Composite material pot handle and preparation method thereof

The composite material was solved by using aluminum chloride hexahydrate and 1,2-propylene oxide to prepare an alumina gel in a composite pot handle, and adding graphene and azo compounds to form an aerogel structure on the ceramic surface. The problem of insufficient heat resistance of pot handles is achieved by achieving heat resistance and insulation effects at high temperatures, ensuring safety and stability in use.

CN117820022BActive Publication Date: 2024-10-22JIANGMENG CITY DEYIBAO STAINLESS STEEL PROD CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202311123651.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-09-01
Publication Date
2024-10-22
Estimated Expiration
2043-09-01

AI Technical Summary

Technical Problem

Composite pot handles have poor heat resistance and are not suitable for long-term use in high-temperature environments. The resin will undergo chemical reactions at high temperatures, resulting in material performance degradation or damage, limiting its application in high-temperature cooking or baking and other scenarios.

Method used

Aluminum chloride hexahydrate and 1,2-epoxypropane were used to prepare alumina gel, and graphene with heat and high temperature resistance was added to it. An aerogel structure was formed on the ceramic surface through vacuum freeze-drying, combined with coupling Nitride enhances adhesion, resulting in a composite material with heat-resistant, high-temperature resistance and insulating properties.

Benefits of technology

The heat resistance, high temperature resistance and insulation performance of the composite pot handle have been improved, making it less likely to deform or burn at extremely high temperatures, ensuring safety and stability during use, and effectively preventing burns.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004427435100000011
    Figure BDA0004427435100000011
  • Figure BDA0004427435100000041
    Figure BDA0004427435100000041
  • Figure BDA0004427435100000042
    Figure BDA0004427435100000042
Patent Text Reader

Abstract

The present invention relates to the technical field of pot handle production, specifically, to a composite pot handle and a preparation method thereof. The mass percentages of its constituent components are: aluminum chloride hexahydrate: 20-34%; 1,2-propylene oxide: 4-26%; graphene: 20-28%; ceramic: 20-36%; sodium hydroxide: 4-12%. Aluminum chloride hexahydrate and 1,2-propylene oxide are reacted to generate alumina gel, and then graphene is evenly dispersed in the gel, and then evenly applied to the ceramic surface, and then the water is removed by vacuum freeze drying to obtain a composite material with high temperature resistance and heat insulation. Among them, the hydrolysis of inorganic aluminum salt cannot obtain gel, and it is necessary to rely on 1,2-propylene oxide to promote the hydrolysis and polycondensation of sol particles to obtain alumina gel in sequence.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of pot handle production, in particular to a composite pot handle and a preparation method thereof. Background Art

[0002] In the process of designing and manufacturing composite pot handles, different functions and characteristics can be achieved by adding different fibers and resins with reinforcing capabilities, so that composite pot handles can meet different usage requirements, such as increasing strength and reducing weight. In addition, composite pot handles usually have good aesthetics and can provide a variety of colors and styles to meet the aesthetic needs of consumers. However, composite pot handles also have some disadvantages. Compared with traditional metal pot handles, composite pot handles have poor heat resistance. The resin and fiber in the composite material are easily deformed or damaged at high temperatures, so they are not suitable for long-term use in high temperature environments; secondly, the high temperature resistance of composite pot handles is poor. At high temperatures, the resin in the composite material will undergo chemical reactions, resulting in a decrease in material performance or damage. Therefore, composite pot handles are not suitable for scenes such as high-temperature cooking or baking. In view of this, the present invention provides a composite pot handle and a preparation method. Summary of the invention

[0003] The object of the present invention is to provide a composite material pot handle and a preparation method thereof, so as to solve the problems raised in the above background technology.

[0004] To achieve the above object, the present invention provides the following technical solutions:

[0005] The mass percentages of the components of a composite material pot handle are:

[0006]

[0007] Preferably, the ratio of aluminum chloride hexahydrate to 1,2-propylene oxide is 1:0.2-0.3.

[0008] Preferably, the ratio of aluminum chloride hexahydrate to graphene is 1:0.8-1. When the graphene content is too low or too high, the gel morphology formed is too thin or viscous, and it is not easy to adhere to the ceramic surface, which is not conducive to the subsequent process.

[0009] Preferably, the ratio of aluminum chloride hexahydrate to ceramic is 1:1-1.2.

[0010] Preferably, the particle size of the graphene is 80-100 nm.

[0011] Preferably, the concentration of the sodium hydroxide is 2.5-2.7 mol / L.

[0012] Preferably, the preparation method of the composite material pot handle is as follows:

[0013] S1: dissolving aluminum chloride hexahydrate in deionized water and stirring;

[0014] S2: Add 1,2-propylene oxide to the aluminum chloride hexahydrate solution and stir evenly;

[0015] S3: adding graphene to the solution in S2, stirring evenly, adjusting the pH with sodium hydroxide, and standing for a period of time to obtain an aluminum oxide / graphene gel;

[0016] S4: adding azo compounds to the gel and mixing them evenly, then coating them evenly on the ceramic surface, and then freezing them in a refrigerator;

[0017] S5: placing the frozen material in a vacuum freeze dryer, and obtaining a composite material pot handle after vacuum freeze drying.

[0018] Among them, the inorganic metal salt aluminum source is cheap, easy to use, easy to control the preparation process conditions, and easy to achieve large-scale production. Aluminum chloride hexahydrate is dissolved in deionized water, and the solution is filled with water and Al 3+ and Al(OH)3 colloid particles obtained by hydrolysis. Hydrolysis of inorganic aluminum salts cannot produce gels, and a coagulant is needed to promote the hydrolysis and polycondensation of sol particles. 1,2-Propylene oxide is a good proton scavenger. 3+ In the solution, 1,2-propylene oxide will undergo ring opening to form free radicals C3H7O - The free radical is a highly reactive group that reacts easily with Al 3+ Combination, thereby promoting hydrated Al 3+ The hydrolysis reaction forms the hydroxyl groups required for the polycondensation reaction. After the hydroxyl groups are formed, the polycondensation reaction and the hydrolysis reaction proceed simultaneously to form the required Al(OH)3 gel. The specific reaction equation is shown below:

[0019] Al(C3H7O)3+H2O→Al(C3H7O)2(OH)+C3H7OH;

[0020] Al(C3H7O)2(OH)+Al(C3H7O)2(OH)→(C3H7O)2-Al-O-Al-(C3H7O)2+H2O;

[0021] Al(C3H7O)3+Al(C3H7O)2(OH)→(C3H7O)2-Al-O-Al-(C3H7O)2+H2O.

[0022] Forming aerogel with Al(OH)3 as the skeleton alone will cause deformation and structural collapse during the freeze-drying process. Adding graphene materials with heat and high temperature resistance can avoid this phenomenon, enhance the mechanical properties of aerogel materials and increase heat and high temperature resistance. The Al(OH)3-based gel is evenly coated on the surface of the ceramic material, and a layer of aerogel structure is formed on the ceramic surface after vacuum freeze drying. Aerogel has the characteristics of light weight, low density and heat insulation. The prepared composite material has the characteristics of heat resistance, high temperature resistance, heat insulation and light weight.

[0023] Furthermore, the azo compound contains two nitrogen atoms connected by a double bond, and the groups containing the π electron system produce π-π stacking force, which enhances the interaction between the aerogel structure and the ceramic through the π-π stacking force, thereby enhancing the adhesion ability and preventing it from falling off and deforming at high temperatures.

[0024] Preferably, the stirring time in S1 is 10-20 min; the stirring time in S2 is 30-60 min; the stirring time in S3 is 1-2 h, the pH range is 6-8, and the standing time is 8-12 h.

[0025] Preferably, the coating thickness in S4 is 1-3 mm, and the freezing time in the refrigerator is 20-24 h.

[0026] Preferably, the vacuum freeze-drying time in S5 is 36-48 hours.

[0027] Compared with the prior art, the present invention has the following beneficial effects:

[0028] Aluminum oxide gel is made by using aluminum chloride hexahydrate and 1,2-propylene oxide, and graphene with heat and high temperature resistance is dispersed in the gel and coated on the ceramic material. The composite material formed after freeze-drying has heat resistance, high temperature resistance and heat insulation properties. The pot handle made of this composite material can withstand extremely high temperatures and is not easy to deform, melt or burn, ensuring safety and stability during use. The excellent heat insulation performance can effectively prevent burns during use. DETAILED DESCRIPTION

[0029] The technical solutions in the embodiments of the present invention will be clearly and completely described below in combination with the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments in the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention. In the present invention, unless otherwise specified, all equipment and raw materials can be purchased from the market or are commonly used in the industry. The methods in the following embodiments are conventional methods in the art unless otherwise specified.

[0030] The following embodiments of the present invention are used:

[0031] Aluminum chloride hexahydrate was purchased from Dongtai Yongtai Chemical Co., Ltd.;

[0032] 1,2-Propylene oxide was purchased from Jinan Century Tongda Chemical Co., Ltd., CAS No.: 75-56-9;

[0033] Graphene was purchased from Xianfeng Nanotechnology Co., Ltd.;

[0034] Ceramics were purchased from Guangdong Wumeng Precision Ceramics Co., Ltd.;

[0035] Sodium hydroxide was purchased from Cangzhou Xinjia Chemical Products Co., Ltd., CAS No.: 1310-73-2.

[0036] The azo compound used was 4,4'-dihydroxymethylazobenzene, purchased from Henan Weitixi Chemical Technology Co., Ltd., CAS No.: 37797-30-1.

[0037] Example 1

[0038] In this embodiment, the mass percentages of the components of the composite material pot handle are:

[0039]

[0040] The preparation method of the composite material pot handle is as follows:

[0041] Aluminum chloride hexahydrate was dissolved in deionized water and stirred for 20 minutes; 1,2-propylene oxide was added to the aluminum chloride hexahydrate solution and stirred for 45 minutes; 90 nm graphene was added to the above solution, stirred for 2 hours, and then the pH was adjusted to 7.2 with 2.5 mol / L sodium hydroxide, and allowed to stand for 12 hours to obtain an aluminum oxide / graphene gel; 4,4'-dihydroxymethylazobenzene was added to the gel and mixed evenly, and then evenly coated on the ceramic surface with a thickness of 2 mm, and then placed in a refrigerator for freezing for 24 hours; the frozen material was placed in a vacuum freeze dryer and vacuum freeze-dried for 48 hours to obtain a test sample 1.

[0042] Example 2

[0043] In this embodiment, the mass percentages of the components of the composite material pot handle are:

[0044]

[0045] The preparation method of the composite material pot handle is as follows:

[0046] Aluminum chloride hexahydrate was dissolved in deionized water and stirred for 20 minutes; 1,2-propylene oxide was added to the aluminum chloride hexahydrate solution and stirred for 45 minutes; 90 nm graphene was added to the above solution, stirred for 2 hours, and then the pH was adjusted to 7.2 with 2.5 mol / L sodium hydroxide, and allowed to stand for 12 hours to obtain an aluminum oxide / graphene gel; 4,4'-dihydroxymethylazobenzene was added to the gel and mixed evenly, and then evenly coated on the ceramic surface with a thickness of 2 mm, and then placed in a refrigerator for freezing for 24 hours; the frozen material was placed in a vacuum freeze dryer and vacuum freeze-dried for 48 hours to obtain test sample 2.

[0047] Example 3

[0048] In this embodiment, the mass percentages of the components of the composite material pot handle are:

[0049]

[0050] The preparation method of the composite material pot handle is as follows:

[0051] Aluminum chloride hexahydrate was dissolved in deionized water and stirred for 20 minutes; 1,2-propylene oxide was added to the aluminum chloride hexahydrate solution and stirred for 45 minutes; 90 nm graphene was added to the above solution, stirred for 2 hours, and then the pH was adjusted to 7.2 with 2.5 mol / L sodium hydroxide, and allowed to stand for 12 hours to obtain an aluminum oxide / graphene gel; 4,4'-dihydroxymethylazobenzene was added to the gel and mixed evenly, and then evenly coated on the ceramic surface with a thickness of 2 mm, and then placed in a refrigerator for freezing for 24 hours; the frozen material was placed in a vacuum freeze dryer and vacuum freeze-dried for 48 hours to obtain test sample 3.

[0052] Example 4

[0053] In this embodiment, the mass percentages of the components of the composite material pot handle are:

[0054]

[0055] The preparation method of the composite material pot handle is as follows:

[0056] Aluminum chloride hexahydrate was dissolved in deionized water and stirred for 20 minutes; 1,2-propylene oxide was added to the aluminum chloride hexahydrate solution and stirred for 45 minutes; 90 nm graphene was added to the above solution, stirred for 2 hours, and then the pH was adjusted to 7.2 with 2.5 mol / L sodium hydroxide, and allowed to stand for 12 hours to obtain an aluminum oxide / graphene gel; 4,4'-dihydroxymethylazobenzene was added to the gel and mixed evenly, and then evenly coated on the ceramic surface with a thickness of 2 mm, and then placed in a refrigerator for freezing for 24 hours; the frozen material was placed in a vacuum freeze dryer and vacuum freeze-dried for 48 hours to obtain test sample 4.

[0057] Example 5

[0058] In this embodiment, the mass percentages of the components of the composite material pot handle are:

[0059]

[0060] The preparation method of the composite material pot handle is as follows:

[0061] Aluminum chloride hexahydrate was dissolved in deionized water and stirred for 20 minutes; 1,2-propylene oxide was added to the aluminum chloride hexahydrate solution and stirred for 45 minutes; 90 nm graphene was added to the above solution, stirred for 2 hours, and then the pH was adjusted to 7.2 with 2.5 mol / L sodium hydroxide, and allowed to stand for 12 hours to obtain an aluminum oxide / graphene gel; 4,4'-dihydroxymethylazobenzene was added to the gel and mixed evenly, and then evenly coated on the ceramic surface with a thickness of 2 mm, and then placed in a refrigerator for freezing for 24 hours; the frozen material was placed in a vacuum freeze dryer and vacuum freeze-dried for 48 hours to obtain a test sample 5.

[0062] Comparative Example 1

[0063] The same formula and preparation process as in Example 1 were used, except that no graphene was added, to obtain test sample 6.

[0064] Comparative Example 2

[0065] The same formula and preparation process as in Example 1 were used, except that 1,2-propylene oxide was not added, to obtain Test Sample 7.

[0066] Comparative Example 3

[0067] The same formula and preparation process as in Example 1 were used, except that 4,4'-dihydroxymethylazobenzene was not added, to obtain test sample 8.

[0068] The obtained test samples 1-8 were subjected to high temperature resistance and thermal insulation performance tests, and the test results are shown in the following table:

[0069] Deformation rate after high temperature (%) Heat insulation rate (%) Test sample 1 3.3 97.2 Test sample 2 4.1 95.4 Test sample 3 4.3 94.9 Test sample 4 5.5 89.1 Test sample 5 5.9 87.3 Test sample 6 10.8 77.1 Test sample 7 13.3 69.6 Test sample 8 8.1 85.1

[0070] It can be seen from the data in the above table that the composite material composed of aerogel structure formed on the outside of ceramic can effectively resist high temperature and insulate. By comparing test samples 1-3, it can be found that when the content of alumina gel changes, the high temperature resistance and thermal insulation of the composite pot handle will be affected. With the increase of alumina gel content, the high temperature resistance and thermal insulation performance increase accordingly. After reaching the optimal effect, with the increase of alumina gel content, the high temperature resistance and thermal insulation performance decrease accordingly; By comparing test samples 1, 4, and 5, it can be found that when the alumina gel content or the graphene content exceeds a certain proportion, the high temperature resistance and thermal insulation performance of the composite pot handle will be reduced to a certain extent. This is because the formed aerogel structure affects the high temperature resistance and thermal insulation performance of the composite material; By comparing test samples 1, 6, and 7, it can be found that when alumina gel and graphene do not exist, the high temperature resistance and thermal insulation performance of the composite pot handle are greatly reduced. This is because the aerogel structure formed is incomplete when alumina gel or graphene is missing, which affects the overall structure of the composite pot handle, and then affects the high temperature resistance and thermal insulation performance of the composite pot handle. By comparing test samples 1 and 8, it can be found that when the product lacks azo compounds, although there is no obvious effect on the thermal insulation performance, the deformation rate produced after high temperature will increase significantly due to the weakened adhesion between the aerogel structure and the ceramic.

[0071] The above shows and describes the basic principles, main features and advantages of the present invention. Those skilled in the art should understand that the present invention is not limited by the above embodiments. The above embodiments and descriptions are only preferred examples of the present invention and are not intended to limit the present invention. Without departing from the spirit and scope of the present invention, the present invention may have various changes and improvements, which fall within the scope of the present invention. The scope of protection of the present invention is defined by the attached claims and their equivalents.

Claims

1. A composite material pot handle, characterized in that :The mass percentage of its raw materials is: Aluminum chloride hexahydrate: 20-28%; 1,2-Propylene oxide: 4-15%; Graphene: 20-25%; Ceramics: 20-36%; Sodium hydroxide: 4-12%; 4,4'-dihydroxymethylazobenzene: 4-8%; The preparation method of the composite material pot handle is as follows: S1: dissolving aluminum chloride hexahydrate in deionized water and stirring; S2: Add 1,2-propylene oxide to the aluminum chloride hexahydrate solution and stir evenly; S3: adding graphene to the solution in S2, stirring evenly, adjusting the pH with sodium hydroxide, and standing for a period of time to obtain an aluminum oxide / graphene gel; S4: adding 4,4'-dihydroxymethylazobenzene into the gel and mixing evenly, then coating evenly on the ceramic surface, and then freezing in a refrigerator; S5: placing the frozen material in a vacuum freeze dryer, and obtaining a composite material pot handle after vacuum freeze drying.

2. The composite material pot handle according to claim 1, characterized in that : The ratio of aluminum chloride hexahydrate to 1,2-propylene oxide is 1:0.2-0.

3.

3. The composite material pot handle according to claim 1, characterized in that :The ratio of aluminum chloride hexahydrate to graphene is 1:0.8-1.

4. The composite material pot handle according to claim 1, characterized in that The ratio of aluminum chloride hexahydrate to ceramic is 1:1-1.

2.

5. The composite material pot handle according to claim 1, characterized in that :The particle size of the graphene is 80-100nm.

6. The composite material pot handle according to claim 1, characterized in that :The concentration of described sodium hydroxide is 2.5-2.7mol / L.

7. The composite material pot handle according to claim 1, characterized in that : The stirring time in S1 is 10-20 min; the stirring time in S2 is 30-60 min; the stirring time in S3 is 1-2 h, the pH range is 6-8, and the standing time is 8-12 h.

8. The composite material pot handle according to claim 1, characterized in that : The coating thickness in the S4 is 1-3 mm, and the freezing time in the refrigerator is 20-24 h.

9. The composite material pot handle according to claim 1, characterized in that :The vacuum freeze drying time in the described S5 is 36-48h.