities; accordingly, the signal adjustment module 21 includes:

[0193] The first regulating unit 11 is configured to send a first time reduction signal to the gradient control module of the heating box when the concentrated heat preservation method enters the pyrolysis temperature and reaches the first set time and does not reach the second time length T2 (i.e., the preset pyrolysis heat preservation time length), and the first concentration index belongs to the first concentration threshold range X1, wherein the control unit can reduce the second time length T2 in response to the first time reduction signal;

[0194] And / or, the second adjustment unit 12 is configured to send a first delay signal to the control unit when the centralized insulation method enters the pyrolysis temperature and reaches or exceeds the second time length T2, and the first concentration index belongs to the corresponding second concentration threshold range X2, wherein the control unit can extend the second time length T2 in response to the first delay signal.

[0195] When the first concentration index enters the first concentration threshold range X1, the heat preservation is ended and the rapid heating stage is entered.

[0196] In some embodiments, the signal conditioning module 21 further includes:

[0197] The speed change unit 13 is configured to send a first speed regulation signal to the control unit when the centralized insulation method heats up from the pyrolysis temperature to the target heating temperature and monitors that the first concentration index belongs to the third concentration threshold range X3, wherein the control unit can speed up the third set speed VIII (i.e., the heating speed in the third heating stage) in response to the first speed regulation signal.

[0198] In some embodiments, the impurity monitoring module 20 is further configured to monitor the second type of impurities discharged from the heating box during the centralized heat preservation method stage.

[0199] In some embodiments, the signal conditioning module 21 further includes:

[0200] The comprehensive adjustment unit 14 is configured to send a first time reduction signal to the control unit of the heating box when the heating box enters the pyrolysis temperature and reaches the first set time but does not reach the second time length T2, and the first concentration index belongs to the first concentration threshold range X1, and the second concentration index belongs to the fourth concentration threshold range X4, wherein the control unit can reduce the second time length T2 in response to the first time reduction signal.

[0201] The first, second and fifth concentration threshold ranges are sequentially set according to the concentration of the first type of impurities, and the fourth and sixth concentration threshold ranges are sequentially set according to the concentration of the second type of impurities.

[0202] In some embodiments, the signal adjustment module 21 also includes: a user adjustment unit 15, which is configured to send a first prompt signal to the user when the heating box enters the pyrolysis temperature and when the first concentration index belongs to the fifth concentration threshold range X5, or the second concentration index belongs to the sixth concentration threshold range X6, to prompt the user to adjust the centralized insulation method of the gradient control module.

[0203] In this embodiment, the pyrolysis temperature holding time can be dynamically adjusted according to the ranges corresponding to the first and second concentration indicators. For example, when the concentration indicator is relatively small (i.e., the first concentration indicator is within the first concentration threshold range, and the second concentration indicator is within the fifth concentration threshold range), the pyrolysis temperature holding time is automatically reduced.

[0204] When at least one concentration index is too high, for example, when the first concentration index belongs to the fifth concentration threshold range X5, or when the second concentration index belongs to the sixth concentration threshold range X6, manual borrowing is urgently introduced.

[0205] Alternatively, in some embodiments, the comprehensive adjustment unit 14 is also configured to send a first delay signal to the control unit in the same manner when the first concentration index belongs to the second concentration threshold range, or the second concentration index is in the seventh concentration threshold range (i.e., between the fourth concentration threshold range and the sixth concentration threshold range), and correspondingly, the control unit can extend the second time length T2 in response to the first delay signal.

[0206] In the actual processing process, due to different processing environments, equipment models and product requirements, the preparation conditions may be frequently adjusted. The present invention adopts an automated adjustment process to adjust only key nodes (such as the pyrolysis insulation time in the low-temperature area), that is, it can flexibly and dynamically adjust the preparation conditions, and can also use limited factors to perform multi-level adjustments, so as to perform more accurate automatic adjustment of the pyrolysis insulation time without increasing the application cost, thereby reducing the necessity of manual user participation.

[0207] In some embodiments, the invention further includes: a grid-based process monitoring subsystem, wherein the grid-based process monitoring subsystem includes:

[0208] The first view acquisition module 30 is configured to acquire morphological information of the gridded precursor, wherein the morphological information includes: a first image for displaying the size characteristics of the gridded precursor;

[0209] The view analysis module 40 is configured to obtain characteristic indicators of the grid precursor according to the morphological information; wherein the grid precursor includes: a main body, and a hollow area arranged in the middle of the main body; the characteristic indicators include a first characteristic indicator for standardizing the size characteristics, and the first characteristic indicator includes: a line width of a grid hole;

[0210] The execution condition judgment module 50 is configured to judge whether the gridded precursor meets the preset execution condition of the centralized insulation method (such as the execution condition is the standard line width of the grid hole) according to the characteristic index.

[0211] In some embodiments, the morphological information further includes: a second image for displaying the morphological features of the gridded precursor; accordingly, the characteristic index further includes: a second characteristic index obtained from the second image for indicating the number of defects.

[0212] For example, in some embodiments, an image dimension measuring instrument may be used to obtain corresponding dimension data.

[0213] In some embodiments, the execution condition determination module 50 includes:

[0214] The first judging unit 51 is configured to judge the monitoring level of the centralized heat preservation method according to the first characteristic index, and is divided into: first-level monitoring; second-level monitoring according to the difference between the first characteristic index and the standard size characteristic;

[0215] The second judgment unit 52 is configured to judge the monitoring level of the centralized heat preservation method according to the second characteristic index, and is divided into: first-level monitoring; second-level monitoring according to the difference between the second characteristic index and the standard morphological feature;

[0216] An execution risk analysis unit 53 is configured to determine the execution risk level of the centralized heat preservation method according to the monitoring level and the monitoring level; wherein, when the monitoring level and the monitoring level are both level one, the execution risk level is low, and a first start signal is sent to the gradient control module, and the gradient control module starts the centralized heat preservation method in response to the first start signal, and starts the signal adjustment module 21;

[0217] When the monitoring level is level one and the monitoring level is level two, or when the monitoring level is level two and the monitoring level is level one, and the execution risk level is medium, a second start signal is sent to the gradient control module, and the gradient control module is started in response to the second start signal and executes a centralized heat preservation method in response to a gradient control parameter input by a user;

[0218] When the monitoring level and the surveillance level are both level two, the execution risk level is high at this time, a prompt signal is sent to the user, and a control signal input by the user in real time is received within a set time.

[0219] In some embodiments, when the difference between a first characteristic indicator (such as the line width of a grid hole) and a standard size characteristic (such as a preset standard line width) is less than or equal to a preset first difference, a first-level monitoring (mode) is selected; when the difference is greater than the first difference and less than a preset second difference, a second-level monitoring (mode) is selected.

[0220] In some embodiments, when the difference between the second characteristic indicator (such as the number of defects) and the standard morphological characteristic (standard number of defects) is less than or equal to a preset third difference, the first-level monitoring (mode) is selected, and when the corresponding difference is greater than the third difference and less than the preset fourth difference, the second-level monitoring (mode) is selected.

[0221] For example, in some embodiments, when faced with batch process production, before using a batch of gridded precursors for a centralized insulation method, some gridded precursors can be selected as test samples, and the monitoring level (or surveillance level) under the low-temperature gradient insulation process can be determined through the gridded process monitoring subsystem, thereby improving the effectiveness of the entire preparation process.

[0222] In addition, the present embodiment uses two clear indicators, line width and defect quantity, to quickly and standardizedly evaluate the quality of the test sample, thereby flexibly linking with the subsequent low temperature gradient process. For example, when the monitoring and surveillance levels of the test sample are both level one, it is preferred to start the signal adjustment module 21 to dynamically adjust the low temperature process.

[0223] In some embodiments, the defect quantity may also be characterized by defect area.

[0224] It should be noted that in this embodiment, "monitoring" and "monitoring" have the same meaning, and different expressions are used here only for the convenience of distinction.

[0225] In this embodiment, in order to improve the accuracy and reliability of automated monitoring, a monitoring scheme based on multi-level dynamic regulation of different types of parameters is proposed. In addition, in order to reduce the difficulty of the monitoring process, the present invention mainly monitors the key dimensional features (such as the width of the grid holes) in the grid technology and the key output impurities (such as nitrogen) in the centralized insulation method, thereby using a limited combination of factors to form a multi-level monitoring mode. Therefore, this multi-level dynamically adjusted monitoring scheme can not only use a combination of limited factors to reduce the possibility of process failure caused by monitoring errors (or failure of a single monitoring device); at the same time, it can also avoid the monitoring and analysis difficulties that may be brought about by multi-factor monitoring to a certain extent (on the contrary, the present invention uses limited and standardized factor comparisons to quickly discover difficult problems (such as when the risk level is high), and then notify the user in the first time, realizing the coordination of automated control and manual monitoring).

[0226] In some embodiments, the system further includes: an evaluation subsystem including:

[0227] The second image acquisition module 60 is configured to acquire a third image of the gridded microneedle product prepared from the gridded precursor;

[0228] An image comparison module 70 is configured to compare the third image with the first image to obtain shrinkage data and morphological difference data of the gridded microneedle product, wherein the morphological difference data is a difference in deformation ratio between the gridded precursor and the gridded microneedle product at at least two points;

[0229] The quality assessment module 80 is configured to perform product quality analysis on the gridded microneedle product according to the shrinkage data and the morphology difference data.

[0230] For example, in some embodiments, when the shrinkage data and the morphological difference data are both within the preset standard range, it is considered that the product quality meets expectations and the current preparation process also meets the specifications.

[0231] In this embodiment, the image comparison technology can also be used to quickly evaluate the final prepared product. If the product quality is monitored to be significantly lower than the expected quality, the user can be notified in time to make process adjustments.

[0232] Embodiment 4

[0233] The present invention also provides a semi-automatic monitoring method for glassy carbon preparation, comprising the steps of:

[0234] S200 When the glassy carbon preparation enters the centralized heat preservation method step, the concentration index of impurities discharged through the exhaust pipe of the heating box is monitored; wherein the impurities include: first-class impurities, and the first-class impurities include one or more of the following: carbon monoxide, carbon dioxide, nitric oxide, nitrogen dioxide and nitrogen;

[0235] S201 automatically adjusts the centralized heat preservation method according to the concentration index and the current state of the centralized heat preservation method; wherein the concentration index includes: a first concentration index for characterizing the concentration of the first type of impurities; accordingly, S201 includes the steps of:

[0236] S11: when the low-temperature gradient insulation process enters the pyrolysis temperature and reaches the first set time but does not reach the second time length T2 (i.e., the pyrolysis insulation time length), and the first concentration index belongs to the first concentration threshold range X1, a first time reduction signal is sent to the gradient control module of the heating box, wherein the control unit can reduce the second time length T2 in response to the first time reduction signal;

[0237] S12: When the heating box enters the pyrolysis temperature and reaches or exceeds the second time length T2, and the first concentration index belongs to the corresponding second concentration threshold range X2, a first delay signal is sent to the control unit, wherein the control unit can extend the second time length T2 in response to the first delay signal.

[0238] In some embodiments, the S201 further includes the steps of:

[0239] S13 When the heating box is heated from the pyrolysis temperature to the heating temperature, and when it is monitored that the first concentration index belongs to the third concentration threshold range X3, a first speed regulation signal is sent to the control unit, wherein the control unit can increase the third set speed VIII (i.e., the heating speed in the third heating stage) in response to the first speed regulation signal.

[0240] In some embodiments, S200 further includes the steps of:

[0241] In the centralized heat preservation method steps (such as the second heating stage and the third heating stage), the second type of impurities discharged from the heating box are monitored.

[0242] In some embodiments, the S201 includes the steps of:

[0243] When the heating box enters the pyrolysis temperature and reaches the first set time but does not reach the second time length T2, and the first concentration index belongs to the first concentration threshold range X1, and the second concentration index belongs to the fourth concentration threshold range X4, a first time reduction signal is sent to the control unit of the heating box, wherein the control unit can reduce the second time length T2 in response to the first time reduction signal;

[0244] And / or, after the heating box enters the pyrolysis temperature, and when the first concentration index belongs to the fifth concentration threshold range X5, and the second concentration index belongs to the sixth concentration threshold range X6, a first prompt signal is sent to the user to prompt the user to adjust the centralized insulation method of the gradient control module.

[0245] In some embodiments, before S200, the step further includes:

[0246] S203 collects morphological information of the gridded precursor, the morphological information comprising: a first image for displaying the size characteristics of the gridded precursor;

[0247] S204: acquiring characteristic indicators of the gridded precursor according to the morphological information; wherein the gridded precursor comprises: a main body, and a hollow area arranged in the middle of the main body; the characteristic indicators comprise a first characteristic indicator for standardizing the size characteristics, and the first characteristic indicator comprises: an edge width of a grid hole on the main body, and a radius of the main body;

[0248] S205 determines whether the gridded precursor meets the preset execution conditions of the low-temperature gradient insulation process according to the characteristic index.

[0249] In some embodiments, the morphological information further includes: a second image for displaying the morphological features of the gridded precursor; accordingly, the characteristic index further includes: a second characteristic index for indicating the number of defects. The number of defects can be represented by the defect area. The defects may include: foaming, breakage, deformation, etc.

[0250] The defect area can be calculated by image comparison. For example, the points with pixel differences between the test sample photo (i.e., the surface photo of the prepared glassy carbon product) and the standard sample photo (the surface photo of the glassy carbon product selected as the standard sample) can be used as defect areas to calculate the defect area. Alternatively, other automated defect detection equipment or automated defect detection technology can be used to calculate the defect area (or the number of defects).

[0251] In some embodiments, S205 includes the steps of:

[0252] S51 determines the monitoring level of the low temperature gradient insulation process according to the first characteristic index, and according to the difference between the first characteristic index and the standard size characteristic, there are: first-level monitoring; second-level monitoring;

[0253] S52 determines the monitoring level of the low temperature gradient insulation process according to the second characteristic index, and according to the difference between the second characteristic index and the standard morphological characteristic, there are: first-level monitoring; second-level monitoring;

[0254] S53 determines the execution risk level of the low-temperature gradient insulation process according to the monitoring level and the surveillance level;

[0255] Wherein, when the monitoring level and the surveillance level are both level 1, a first start signal is sent to the gradient control module, and the gradient control module starts the low-temperature gradient insulation process in response to the first start signal, and executes S200;

[0256] When the monitoring level is level one and the monitoring level is level two, or when the monitoring level is level two and the monitoring level is level one, a second start signal is sent to the gradient control module, and the gradient control module is started in response to the second start signal and performs a low-temperature gradient insulation process in response to the gradient control parameters input by the user (such as pyrolysis insulation time, heating speed of the third stage heating);

[0257] When the monitoring level and the surveillance level are both level 2, a prompt signal is sent to the user, and a control signal input by the user in real time is received within a set time.

[0258] In some embodiments, the steps include:

[0259] S206 collects a third image of the gridded microneedle product prepared from the gridded precursor;

[0260] S207: Comparing the third image with the first image to obtain shrinkage data and morphological difference data of the gridded microneedle product, wherein the morphological difference data is the difference in deformation ratio between the gridded precursor and the gridded microneedle product at at least two points;

[0261] S208: Perform product quality analysis on the gridded microneedle product according to the shrinkage data and the morphology difference data.

[0262] It should be noted that the set threshold or range adopted in the present invention can be adjusted by the user in combination with the actual process.

[0263] It should be noted that the temperature value actually selected in the present invention may be the recommended temperature or a value adjacent to the recommended temperature.

[0264] The microneedle product prepared by using the grid precursor and the heat preservation temperature in the present invention has multiple advantages such as strong rigidity, good biocompatibility, heat resistance, chemical resistance, good conductivity, high purity, etc. It can be applied not only to conventional solid and hollow microneedle arrays, but also to the preparation of parts for precision devices such as electrospinning nozzles, extrusion printing nozzles, brain-computer interfaces, biochemical sensors, etc.

[0265] It should be noted that, in this article, the terms "include", "comprises" or any other variations thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device. In the absence of further restrictions, an element defined by the sentence "comprises a ..." does not exclude the existence of other identical elements in the process, method, article or device including the element.

[0266] Through the description of the above implementation methods, those skilled in the art can clearly understand that the above-mentioned embodiment methods can be implemented by means of software plus a necessary general hardware platform, and of course by hardware, but in many cases the former is a better implementation method. Based on such an understanding, the technical solution of the present invention, or the part that contributes to the prior art, can be embodied in the form of a software product, which is stored in a storage medium (such as ROM / RAM, magnetic disk, optical disk), and includes a number of instructions for a computer terminal (which can be a mobile phone, computer, server, or network device, etc.) to execute the methods described in each embodiment of the present invention.

[0267] The embodiments of the present invention are described above in conjunction with the accompanying drawings, but the present invention is not limited to the above-mentioned specific implementation modes, which are merely illustrative rather than restrictive. Under the guidance of the present invention, ordinary technicians in this field can also make many forms without departing from the scope of protection of the present invention and the claims, all of which are within the protection of the present invention.

Claims

1. A method for preparing a glassy carbon microneedle patch, characterized in that: include: S10: preparing a grid precursor using a carbon-based polymer raw material, wherein the grid precursor comprises a plurality of grid holes arranged at intervals, the grid holes intersect each other to form a grid arrangement, and microneedles or microneedle-like structures to be formed are arranged at the edges of the grid holes; S20: placing the gridded precursor in a heating box and starting a centralized heat preservation method; And S20 includes: S21: In the first heating stage, a stress relief temperature is selected to perform heat preservation treatment on the gridded precursor to relieve stress on the gridded precursor; wherein the stress relief temperature is selected by a first selection rule; and the first selection rule is: the stress relief temperature is selected from the weight loss rate fluctuation temperature; and the weight loss rate fluctuation temperature corresponds to the temperature value corresponding to the data point with the largest curvature change in the thermogravimetric differential curve within the interval less than the pyrolysis carbonization temperature; S22 is heated to enter the second heating stage, and in the second heating stage, the pyrolysis carbonization temperature is selected to perform heat preservation treatment on the grid precursor again to make the grid precursor pyrolysis carbonized. At this time, the microneedles or microneedle-like structures to be formed on the grid precursor and the grid holes shrink during the pyrolysis carbonization process, and the impurities generated can be evenly discharged outward using the grid arrangement; wherein the pyrolysis carbonization temperature is selected by the second selection rule; the second selection rule is: the pyrolysis carbonization temperature is selected from the weight loss fluctuation temperature; wherein the weight loss fluctuation temperature corresponds to the temperature value corresponding to the curve segment with the largest curvature change in the interval where the slope of the thermogravimetric analysis curve gradually decreases; S30 In the subsequent third heating stage, the temperature is continuously raised from the pyrolysis carbonization temperature to the target heating temperature; and finally the grid precursor prepared from the carbon-based polymer is converted into a glassy carbon microneedle patch.

2. The preparation method according to claim 1, characterized in that: Also includes: During the heating stage of the gridded precursor, an inert gas is introduced into the heating box to protect the precursor and discharge the impurities; The concentration index of the impurities is collected through a gas monitoring device.

3. The preparation method according to claim 2, characterized in that: Also includes: In the third heating stage, when the concentration index of the impurity is monitored to be lower than the set concentration range, a switching time is selected according to the current time, wherein the difference between the switching time and the current time is less than the set difference range; At the conversion moment, the current first heating rate is increased to the second heating rate, and the temperature is continuously increased to the target heating temperature.

4. The preparation method according to claim 1, characterized in that: The carbon-based polymer includes: a carbon-rich polymer, wherein the carbon-rich polymer includes one or more of the following: polyurethane, epoxy resin, phenolic resin, polyacrylonitrile, polyimide, polystyrene, polytetrafluoroethylene, polyethylene, polyaniline, or a product obtained by further modifying the carbon-rich polymer; And / or, the preparation method of the gridded precursor includes: mold forming, and / or 3D printing.

5. The preparation method according to claim 1, characterized in that: The line width L1 of the grid holes in the grid precursor is less than or equal to 2 mm, and the radius L2 of the main body of the grid precursor is less than or equal to 100 mm.

6. The preparation method according to claim 1, characterized in that: The gridded precursor comprises: a main body, in which a hollow area is arranged; a plurality of grid holes are arranged on the main body at intervals, and the main body can be in one or more of the following shapes: circular, annular, elliptical, and rounded rectangular.

7. The preparation method according to claim 1, characterized in that: The base of the microneedle-like structure can be in one or more of the following shapes: circular, rectangular, cross-shaped, and 'P'-shaped.