A nickel-based powder brazing material and its preparation method and application in connecting homogeneous alloys or heterogeneous alloys

Through the design of nickel-based powder solder and the preparation of gas atomization method, combined with the regulation of alloy elements, welding defects and wear problems in the connection of high-temperature alloys and wear-resistant alloy parts are solved, and the high-temperature mechanical properties are improved and the weld seam is achieved. stability.

CN117817185BActive Publication Date: 2024-11-12INST OF METAL RESEARCH - CHINESE ACAD OF SCI
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310248080.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-03-15
Publication Date
2024-11-12
Estimated Expiration
2043-03-15

AI Technical Summary

Technical Problem

The existing high-temperature brazing materials are difficult to meet the connection needs of high-temperature alloys and wear-resistant alloy components in harsh environments, especially under high temperature and stress, welding defects and wear problems are prone to occur.

Method used

Using nickel-based powder solder, the spherical or nearly spherical alloy powder is prepared by adding elements such as Co, Cr, W, Mo, Al, Si, B, etc., and the structure is regulated during the vacuum brazing process. The formation of high melting point borides is carried out to improve the temperature bearing capacity of the weld and avoid the formation of low melting point eutectic structure.

Benefits of technology

It significantly improves the high-temperature mechanical properties of the brazed joint, enhances the tensile strength and wear resistance of the weld, reduces the risk of weld cracking, and is suitable for brazing connections between the same high-temperature alloys and high-temperature alloys and wear-resistant alloys.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117817185B_ABST
    Figure CN117817185B_ABST
Patent Text Reader

Abstract

The invention discloses a nickel-based powder brazing material, a preparation method thereof and an application thereof in the connection of homogeneous alloys or heterogeneous alloys, and belongs to the technical field of high-temperature brazing materials. The chemical composition (wt.%) of the brazing material is: Co 8.0-12.0%, Cr 8.0-12.5%, W 2.0-6.0%, Mo 1.3-3.5%, Al 1.5-6.5%, Si 0-4.0%, B 0.5-1.8%, Nb 0-5.0%, C 0-0.3%, and Ni balance. The brazing material is prepared by gas atomization method and is used for alloy brazing connection. The brazing temperature is 1200-1300°C and the brazing time is 10-90 minutes. The invention solves the temperature bearing problem of high-temperature alloy brazing connection joints and the high-performance connection problem between high-temperature alloys and wear-resistant alloys, and has important application value for the connection of parts that need to be in a high-temperature service environment.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of high-temperature brazing materials, and in particular to a nickel-based powder brazing material and a preparation method thereof and application in the connection of homogeneous alloys or heterogeneous alloys. The brazing material is suitable for vacuum brazing connection of high-temperature alloy base materials or high-temperature alloys and wear-resistant alloy base materials. Background Art

[0002] High-temperature alloys refer to highly alloyed iron-based, nickel-based or cobalt-based austenitic metal materials that can work for a long time at high temperatures above 600°C and under certain stresses. Since their introduction, they have been widely used in hot-end components of aircraft engines and various industrial gas turbines. However, due to the complex internal cooling structure used in the design of parts such as turbine blades and guide vanes, it is difficult to achieve their final structure with precision casting technology alone. Reliable brazing connection technology is required to achieve high-performance connection of high-temperature alloy blades and other high-temperature alloy components. In addition, the blade crown contact surface of the turbine blade is prone to severe wear, and it is also necessary to use reliable heterogeneous material brazing connection technology to braze the wear-resistant alloy material to the blade crown to reduce wear.

[0003] In recent years, due to the update of blade materials, changes in structure and increasingly harsh blade service environment, cracks in blade covers and wear-resistant blocks have occurred frequently. Existing high-temperature brazing materials can no longer meet their use requirements. Therefore, it is urgently necessary to develop new high-temperature brazing materials that are more suitable for high-temperature brazing and have excellent high-temperature performance to solve the problems of high-performance brazing connections of high-temperature alloy materials and high-performance brazing connections of high-temperature alloy materials and wear-resistant alloy materials. Summary of the invention

[0004] The purpose of the present invention is to provide a nickel-based powder brazing material, a preparation method thereof and an application in the connection of homogeneous alloys or heterogeneous alloys. The prepared powder brazing material is mainly used for high-temperature brazing (1200-1300°C), which can effectively solve the connection problem of homogeneous (same high-temperature alloy) or heterogeneous alloy (high-temperature alloy and wear-resistant alloy) parts working in harsh environments, and has important application value.

[0005] To achieve the above object, the technical solution of the present invention is as follows:

[0006] A nickel-based powder solder, which is a nickel-based alloy powder; the chemical composition of the solder is as follows by weight percentage: Co 8.0-12.0%, Cr 8.0-12.5%, W 2.0-6.0%, Mo 1.3-3.5%, Al 1.5-6.5%, Si 0-4.0%, B 0.5-1.8%, Nb 0-5.0%, C 0-0.3%, and Ni is the balance; wherein the powder solder is spherical or nearly spherical, and the particle size is not greater than 100 meshes.

[0007] The preparation process of the powder solder comprises the following steps:

[0008] (1) According to the composition of the solder, a mother alloy ingot of the solder is smelted in a vacuum induction furnace. The smelting process is: keeping at 1450-1570° C. for 1-5 min and pouring at 1390-1490° C.

[0009] (2) preparing the master alloy ingot into alloy powder by gas atomization method, wherein the process parameters of the gas atomization method are: powder spraying temperature of 1400-1550° C., mass flow rate of 2-6 kg / min, powder spraying gas of argon, and powder spraying pressure of 3-10 MPa;

[0010] (3) The prepared alloy powder is sieved to obtain alloy powder with a size not larger than 100 meshes, thereby obtaining the powder solder.

[0011] The powder solder alloy is used for brazing connection of homogeneous alloys or heterogeneous alloys. Homogeneous alloys refer to the same kind of high-temperature alloys, and heterogeneous alloys refer to high-temperature alloy materials and wear-resistant alloys; the wear-resistant alloys include Ni3Al-based wear-resistant alloys; Co-Cr-Mo, Co-Cr-W, Co-Nb-Cr and other cobalt-based wear-resistant alloys; and WC wear-resistant alloys.

[0012] During the brazing process, the brazing alloy powder is mixed into a paste using a water-based or oily binder and then applied to the part to be welded of the sample. The sample is placed in a vacuum brazing furnace for brazing connection. The brazing insulation time is 10 to 90 minutes. The tensile strength of the high-temperature alloy brazed joint at 980°C is not less than 600MPa; the tensile strength of the high-temperature alloy and wear-resistant alloy brazed joint at 980°C is not less than 200MPa.

[0013] The design ideas and principles of the present invention are as follows:

[0014] In the traditional high-temperature alloy brazing process, the residual liquid phase in the weld is easily solidified to form a large amount of nickel silicide and M 23 Low melting point eutectic structures such as B6 and M5B3 type borides and welding defects such as holes and cracks. These low melting point structures and welding defects will become weak links affecting the reliability of joints under increasingly high joint use temperatures and performance requirements, especially when brazing heterogeneous alloy base materials with different thermal expansion coefficients.

[0015] In view of the above problems, the present invention adopts nickel as the matrix and adds a variety of alloy elements to regulate the organization. During the brazing cooling process, high melting point elements such as W, Mo, etc. and Cr elements derived from the brazing filler metal itself and the diffusion from the base metal are first precipitated, and after combining with the B element, a stable M3B2 type high melting point boride is formed, and it continues to grow. The reaction process is 2B+W+Mo+Cr→(Cr, W, Mo)3B2. This process is also a process of rapid consumption of the melting element B and improvement of the overall temperature bearing capacity of the weld. The present invention regulates the organization formation at this stage by combining elements with processes: with the help of high melting point elements such as W and Mo added to the brazing filler metal itself and a higher brazing temperature, the diffusion of refractory elements in the base metal to the brazing filler metal and the diffusion of B elements in the brazing filler metal to the base metal are accelerated, so that the liquid brazing filler metal obtains a higher concentration of refractory elements, thereby consuming a large amount of B elements at this stage by diffusion and reaction to increase the melting point of the weld and inhibit the formation of low melting point eutectic organization in the next stage. As solidification continues, the composition of the remaining liquid solder changes significantly, and refractory elements are consumed in large quantities. The residual liquid phase with a lower melting point will gradually form low-melting-point eutectic structures such as borides and silicides in the subsequent solidification process. In order to avoid the formation of these low-melting-point eutectic structures that are not conducive to the high-temperature performance of the joint, the Si content in the solder of the present invention is moderate, and Si can still be dissolved in the weld matrix without forming silicides in the later stage of cooling. However, since the solubility of the B element in the matrix Ni is very low, if there are still more B elements and boride-forming elements in the liquid phase in the later stage of cooling, it is difficult to avoid the appearance of a large number of low-melting-point borides even if the cooling rate is increased. Moreover, a faster cooling rate is more likely to cause joint cracking, especially when connecting heterogeneous materials. During brazing, the solder of the present invention has basically eliminated the B element in the growth stage of the M3B2 phase, avoiding the appearance of low-melting-point eutectic structures from the source, and the Cr element is also consumed in large quantities in the early stage of solidification. The remaining Cr element and elements such as Co, Mo, Al, and Nb continue to form the weld matrix with the Ni element. The concentration of elements such as Cr and Co in the final weld matrix is ​​close to that of the parent material, which together play the role of solid solution strengthening the weld and coordinating the weld metal and the parent material. Elements such as Al and Nb in the weld improve the high temperature performance of the joint through precipitation strengthening. When brazing materials with large differences in thermal properties, the plasticity, composition and organizational coordination of the weld are also particularly important. The brazing material of the present invention adds Co elements with a content similar to that of the parent material matrix, and does not add Ti elements that are prone to stress concentration. While improving strength and wear resistance, it reduces the risk of weld cracking.

[0016] In summary, in response to the increasingly higher operating temperature and performance requirements of high-temperature alloy joints and wear-resistant alloy joints, the present invention adjusts the alloy element ratio, relies on the element interaction between the liquid brazing material and the base alloy during the brazing solidification process, regulates the weld structure, eliminates the low-melting point eutectic, and thus greatly improves the temperature-bearing capacity of the joint.

[0017] The beneficial effects of the present invention are:

[0018] By using the brazing material and brazing process of the present invention, the matrix of the obtained brazed joint is nickel-based austenite, a large amount of alloy elements are solid-dissolved in the matrix, and some alloy elements are precipitated in the matrix in the form of high-melting-point borides with stable properties, and the joint is mainly strengthened by solid solution strengthening and precipitation strengthening. The fluidity of the brazing material is good, the melting corrosion of the substrate is small, the high-temperature mechanical properties of the brazed joint are significantly higher than those of the traditional brazed joint, and compared with the traditional brazing material, the brazing material of the present invention is suitable for the brazing of the same high-temperature alloy material, and is also suitable for the brazing of high-temperature alloy and wear-resistant alloy material, and has a wider range of applications. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] Figure 1 This is the appearance of nickel-based alloy powder brazing material.

[0020] Figure 2 This is the DTA curve of the solder powder in Example 1.

[0021] Figure 3 The microstructure of the joint of DD419 alloy brazed with nickel-based powder brazing filler metal in Example 1.

[0022] Figure 4 The tensile strength of the joint brazed with DD419 alloy using nickel-based powder brazing filler metal in Example 1.

[0023] Figure 5 The microstructure of the joint of DD419 alloy brazed with nickel-based powder brazing filler metal in Example 2.

[0024] Figure 6 The tensile strength of the joint brazed with DD419 alloy using nickel-based powder brazing filler metal in Example 2.

[0025] Figure 7 The microstructure of the joint between DD426 and Co-Nb-Cr alloy brazed with nickel-based powder brazing filler metal in Example 3.

[0026] Figure 8 The tensile strength of the joint between DD426 and Co-Nb-Cr alloy brazed using nickel-based powder brazing filler metal in Example 3.

[0027] Fig. 9 The microstructure of the joint of DD419 alloy brazed with nickel-based powder brazing filler metal in Comparative Example 1.

[0028] Fig.10 The tensile strength of the joint brazed with DD419 alloy using nickel-based powder brazing filler metal in Comparative Example 1.

[0029] Fig.11 This is the microstructure of the joint of DD5 and MX25B alloy brazed with nickel-based powder brazing filler metal in comparative example 2.

[0030] Fig.12 The tensile strength of the joint between DD5 and MX25B alloy brazed using nickel-based powder brazing filler metal in comparative example 2. DETAILED DESCRIPTION

[0031] The present invention is described in detail below with reference to the accompanying drawings and embodiments.

[0032] In the following examples, master alloy ingots were prepared into alloy powders by gas atomization, and the process parameters of the gas atomization method were: powder spraying temperature of 1480° C., mass flow rate of 3.5 kg / min, powder spraying gas of argon, and powder spraying pressure of 5.5 MPa.

[0033] Example 1

[0034] The base material to be welded in this embodiment is a nickel-based high-temperature alloy DD419, and the chemical composition of the alloy is (wt.%):

[0035] Co 9.5%, Cr 6.3%, W 6.5%, Ta 6.6%, Al 5.5%, Re 3.1%, Ti 0.9%, Mo0.5%, balance Ni.

[0036] The chemical composition of solder is (wt.%):

[0037] Co 9%, Cr 12.4%, W 4.5%, Mo 3.4%, Al 6%, Si 0.2%, B 0.8%, C 0.04%, Ni balance.

[0038] Preparation method of solder: Raw materials with a purity greater than 99.99% are mixed in proportion and placed in a vacuum arc melting furnace to be melted into alloy ingots. The melting process is: 1550℃ insulation for 3min→1480℃ pouring; then the melted alloy ingot is prepared into alloy powder by gas atomization, that is, the mother alloy ingot is remelted to form a liquid flow, and argon gas is used to impact it to atomize it into fine droplets, and then it is quickly cooled to form alloy powder, and the powder with a size of no more than 100 mesh is sieved out. The morphology of the prepared nickel-based powder solder is as follows: Figure 1 As shown in FIG. 1 , it is spherical or nearly spherical. The DTA curve of the powder solder in this embodiment is as follows: Figure 2 .

[0039] Before welding, the solid solution nickel-based high temperature alloy DD419 is processed into For the samples, the surface to be welded was polished with No. 800 sandpaper, and the surface oil of the samples to be welded was removed by ultrasonic cleaning in acetone for 15 minutes. The solder powder was mixed into a paste with nicrobraz's'binder and applied to the part to be welded of the samples. Nicorobraz White Stop Off Type II solder resist was applied to the area near the paste solder to prevent the loss of solder during brazing. The samples were placed in a vacuum brazing furnace for brazing at a temperature of 1290°C and a brazing time of 90 minutes. The samples were taken out of the furnace after cooling to below 80°C and subjected to aging treatment.

[0040] Figure 3 This is the microstructure of the sample brazed joint. It can be seen that the weld structure is dense, white borides are distributed in the matrix, and no defects and low-melting-point eutectic structure are found. Figure 4 The results of the 980℃ tensile properties test of the brazed joint of the connected samples.

[0041] Example 2

[0042] The base material to be welded in this embodiment is a nickel-based high-temperature alloy DD419, and the chemical composition of the alloy is (wt.%):

[0043] Co 9.5%, Cr 6.3%, W 6.5%, Ta 6.6%, Al 5.5%, Re 3.1%, Ti 0.9%, Mo0.5%, balance Ni.

[0044] The chemical composition of solder is (wt.%):

[0045] Co 9%, Cr 9%, W 4%, Mo 3.2%, Al 4.2%, Si 3.3%, B 1.2%, Nb 1.5%, C 0.15%, Ni balance.

[0046] Preparation method of solder: raw materials with a purity greater than 99.99% are mixed in proportion and placed in a vacuum arc melting furnace to be melted into alloy ingots. The melting process is: 1540℃ insulation for 3min→1470℃ pouring; then the melted alloy ingot is prepared into alloy powder by gas atomization, that is, the mother alloy ingot is remelted to form a liquid flow, and argon gas is used to impact it to atomize it into fine droplets, and then it is quickly cooled to form alloy powder, and the powder not larger than 100 mesh is sieved out.

[0047] Before welding, the solid solution cobalt-based high-temperature alloy DD419 is processed into For the sample, use No. 800 sandpaper to grind the surface to be welded, and ultrasonically clean it in acetone for 15 minutes to remove the oil on the surface of the sample to be welded. Use nicrobraz's'binder to mix the solder powder into a paste and apply it to the part to be welded of the sample. Apply Nicrobraz White Stop Off Type II solder resist to the area near the paste solder to prevent the loss of solder during brazing. Put the sample into a vacuum brazing furnace for brazing at a brazing temperature of 1240℃ and a brazing time of 25 minutes. After cooling to below 80℃, take it out of the furnace and perform aging treatment.

[0048] Figure 5 This is the microstructure of the sample brazed joint. It can be seen that the weld structure is dense, white borides are distributed in the matrix, and no defects and low-melting-point eutectic structure are found. Figure 6 The results of the 980℃ tensile properties test of the brazed joint of the connected samples.

[0049] Example 3

[0050] In this embodiment, the base materials to be welded are nickel-based high-temperature alloy DD426 and a Co-Nb-Cr wear-resistant alloy.

[0051] The chemical composition of DD426 alloy is (wt.%):

[0052] Co 9%, Cr 5%, W 12%, Al 6%, Ti 1.1%, Mo 1.1%, Nb 1.4%, C 0.15%, Ni balance.

[0053] The chemical composition of Co-Nb-Cr wear-resistant alloy is (wt.%):

[0054] Nb 26%, Cr 19%, Co balance.

[0055] The chemical composition of solder is (wt.%):

[0056] Co 9%, Cr 8.5%, W 4%, Mo 1.7%, Al 4.5%, B 1%, Nb 3.7%, C 0.16%, Ni balance.

[0057] Preparation method of solder: raw materials with a purity greater than 99.99% are mixed in proportion and placed in a vacuum arc melting furnace to be melted into alloy ingots. The melting process is: 1540℃ insulation for 3min→1470℃ pouring; then the melted alloy ingot is prepared into alloy powder by gas atomization, that is, the mother alloy ingot is remelted to form a liquid flow, and argon gas is used to impact it to atomize it into fine droplets, and then it is quickly cooled to form alloy powder, and the powder not larger than 100 mesh is sieved out.

[0058] Before welding, the solid solution DD426 and Co-Nb-Cr wear-resistant alloy were processed into For the sample, use No. 800 sandpaper to grind the surface to be welded, and ultrasonically clean it in acetone for 15 minutes to remove the oil on the surface of the sample to be welded. Use nicrobraz's'binder to mix the solder powder into a paste and apply it to the part to be welded of the sample. Apply Nicrobraz White Stop Off Type II solder resist to the area near the paste solder to prevent the loss of solder during brazing. Put the sample into a vacuum brazing furnace for brazing at a brazing temperature of 1220℃ and a brazing time of 12 minutes. After cooling to below 80℃, take it out of the furnace and perform aging treatment.

[0059] Figure 7 This is the microstructure of the sample brazed joint. The left side of the weld is Co-Nb-Cr wear-resistant alloy, and the right side of the weld is DD426 alloy. It can be seen that the weld structure is dense, white borides are distributed in the matrix, and no defects and low-melting-point eutectic structure are found. Figure 8 The results of the 980℃ tensile properties test of the brazed joint of the connected samples.

[0060] Comparative Example 1

[0061] The base material to be welded in this comparative example is nickel-based high-temperature alloy DD419, and the chemical composition of the alloy is (wt.%):

[0062] Co 9.5%, Cr 6.3%, W 6.5%, Ta 6.6%, Al 5.5%, Re 3.1%, Ti 0.9%, Mo0.5%, balance Ni.

[0063] The chemical composition of solder is (wt.%):

[0064] Co 8%, Cr 11%, W 7%, Mo 3%, Al 5%, Si 0.2%, B 0.4%, Nb 0.2%, C 0.1%, Ni balance.

[0065] Preparation method of solder: raw materials with a purity greater than 99.99% are mixed in proportion and placed in a vacuum arc melting furnace to be melted into alloy ingots. The melting process is: 1550℃ insulation for 3min→1480℃ pouring; the melted alloy ingot is then prepared into alloy powder by gas atomization, that is, the mother alloy ingot is remelted to form a liquid flow, and argon gas is used to impact it to atomize it into fine droplets, and alloy powder is formed after rapid cooling, and powder not larger than 100 mesh is sieved out.

[0066] Before welding, the solid solution nickel-based high temperature alloy DD419 is processed into For the samples, the surface to be welded was polished with No. 800 sandpaper, and the surface oil of the samples to be welded was removed by ultrasonic cleaning in acetone for 15 minutes. The solder powder was mixed into a paste with nicrobraz's'binder and then applied to the part to be welded of the samples. Nicorobraz White Stop Off Type II solder resist was applied to the area near the paste solder to prevent the loss of solder during brazing. The samples were placed in a vacuum brazing furnace for brazing at a temperature of 1290°C and a brazing time of 60 minutes. The samples were taken out of the furnace after cooling to below 80°C and subjected to aging treatment.

[0067] Fig. 9 This is the microstructure of the sample brazed joint. It can be seen that there are multiple hole defects in the weld. Fig.10 The results of the 980℃ tensile properties test of the brazed joint of the connected samples.

[0068] Comparative Example 2

[0069] The base materials to be welded in this comparative example are nickel-based high-temperature alloy DD405 and wear-resistant alloy MX25B.

[0070] The chemical composition of DD405 alloy is (wt.%):

[0071] Cr 7%, Co 8%, W 5%, Al 6%, Ta 6.3%, Mo 1.7%, Re 3%, Hf 0.1%, Ni balance.

[0072] The chemical composition of MX25B alloy is (wt.%):

[0073] Cr 5%, Al 10%, Ti 2%, W 3%, balance Ni.

[0074] The chemical composition of solder is (wt.%):

[0075] Co 11%, Cr 12%, W 3.5%, Mo 0.3%, Al 2%, Si 5%, B 1.3%, Nb1%, C 0.2%, Ni balance.

[0076] Preparation method of solder: raw materials with a purity greater than 99.99% are mixed in proportion and placed in a vacuum arc melting furnace to be melted into alloy ingots. The melting process is: 1530℃ insulation for 3min→1450℃ pouring; the melted alloy ingot is then prepared into alloy powder by gas atomization, that is, the mother alloy ingot is remelted to form a liquid flow, and argon gas is used to impact it to atomize it into fine droplets, and alloy powder is formed after rapid cooling, and powder not larger than 100 mesh is sieved out.

[0077] Before welding, the solid solution nickel-based high temperature alloy DD405 and MX25B wear-resistant alloy are processed into For the samples, the surface to be welded was polished with No. 800 sandpaper, and the surface oil of the samples to be welded was removed by ultrasonic cleaning in acetone for 15 minutes. The solder powder was mixed into a paste with nicrobraz's'binder and applied to the part to be welded of the samples. Nicorobraz White Stop Off Type II solder resist was applied to the area near the paste solder to prevent the loss of solder during brazing. The samples were placed in a vacuum brazing furnace for brazing at a temperature of 1180°C and a brazing time of 30 minutes. The samples were taken out of the furnace after cooling to below 80°C and subjected to aging treatment.

[0078] Fig.11 This is the microstructure of the sample brazed joint. It can be seen that there are multiple hole defects and a large amount of low-melting-point eutectic structures in the weld. Fig.12 The results of the 980℃ tensile properties test of the brazed joint of the connected samples.

[0079] It can be seen from the microstructure diagram of the sample brazed joints in the above examples 1-3 that the weld matrix is ​​uniform and dense, no obvious welding defects and low melting point eutectic structures are observed, and some refractory elements are precipitated in the weld matrix in the form of borides under supersaturated conditions. It can be seen from the 980°C tensile performance test results of the samples after brazing connection in the above examples 1-3 that the high temperature strength of the joint after brazing connection is relatively high, the tensile strength of the high temperature alloy brazed joint under the 980°C test condition is not less than 600MPa, and the tensile strength of the high temperature alloy and wear-resistant alloy brazed joint under the 980°C test condition is not less than 200MPa, which shows that compared with traditional brazing filler metals, the brazing filler metal of the present invention is more suitable for high performance connection of parts under high temperature service environment.

[0080] It can be seen from the microstructure diagram of the brazed joints of the samples in the above-mentioned comparative examples 1-2 that, compared with examples 1-3, there are more welding defects in the brazed joints, among which the brazed joint of comparative example 2 also has a large amount of low melting point eutectic structure, which will lead to reduced high temperature performance of the joint. It can be seen from the tensile performance test results of the connected samples in comparative examples 1-2 that the tensile strength of the high temperature alloy brazed joint under the test condition of 980°C is less than 600MPa, and the tensile strength of the high temperature alloy and wear-resistant alloy brazed joint under the test condition of 980°C is less than 200MPa, which indicates that the brazing material composition exceeds the limit range of the brazing material composition or the brazing temperature exceeds the brazing temperature range specified by the brazing material, and the tensile strength requirements of the joint cannot be met.

Claims

1. A nickel-based powder brazing material, characterized in that: The solder is a nickel-based alloy powder; the chemical composition of the solder is as follows by weight percentage: Co 8.0~12.0%, Cr 8.0~12.5%, W 2.0~6.0%, Mo 1.3~3.5%, Al 1.5~6.5%, Si 0~4.0%, B0.5~1.8%, Nb 0~5.0%, C 0.04~0.3%, Ni is the balance; The preparation method of nickel-based powder brazing material comprises the following steps: (1) Preparing the solder according to the composition of the solder and melting a master alloy ingot of the solder in a vacuum induction furnace; (2) preparing alloy powder from the master alloy ingot by gas atomization method, wherein the process parameters of the gas atomization method are: powder spraying temperature of 1400-1550° C., mass flow rate of 2-6 kg / min, powder spraying gas of argon, and powder spraying pressure of 3-10 MPa; (3) The prepared alloy powder is sieved to select alloy powder with a size not larger than 100 meshes, thereby obtaining the powder solder.

2. The nickel-based powder brazing material according to claim 1, characterized in that: The powder solder is spherical or nearly spherical, and the particle size is not greater than 100 meshes.

3. The method for preparing the nickel-based powder solder according to claim 1, characterized in that: The method comprises the following steps: (1) Preparing the solder according to the composition of the solder and melting a master alloy ingot of the solder in a vacuum induction furnace; (2) preparing alloy powder from the master alloy ingot by gas atomization method, wherein the process parameters of the gas atomization method are: powder spraying temperature of 1400-1550° C., mass flow rate of 2-6 kg / min, powder spraying gas of argon, and powder spraying pressure of 3-10 MPa; (3) The prepared alloy powder is sieved to obtain alloy powder with a size not larger than 100 meshes, thereby obtaining the powder solder.

4. The preparation method according to claim 3, characterized in that: In step (1), the smelting process is: keeping at 1450-1570°C for 1-5 minutes and pouring at 1390-1490°C.

5. The use of the nickel-based powder brazing material according to claim 1 in connecting homogeneous alloys or heterogeneous alloys, characterized in that: The powder brazing filler metal is used for brazing connection of the same high-temperature alloy material, and the brazing temperature is 1200-1300°C; or, the powder brazing filler metal is used for brazing connection between a high-temperature alloy material and a wear-resistant alloy, and the brazing temperature is 1200-1300°C, and the wear-resistant alloy is a Ni3Al-based wear-resistant alloy or a Co-Cr-Mo, Co-Cr-W, Co-Nb-Cr cobalt-based wear-resistant alloy or a WC wear-resistant alloy.

6. The use of the nickel-based powder brazing material according to claim 5 in connecting homogeneous alloys or heterogeneous alloys, characterized in that: During the brazing connection process, the brazing alloy powder is mixed into a paste using an aqueous or oily binder and then applied to the part of the sample to be welded. The sample is placed in a vacuum brazing furnace for brazing connection, and the brazing insulation time is 10 to 90 minutes.

7. The use of the nickel-based powder brazing material according to claim 6 in connecting homogeneous alloys or heterogeneous alloys, characterized in that: After the brazing connection, the tensile strength of the high-temperature alloy brazing joint at 980°C is not less than 600MPa; the tensile strength of the high-temperature alloy and wear-resistant alloy brazing joint at 980°C is not less than 200MPa.