A method for preparing gelatin microcarrier for cell culture

The gelatin microcarrier is prepared through spray freezing and crosslinking technology, which solves the cumbersome operation and high cost problems of gelatin microcarrier preparation in the prior art, and obtains a through-pore structure suitable for cell growth, achieving environmentally friendly and efficient cell culture vectors .

CN117820718BActive Publication Date: 2024-11-05LUOYANG SAIAO BIOENGINEERING TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410012955.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-01-04
Publication Date
2024-11-05
Estimated Expiration
2044-01-04

AI Technical Summary

Technical Problem

The existing gelatin microcarrier preparation methods have cumbersome operations, high costs, adverse environment and emulsifier residues in the emulsification method and spray drying method, and the prepared microsphere structure is not suitable for cell growth.

Method used

The gelatin frozen microspheres were prepared by spray freezing, and a microporous structure was formed by de-icing and dispersing, and a cross-linking agent was added for secondary freezing and cross-linking and curing, and finally a gelatin microcarrier was obtained through the macroporous structure.

Benefits of technology

It realizes the preparation of gelatin microcarrier with simple operation, environmental protection and low cost, has a through-pore structure, is suitable for cell growth, avoids the problem of emulsifier residue and high cost, and improves the performance and process level of the carrier.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117820718B_ABST
    Figure CN117820718B_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of gelatin microcarriers for cell culture, comprising the following steps: S1, preparing a gelatin solution with a mass percentage concentration of 1-30wt%; S2, spraying the gelatin solution, freezing it once, and obtaining gelatin frozen microspheres; S3, adding the gelatin frozen microspheres to cold water for thawing and dispersion, and obtaining microporous gelatin gel microspheres; S4, dispersing the microporous gelatin gel microspheres in pure water, adding a cross-linking agent for secondary freezing and cross-linking solidification; S5, thawing the gelatin frozen solution obtained after secondary freezing and cross-linking solidification, washing, freeze drying, and obtaining gelatin microcarriers. The preparation method of the present invention has the characteristics of simple operation, green environmental protection, and low cost, and the obtained gelatin microcarriers not only have the characteristics of penetrating macroporous structure and uniform pore size distribution, but also have large specific surface area and good biocompatibility, good cell attachment, and can be quickly attached to the carrier surface.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of cell culture, and particularly relates to a method for preparing a gelatin microcarrier for cell culture. Background Art

[0002] Microcarrier culture technology is widely used in the production of vaccines, genetic engineering products, etc. Microcarrier culture is currently recognized as the most promising large-scale animal cell culture technology, which combines the advantages of suspension culture and adherent culture and is easy to scale up. This technology has been widely used to culture various types of cells, such as 293 cells, myoblasts, Vero cells, CHO cells, etc.

[0003] Microcarriers refer to microbeads with a diameter of 60-500μm that are suitable for the growth of adherent cells. There are various microcarrier materials on the market, which can be divided into solid microsphere microcarriers and porous microcarriers according to their structure. Cells adhere and grow on the surface of solid microcarriers, and the growth space is relatively small. In addition, the cells are exposed on the surface of the carrier and are easily affected by external factors such as collisions. Porous microcarriers have a three-dimensional porous structure, and cells can adhere and proliferate inside the carrier. The surface area available for cell growth is larger, and cells can obtain a stable growth environment inside the carrier. Therefore, porous microcarriers have more advantages than solid microcarriers.

[0004] Gelatin is derived from collagen. As a natural biomaterial, it has the advantages of biodegradability, biocompatibility, gelling properties and low cost. It is a traditional biomaterial widely used in the medical field. Due to the presence of a wide range of RGD (arginine-glycine-aspartic acid) recognition sites in the molecular structure of gelatin, cells have a good affinity for gelatin. Even cells that are poorly attached to the surface of other materials can grow well on the surface of gelatin. Therefore, using gelatin as a raw material for cell culture microcarriers has great advantages.

[0005] There are related reports on the use of gelatin for microcarrier culture. For example, Chinese patents CN107073165A and CN114516974A disclose methods for preparing porous gelatin microcarriers, both of which are to emulsify the gelatin aqueous phase into small droplets of suitable size in the oil phase by adding an emulsifier, and prepare porous gelatin microcarriers with the aid of freezing pore-making technology. However, the emulsifier and oil phase solvent are introduced in the above-mentioned emulsification process, the preparation process is cumbersome, and multiple washing steps with organic solvents are required to wash away the emulsifier residues. The large-scale use of organic solvents is costly and not conducive to environmental protection. The residual emulsifier has an adverse effect on the cell adhesion growth, and the overall cost performance is poor. Chinese patent CN112266487A discloses a method for preparing gelatin microspheres, which is spray-freeze-dried by mixing chitosan and gelatin in a certain proportion, washing the dried microspheres with a detergent to obtain solid microspheres, and then freeze-drying them twice to obtain the finished product. The preparation method requires two freeze-drying steps, which has high preparation costs, and a freeze-drying protective agent needs to be added in the second freeze-drying step, which is cumbersome to operate. The prepared microspheres are solid microspheres mixed with chitosan and gelatin, which cannot be quickly and completely degraded under the action of trypsin, and the surface of the freeze-dried microspheres is only an uneven crack structure, which is far from a through porous structure, and is not suitable for use as a cell carrier, and has certain limitations. Summary of the invention

[0006] In view of the technical problems existing in the prior art, the purpose of the present invention is to provide a method for preparing gelatin microcarriers for cell culture which is simple to operate, green and environmentally friendly, and low in cost. The prepared gelatin microcarriers have a through-hole macroporous structure, which solves the technical problems existing in the above-mentioned traditional emulsification method or spray drying method in the process of preparing gelatin microspheres and microcarriers.

[0007] In order to achieve the above object, the present invention adopts the following technical solutions:

[0008] The first aspect of the present invention provides a method for preparing a gelatin microcarrier for cell culture, comprising the following steps:

[0009] S1. Add gelatin particles into water, heat and stir to completely dissolve the gelatin, and prepare a gelatin solution;

[0010] S2, spraying and freezing the prepared gelatin solution once to obtain frozen gelatin microspheres;

[0011] S3, adding the obtained frozen gelatin microspheres into cold water for thawing and dispersion to obtain microporous gelatin gel microspheres;

[0012] S4, dispersing the obtained microporous gelatin gel microspheres into pure water, adding a cross-linking agent for secondary freezing and cross-linking solidification;

[0013] S5. Thawing, washing, and freeze-drying the gelatin frozen solution obtained after secondary freezing and cross-linking solidification to obtain gelatin microcarriers.

[0014] Preferably, the types of gelatin include but are not limited to gelatin from animal sources such as pig skin and fish skin, and gelatin from plant sources or genetically recombinant gelatin is also acceptable.

[0015] Preferably, the gelatin solution may be acidic, alkaline or neutral, more preferably neutral.

[0016] Preferably, in order to make the gelatin solution neutral, a pH adjuster needs to be added, and the pH adjuster includes but is not limited to one or a combination of two or more of sodium carbonate, sodium bicarbonate, sodium hydroxide, hydrochloric acid, sulfuric acid, etc.

[0017] Preferably, in order to control the size of ice crystals formed when the gelatin solution is frozen, a crystal growth controller is also added in the process of preparing the gelatin solution. The crystal growth controller includes but is not limited to one or a combination of two or more of sodium chloride, calcium chloride, potassium chloride, dimethyl sulfoxide, glycerol, etc.

[0018] Preferably, the added amount of the crystal growth controller is 0.1 to 1 wt % of the total mass of the gelatin solution.

[0019] Preferably, the mass percentage concentration of the gelatin solution is 1 to 30 wt %. If the concentration is too high, the viscosity of the gelatin solution is too high, which will lead to the easy formation of filamentous spray during subsequent spraying, which is not conducive to the formation of small droplets with uniform particles; if the concentration is too low, in addition to being uneconomical, it is also not conducive to the formation of stable agglomerates, resulting in insufficient stability of the finally prepared carrier structure.

[0020] Preferably, in step S2, the spray temperature is 30-100°C, the spray mode is pneumatic spray, the spray flow rate is 0.1-5L / min, the pneumatic pressure is 0.1-2.0Mpa, and the pneumatic medium is any one of air, nitrogen, and carbon dioxide; the spray droplet particle size formed by the gelatin microspheres is 100-500μm.

[0021] Preferably, after spraying, there are multiple ways of freezing at one time, and liquid nitrogen or cryogenic cold air can be used as a quick freezing agent, and cryogenic cold air is further preferred as a quick freezing agent. Generally, the small droplets formed by the gelatin spray are mixed with a sufficiently pre-cooled cold air flow to quickly freeze the gelatin droplets. The temperature of the cold air flow will determine the freezing time of the droplets and the size of the ice crystals formed. The high temperature of the cold air flow will cause the droplets to be received by the receiver before they can be completely frozen, which will cause the droplets to agglomerate or the ice crystals to form unevenly, affecting the quality of the carrier. In order to freeze the droplets quickly, the cold air can be pre-cooled to a lower temperature. In order to ensure that large droplets can also be completely frozen, the temperature of the cryogenic cold air is generally required to be below -40°C, preferably -80 to -40°C.

[0022] Preferably, in step S3, the gelatin microspheres obtained after the primary freezing are added to pure water for thawing and dispersion, and the specific steps are: firstly heating the frozen gelatin microspheres to -10 to -15°C, then adding them to pure water at 2 to 15°C, stirring them rapidly to thaw the gelatin microspheres rapidly, and redispersing them in the pure water; wherein the volume ratio of the gelatin frozen microspheres to the pure water is 1:20 to 1. If the temperature of the pure water is too low (lower than 2°C), the gelatin frozen microspheres will melt slowly, or the solution will partially freeze when the gelatin frozen microspheres are added. Under normal circumstances, the gelatin frozen microspheres will thaw rapidly in the aqueous solution, but after thawing, the gelatin gel microspheres will not dissolve because the gelatin has already gelled, so what is formed in the aqueous solution at this time is dispersed gelatin gel microspheres. If the water temperature is too high (higher than 15°C), there is a risk of dissolution of the gelatin frozen microspheres, so the temperature of the pure water should not be too high.

[0023] Preferably, in step S4, the temperature of the pure water is 0-15°C.

[0024] Preferably, the secondary freezing method can be any one of the following four methods: (1) pouring the microsphere solution with the cross-linking agent into a tray and placing it in a low-temperature refrigerator for freezing, wherein the temperature of the low-temperature refrigerator is set below -40°C; (2) blowing cold air below -20°C through a tray containing the gelatin solution through a high-speed fan, and freezing the gelatin microsphere solution by forced convection of low-temperature air; (3) placing the gelatin solution into a cylinder (diameter ≤5 cm) or a flat container (short side ≤4 cm) with good thermal conductivity and immersing the container in a freezing liquid below -10°C to freeze the gelatin microspheres; (4) freezing the gelatin microsphere solution using a liquid nitrogen quick freezer, with a freezing temperature of -20°C to -150°C.

[0025] Preferably, in step S4, the temperature of the cross-linking curing is -40°C to -5°C, and the cross-linking agent is one or a combination of two or more of glutaraldehyde, glyoxal, formaldehyde, 1-ethyl-3[3-dimethylaminopropyl]carbodiimide hydrochloride, N-hydroxysuccinimide, 1,6-hexamethylene diisocyanate, butadiene diepoxide, maleic anhydride, dopamine hydrochloride, and genipin.

[0026] The second aspect of the present invention provides gelatin microcarriers prepared by the above preparation method.

[0027] The third aspect of the present invention provides the use of the above-mentioned gelatin microcarrier in cell culture.

[0028] The present invention has the following beneficial effects:

[0029] The gelatin microcarrier prepared by the method of the present invention has the characteristics of through-hole macroporous structure and uniform pore size, excellent appearance, large specific surface area, and degradability. Since the preparation method of the present invention does not introduce any emulsifier and organic solvent, there will be no emulsifier residue, and no need to be washed with organic solvents or doped with other polymer materials, so the good biocompatibility of gelatin can be fully retained, and cells have good attachment, so that various adherent cells can quickly attach to the carrier surface. In addition, the preparation method of the present invention has the characteristics of short process flow, environmental protection, and low cost, which greatly improves the process and performance level of existing gelatin microcarriers and solves the technical problems existing in the traditional emulsification method or spray drying method in the process of preparing gelatin microspheres and microcarriers. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] In order to more clearly illustrate the technical solutions in the embodiments of the present invention, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0031] Figure 1 This is a microscope photo of the gelatin microcarrier prepared in Example 1;

[0032] Figure 2 This is a microscope photo of the gelatin microcarrier prepared in Example 2;

[0033] Figure 3 This is a microscope photo of the gelatin microcarrier prepared in Example 3;

[0034] Figure 4 This is a second microscope photo of the gelatin microcarrier prepared in Example 3;

[0035] Figure 5 This is a microscope photograph of the microporous gelatin gel microspheres obtained in Example 1. DETAILED DESCRIPTION

[0036] In the following description, for the purpose of illustration rather than limitation, specific details such as specific system structures and technologies are provided to provide a thorough understanding of the embodiments of the present invention. However, it should be clear to those skilled in the art that the present invention may also be implemented in other embodiments without these specific details.

[0037] The present invention provides a method for preparing a gelatin microcarrier for cell culture, comprising the following steps:

[0038] S1: adding gelatin particles into water, heating to 40-50° C., stirring to completely dissolve the gelatin, and preparing a gelatin solution with a mass percentage concentration of 1-30wt%;

[0039] The types of gelatin include but are not limited to gelatin from animals such as pig skin and fish skin, and may also be gelatin from plants or genetically recombinant gelatin.

[0040] The gelatin solution may be acidic, alkaline or neutral, and more preferably neutral.

[0041] Therefore, the gelatin microcarriers finally prepared from the gelatin solution with neutral pH are also neutral and suitable for cell adhesion growth without subsequent neutralization.

[0042] In order to make the gelatin solution neutral, a pH adjuster needs to be added during the preparation of the gelatin solution. The pH adjuster includes but is not limited to one or a combination of two or more of sodium carbonate, sodium bicarbonate, sodium hydroxide, hydrochloric acid, sulfuric acid, etc.

[0043] In addition, in order to control the size of ice crystals formed when the gelatin solution is subsequently frozen, a crystal growth controller is added during the preparation of the gelatin solution. The crystal growth controller includes, but is not limited to, one or a combination of two or more of sodium chloride, calcium chloride, potassium chloride, dimethyl sulfoxide, glycerol, etc. The amount of the crystal growth controller added does not exceed 1% of the total mass of the gelatin solution.

[0044] In step S1, the mass percentage concentration of the prepared gelatin solution is 1 to 30 wt %. If the mass percentage concentration of the gelatin solution is too high, the viscosity will be too high, and it is easy to form a filamentous spray during spraying, which is not conducive to forming small droplets with uniform particles; if the mass percentage concentration of the gelatin is too low, in addition to being uneconomical, it is also not conducive to forming a stable agglomerate, resulting in insufficient stability of the final prepared gelatin microcarrier structure.

[0045] S2, spraying and freezing once: spraying and freezing the prepared gelatin solution once to obtain frozen gelatin microspheres;

[0046] Among them, the spraying temperature is not limited, and high temperature, room temperature or low temperature spraying can be performed. Since the viscosity of the gelatin solution decreases as the temperature increases, it is beneficial to the formation of droplets. Therefore, the present invention preferably adopts high temperature spraying. The spraying temperature is preferably 30-100°C. Too high temperature (over 100°C) will have an adverse effect on the stability of the gelatin structure.

[0047] The spraying method is not limited, and pneumatic spraying is preferably used. The pneumatic medium can be one of air, nitrogen, and carbon dioxide, or a combination of two or more. It is necessary to ensure that the pneumatic medium and the gelatin solution do not chemically react. The parameter setting of the spraying condition is: spray flow rate 0.1-5L / min, pneumatic pressure 0.1-2.0Mpa. The ideal droplet size is obtained by adjusting the spraying conditions. As a carrier for cell culture, the spray droplet size is generally controlled to be 100-500μm.

[0048] After spraying, there are many ways to implement one-time freezing. Generally, the small droplets formed by gelatin spray are mixed with a fully pre-cooled cold air flow to quickly freeze the gelatin droplets. The temperature of the cold air flow will determine the freezing time of the droplets and the size of the ice crystals formed. The high temperature of the cold air flow will cause the droplets to be received by the receiver before they can be completely frozen, which will cause the droplets to agglomerate or ice crystals to form unevenly, affecting the quality of the carrier. In order to freeze the droplets quickly, the cold air can be pre-cooled to a lower temperature. In order to ensure that large droplets can also be completely frozen, it is generally necessary to pre-cool the cold air to below -40°C, preferably -80 to -40°C. Liquid nitrogen can be used in special cases. One is to directly fuse the gelatin droplets with liquid nitrogen spray, and the other is to spray the gelatin droplets directly into a liquid nitrogen pool. Spraying into the liquid nitrogen pool requires auxiliary mechanical stirring to ensure that the droplets are fully dispersed after freezing. Studies have found that the higher the mass percentage concentration of the gelatin solution, the longer the freezing time required. Liquid nitrogen quick freezing will be considered when the cold air cannot ensure complete freezing. Because the temperature of liquid nitrogen is low (-196℃), gelatin solution will freeze very quickly in liquid nitrogen to form very fine ice crystals, while cold air freezes relatively slowly, but the ice crystals formed are relatively large. Microspheres frozen by low-temperature air can be directly collected in the collector, and microspheres sprayed into the liquid nitrogen pool need to be separated from the liquid nitrogen by a sieve before being collected for use.

[0049] S3, adding the obtained gelatin microspheres into pure water for thawing and dispersion to obtain microporous gelatin gel microspheres;

[0050] The temperature of the pure water is 2 to 15°C. If the temperature of the pure water is too low, the gelatin microspheres will melt slowly, or the solution will partially freeze when the low-temperature gelatin microspheres are added; if the water temperature is too high, the microspheres are at risk of dissolving, so the water temperature should not be too high. Under normal circumstances, frozen gelatin microspheres will melt quickly in aqueous solution, but after melting, since the gelation of gelatin has already occurred and the microspheres will not dissolve, what is formed in the aqueous solution at this time are dispersed gelatin gel microspheres.

[0051] S3', washing and / or neutralizing the gelatin microspheres with purified water;

[0052] Since a crystal form control agent needs to be added under certain conditions in step S1, the gelatin gel microspheres need to be washed with pure water to remove the above agent. Since the gelatin microspheres have not been fixed by the crosslinking agent at this time, the gelatin microspheres are only maintained by the intermolecular force of gelatin, so the washing process must be very gentle, otherwise the microspheres will be deformed or agglomerated. There are many forms of washing methods, such as precipitation method. Since the specific gravity of gelatin microspheres is greater than that of water, the gelatin microspheres will slowly settle to the bottom of the container under the action of gravity after stopping stirring. At this time, carefully remove the supernatant on the top of the container, and then re-add distilled water and repeat the above operation several times; centrifugation method can also be used to accelerate the precipitation of microspheres, but the centrifugal force cannot be too large, otherwise it will cause the microspheres to agglomerate. After centrifugation, the supernatant is also removed and re-add distilled water and repeat the above operation several times; in addition, filtration method can also be used for washing. Specifically, a filter with a pore size smaller than that of the microspheres is used, and the microsphere solution is poured into a container with a filter at the bottom. The water slowly flows out through the gap between the filter and the microspheres are retained on the filter. Add distilled water and repeat several times. This process must also be carried out very gently, otherwise it will also cause the microspheres to agglomerate.

[0053] If the gelatin solution is not neutralized in step S1, pH neutralization can be performed in this step. The neutralization method can be performed by adding a pH regulator or by adding a neutral buffer solution during the washing process. Washing can be continued after neutralization.

[0054] The gelatin microspheres do not need to be washed or neutralized, that is, step S3' is not required, but it is necessary to ensure that the obtained gelatin microspheres will not affect the cross-linking reaction after subsequent operations and that no impurities such as crystal modifiers that affect cell adhesion growth remain in the cross-linked gelatin microspheres.

[0055] S4, dispersing the gelatin microspheres into pure water at 0-15°C, adding a cross-linking agent, performing secondary freezing and cross-linking solidification;

[0056] In order to ensure rapid freezing of droplets during spray freezing in step S2, very low temperature air or liquid nitrogen is often required to fully contact the gelatin microspheres. The ice crystals formed at this time are relatively small. Since the micropores (gaps) in the gelatin microspheres prepared in step S2 have a relatively small pore size (<5 μm), they cannot meet the needs of cell culture. These pore structures are cavities left after the ice crystals melt, which cannot meet the needs of cells entering the micropores for growth (generally, the pore size of the carrier is required to be 5 to 50 μm when used as a porous cell carrier). Therefore, it is necessary to obtain porous gelatin microspheres with larger pores through further reaction, and it is necessary to add a cross-linking agent to completely fix the structure of the porous microspheres. The present invention has found through research that porous gelatin microspheres with larger pores can be obtained by secondary freezing.

[0057] The secondary freezing method can be any of the following four methods: (1) pouring the microsphere solution with the crosslinking agent into a tray and then placing it in a low-temperature refrigerator for freezing. The temperature of the low-temperature refrigerator needs to be set below -40°C and the thickness of the freezing plate should not be too thick. If it is above -40°C or the freezing thickness is too large, the freezing speed will be too slow, the pore size will be uneven, or the microspheres will be compressed and deformed by large ice crystals, resulting in an irregular three-dimensional structure; (2) blowing cold air below -20°C through a tray containing gelatin solution through a high-speed fan, and freezing the gelatin microsphere solution by forced convection of low-temperature air; (3) placing the gelatin solution into a cylinder (diameter ≤5cm) or a flat container (short side ≤4cm) with good thermal conductivity and immersing the container in a freezing liquid below -10°C to freeze the gelatin microspheres; (4) using a liquid nitrogen quick freezer to freeze the gelatin microsphere solution, the freezing temperature is -20°C to -150°C. Experiments have shown that the above freezing methods are better than traditional -20°C refrigerators in improving the uniformity of microsphere pore size and regularity of three-dimensional structure.

[0058] The cross-linking and curing of gelatin microspheres is carried out at low temperature, specifically in a frozen state. Studies have found that ice crystals are preferentially generated in the water phase during the secondary freezing process. The water phase includes the water phase outside the gelatin gel and the water phase in the pores inside the gelatin. Since many pores are generated inside the gelatin after the first quick freezing, the ice crystals inside the gelatin are preferentially generated in these pores during the secondary freezing process. The ice crystals generated in the pores continue to grow and compress the gelatin gel phase to concentrate. When the gel phase is concentrated to a certain extent, the growth of ice crystals stops due to the increase in the intermolecular force of the gel phase. At this time, large ice crystals and concentrated gelatin gel networks are formed inside the gelatin microspheres. At this time, the cross-linking agent added before freezing will exist inside the gelatin gel phase, and cross-linking reactions still occur inside and on the surface of the gel phase. Temperature and cross-linking reaction are positively correlated. Preferably, the temperature of the cross-linking reaction is -40°C to -5°C, and the selection of the cross-linking temperature is related to the type and concentration of the cross-linking agent.

[0059] S5, thawing, washing, and freeze-drying the gelatin frozen solution obtained after secondary freezing and cross-linking solidification to obtain gelatin microcarriers;

[0060] Specifically, the gelatin frozen solution obtained after secondary freezing and cross-linking solidification is thawed. After thawing, the carrier needs to be washed with pure water to wash away the incompletely reacted cross-linking agent. The washing method can be a membrane filtration method or a centrifugal method. The specific operation is similar to the aforementioned washing method. The difference is that at this time, the carrier has been solidified and negative pressure or centrifugal force can be applied accordingly to increase the washing efficiency. The carrier can also be treated with high temperature before washing. High temperature can make the residual cross-linking agent react completely or more easily migrate from the inside of the carrier to the washing solution. The temperature range of high temperature treatment is 50°C to 130°C. The washed gelatin carrier is then dispersed in distilled water and freeze-dried to finally obtain gelatin microcarriers.

[0061] Among them, thawing in this step refers to the process of heating the frozen gelatin solution after freezing and cross-linking to re-solution. The thawing process is very important because there may still be residual cross-linking agents in the ice cubes at this time. Too long thawing time or too high thawing temperature may cause excessive cross-linking of the microcarriers. The biggest risk of excessive cross-linking is that the carrier will become undegradable. In addition to the large specific surface area, the gelatin microcarrier prepared by the present invention has another biggest advantage that it can be rapidly degraded and release attached cells under the action of proteases, so the thawing process needs to be controlled to prevent excessive cross-linking.

[0062] In order to prevent excessive cross-linking, the ice cubes need to be thawed as quickly as possible at low temperatures. Specifically, the following two thawing methods can be used: (1) slightly heating the surface of the tray or the surface of the freezing mold to separate the ice cubes from the mold, placing the ice cubes separated from the mold in an ice crusher to crush the ice cubes into smaller pieces, and then mixing the crushed ice with 2-20°C pure water in a certain proportion and applying stirring and heating to quickly thaw the ice; (2) immersing a flat or cylindrical mold with good heat conductivity into a solution of 0-40°C, and using the external solution to heat the mold to quickly thaw the ice cubes in the solution. The thawing time is 2-10 minutes.

[0063] The present invention has found that after gelatin microspheres are redispersed in cold water at 0 to 15°C and melted, the microspheres can be well dispersed in an aqueous solution and smaller micropores or crack structures (<5 μm) are retained. Although these smaller micropores cannot accommodate cells to enter, after quick freezing again (secondary freezing), these micropores can preferentially form ice crystal nuclei inside the gelatin microspheres. These preferentially formed nuclei can further grow to form ice crystals of 5 to 50 μm inside the gelatin microspheres. After being fixed at low temperature with a cross-linking agent, a porous gelatin microcarrier with a network-like through-hole structure is formed. The size of the through-holes of the carrier can be controlled by the temperature and time of the secondary quick freezing. At this time, the pore size of the gelatin carrier is very suitable for the adhesion and proliferation of various adherent cells. The cells can be amplified at a high density inside the carrier, which is very suitable for large-scale suspension culture of cells.

[0064] Example 1

[0065] The gelatin microcarriers were prepared using type A gelatin as raw material and liquid nitrogen as a quick freezing agent. The specific steps are as follows:

[0066] Weigh 10 g of gelatin particles and add them to 100 g of distilled water, then heat to 50°C and stir to completely dissolve the gelatin particles. Then add sodium bicarbonate powder to the dissolved gelatin solution to make the final pH value of the solution reach 7.0-7.2.

[0067] The prepared gelatin solution is added to a pneumatic spray device, wherein the pneumatic medium is nitrogen, the nozzle is a fan-shaped nozzle, the spray flow rate is set to 0.3L / min, the nitrogen pressure is 0.3Mpa, and a liquid nitrogen receiving pool is provided 50cm below the nozzle, and high-speed stirring is applied in the receiving pool. The gelatin solution is sprayed into droplets with an average particle size of 150μm, and quickly frozen into solid ice balls in the liquid nitrogen receiving pool. After the spraying is completed, the liquid nitrogen in the liquid nitrogen receiving pool is filtered through a stainless steel filter membrane and harvested to obtain gelatin frozen microspheres.

[0068] The frozen gelatin microspheres were heated to about -10°C, and then added to 10°C pure water, wherein the ratio of microspheres to water was 1:5. The microspheres were added while being stirred rapidly to allow the gelatin microspheres to thaw quickly and be redispersed. After the microspheres were completely thawed and dispersed, 0.1% glutaraldehyde was added to the dispersion, stirring was stopped, and the microporous gelatin gel microsphere solution containing glutaraldehyde was poured into a stainless steel tray, ensuring that the liquid thickness in the tray was less than 10 mm.

[0069] Place the stainless steel tray containing microporous gelatin gel microspheres and glutaraldehyde crosslinker on the shelf of a -50℃ air-cooled quick freezer, close the quick freezer cabinet door and start secondary freezing for 2 hours. After freezing, place the stainless steel tray in a -20℃ freezer for 48 hours. After 48 hours, take the tray out of the freezer, slightly heat the bottom of the tray, and pour the ice cubes in the tray into an ice crusher for crushing.

[0070] Mix the crushed ice with 15℃ pure water in a ratio of 1:3, and stir quickly to melt the ice. After melting, quickly pour the solution into a suction filter with a 500-mesh stainless steel filter at the bottom, and apply a negative pressure of 0.2Mpa to filter quickly. After filtering, close the valve at the bottom of the suction filter, add pure water from the top to clean the microspheres, open the valve and filter again after completion, and repeat the above operation 2-3 times to complete the cleaning.

[0071] The washed microspheres were mixed with pure water at a mass ratio of 1:5, and then poured into a stainless steel tray, ensuring that the liquid height in the tray did not exceed 1 cm, and then placed in a freeze dryer for freeze drying to obtain porous gelatin microcarriers. Figure 1 .

[0072] Example 2

[0073] Gelatin microcarriers were prepared using type A gelatin as raw material and low temperature cold air as quick freezing agent.

[0074] Specific steps: First, weigh 10g of gelatin particles and add them to 100g of distilled water, then heat to 50°C and stir to completely dissolve the gelatin particles. Then add sodium bicarbonate powder to the dissolved gelatin solution to make the final pH value of the solution reach 7.0-7.2;

[0075] The prepared gelatin solution is added to a pneumatic spray device, wherein the pneumatic medium is nitrogen, the nozzle is a fan-shaped nozzle, the spray flow rate is set to 0.3L / min, the nitrogen pressure is 0.3Mpa, the nozzle is sprayed into a freezing chamber and mixed with a reverse cold air flow at -80°C to freeze the gelatin droplets quickly, and the gelatin frozen microspheres are collected by a collector;

[0076] Warm the frozen gelatin microspheres to about -10°C, then add them to 10°C pure water, where the ratio of microspheres to water is 1:4. Stir quickly while adding the microspheres to quickly thaw and redisperse the gelatin microspheres. After the microspheres are completely thawed and dispersed, add 0.1% glutaraldehyde to the dispersion, stop stirring, and pour the microporous gelatin gel microsphere solution containing glutaraldehyde into a stainless steel tray, ensuring that the liquid thickness in the tray is less than 10mm;

[0077] Place the stainless steel tray containing microporous gelatin gel microspheres and glutaraldehyde crosslinker on the shelf of a -100℃ refrigerator, close the refrigerator door and start secondary freezing for 12 hours. After freezing, place the stainless steel tray in a -20℃ freezer for 48 hours. After 48 hours, take the tray out of the freezer, slightly heat the bottom of the tray, and pour the ice in the tray into an ice crusher to break it;

[0078] Mix the crushed ice with 15℃ pure water in a ratio of 1:3, and stir quickly to melt the ice. After melting, quickly pour the solution into a filtration device with a 500-mesh stainless steel filter at the bottom, apply a negative pressure of 0.2Mpa to filter quickly, close the valve at the bottom of the filter after filtration, add pure water from the top to clean the microspheres, open the valve and filter again after completion, and repeat the above operation 2-3 times to complete the cleaning;

[0079] The washed microspheres were mixed with pure water at a mass ratio of 1:5, and then poured into a stainless steel tray, ensuring that the liquid height in the tray did not exceed 1 cm, and then placed in a freeze dryer for freeze drying to obtain porous gelatin microcarriers. Figure 2 .

[0080] Example 3

[0081] The porous gelatin microcarriers were prepared using type A gelatin as raw material and dimethyl sulfoxide as a crystal form control agent. The specific steps were as follows: first, 5 g of gelatin particles were weighed and added to 100 g of distilled water, then the temperature was raised to 50°C and stirred to completely dissolve the gelatin particles, then sodium bicarbonate powder was added to the dissolved gelatin solution to adjust the final pH value of the solution to 7.0-7.2; finally, 0.5 wt% of dimethyl sulfoxide was added to the neutralized gelatin solution as a crystal form control agent during freezing;

[0082] The prepared gelatin solution is added to a pneumatic spray device, wherein the pneumatic medium is nitrogen, the nozzle is a fan-shaped nozzle, the spray flow rate is set to 0.3L / min, the nitrogen pressure is 0.3Mpa, and a liquid nitrogen receiving pool is provided 50cm below the nozzle, and high-speed stirring is applied in the receiving pool. The gelatin solution is sprayed into droplets with an average particle size of 150μm, and quickly frozen into solid ice balls in the liquid nitrogen receiving pool. After the spraying is completed, the liquid nitrogen in the liquid nitrogen receiving pool is filtered through a stainless steel filter membrane and then harvested to obtain gelatin frozen microspheres;

[0083] The frozen gelatin microspheres are heated to about -10°C, and then added to 10°C pure water, where the ratio of microspheres to water is 1:5. Stir quickly while adding the microspheres to make the gelatin microspheres thaw quickly and redisperse. After the microspheres are completely thawed and dispersed, the microsphere solution is poured into a 300-mesh stainless steel filter cartridge and slowly filtered by gravity at 15°C. After filtering once, add 15°C pure water again to wash and filter again, and repeat the above operation 2-3 times. After completion, the microporous gelatin gel microspheres obtained on the filter screen are redispersed in 15°C pure water and 0.1% glutaraldehyde is added to the dispersion. The gelatin solution containing glutaraldehyde is poured into a stainless steel tray to ensure that the liquid thickness in the tray is less than 10mm.

[0084] Place the stainless steel tray containing microporous gelatin gel microspheres and glutaraldehyde crosslinking agent on the shelf of a liquid nitrogen quick freezer set at a temperature of -50°C, close the quick freezer door and start secondary freezing for 1 hour. After freezing, place the stainless steel tray in a -20°C freezer for 48 hours. After 48 hours, take the tray out of the freezer, slightly heat the bottom of the tray, and pour the ice cubes in the tray into an ice crusher for crushing;

[0085] Mix the crushed ice with 15℃ pure water in a ratio of 1:3, and stir quickly to melt the ice. After melting, quickly pour the solution into a filtration device with a 500-mesh stainless steel filter at the bottom, apply a negative pressure of 0.2Mpa to filter quickly, close the valve at the bottom of the filter after filtration, add pure water from the top to clean the microspheres, open the valve and filter again after completion, and repeat the above operation 2-3 times to complete the cleaning;

[0086] The washed microspheres were mixed with pure water at a mass ratio of 1:5, and then poured into a stainless steel tray, ensuring that the liquid height in the tray did not exceed 1 cm, and then placed in a freeze dryer for freeze drying to obtain porous gelatin microcarriers. Figure 3 and 4 .

[0087] Morphological characterization

[0088] Microscopic pictures of the gelatin microcarriers prepared in Examples 1-3 are shown in Figure 1-4 ,Depend on Figure 1-4 The results show that the gelatin microcarriers prepared in the present invention all have a porous structure with through macropores and uniform pore size distribution.

[0089] Microscopic photographs of the microporous gelatin microspheres obtained in Example 1 are shown in Figure 5 ,Depend on Figure 5 The results show that the gelatin gel microspheres dispersed in aqueous solution have pore structures less than 5μm under a microscope. These pore structures are cavities left after the ice crystals melt. After the gelatin frozen microspheres are thawed, these cavities are retained to a certain extent because the gelatin remains gelled.

[0090] The (porous) gelatin microcarrier with through macropores prepared in Example 1 of the present invention was inoculated with Vero cells at a density of 3 g / L and continuously cultured in serum-free medium for 168 h. The cell proliferation multiple exceeded 20 times, which was 2 to 3 times that of traditional spherical microcarriers. The relevant comparative experimental data are shown in Table 1 below.

[0091] Table 1

[0092]

[0093] The present invention is not limited to the above-mentioned specific implementation modes. Various changes made by ordinary technicians in this field based on the above-mentioned concepts without creative work are all within the protection scope of the present invention.

Claims

1. A method for preparing a gelatin microcarrier for cell culture, characterized in that: Prepared by the following steps: S1. Add gelatin particles into water, heat and stir to completely dissolve the gelatin, and prepare a gelatin solution; S2, spraying and freezing the prepared gelatin solution once to obtain frozen gelatin microspheres; S3, adding the obtained frozen gelatin microspheres into purified water for thawing and dispersion to obtain microporous gelatin gel microspheres; In step S3, the obtained frozen gelatin microspheres are added to pure water for thawing and dispersion, and the specific steps are: firstly heating the frozen gelatin microspheres to -10~-15°C, then adding them to pure water at 2~15°C, stirring rapidly to thaw the gelatin microspheres quickly, and redispersing them in the pure water; wherein the volume ratio of the frozen gelatin microspheres to the pure water is 1:20~1; S4, dispersing the obtained microporous gelatin gel microspheres into pure water, adding a cross-linking agent for secondary freezing and cross-linking solidification; S5. Thawing, washing, and freeze-drying the gelatin frozen solution obtained after secondary freezing and cross-linking solidification to obtain gelatin microcarriers.

2. The method for preparing gelatin microcarriers for cell culture according to claim 1, characterized in that: In step S1, a pH adjuster is added during the preparation of the gelatin solution to adjust the gelatin solution to be neutral. The pH adjuster is one of sodium carbonate, sodium bicarbonate, sodium hydroxide, hydrochloric acid, and sulfuric acid, or a combination of two or more thereof.

3. The method for preparing gelatin microcarriers for cell culture according to claim 1, characterized in that: In step S1, a crystal growth controller is also added during the preparation of the gelatin solution, and the amount of the crystal growth controller added is 0-1wt% of the total mass of the gelatin solution; the crystal growth controller is one or a combination of two or more of sodium chloride, calcium chloride, potassium chloride, dimethyl sulfoxide, and glycerol.

4. The method for preparing gelatin microcarriers for cell culture according to claim 1, characterized in that: The mass percentage concentration of the gelatin solution is 1-30wt%.

5. The method for preparing gelatin microcarriers for cell culture according to claim 1, characterized in that: In step S2, the spray temperature is 30~100℃, the spray mode is pneumatic spray, the spray flow rate is 0.1~5L / min, the pneumatic pressure is 0.1~2.0Mpa, and the pneumatic medium is any one of air, nitrogen, and carbon dioxide; the spray droplet particle size formed by the gelatin microspheres is 100~500μm; the one-time freezing method uses liquid nitrogen or low-temperature cold air as a quick freezing agent, and the temperature of the low-temperature cold air is -80~-40℃.

6. The method for preparing gelatin microcarriers for cell culture according to claim 1, characterized in that: In step S4, the temperature of the pure water is 0-15°C.

7. The method for preparing gelatin microcarriers for cell culture according to claim 1, characterized in that: The secondary freezing method is any one of the following four methods: (1) pouring the microsphere solution with the cross-linking agent into a tray and placing it in a low-temperature refrigerator for freezing, wherein the temperature of the low-temperature refrigerator is set below -40°C; (2) blowing cold air below -20°C through a tray containing the gelatin solution through a high-speed fan, and freezing the gelatin microsphere solution by forced convection of the low-temperature air; (3) placing the gelatin solution into a cylinder with a diameter of ≤5 cm or a flat container with a short side of ≤4 cm and immersing the container in a freezing liquid below -10°C to freeze the gelatin microspheres; (4) freezing the gelatin microsphere solution using a liquid nitrogen quick freezer, with the freezing temperature ranging from -20°C to -150°C.

8. The method for preparing gelatin microcarriers for cell culture according to claim 1, characterized in that: In step S4, the temperature of the cross-linking curing is -40°C to -5°C, and the cross-linking agent is one or a combination of two or more of glutaraldehyde, glyoxal, formaldehyde, 1-ethyl-3[3-dimethylaminopropyl]carbodiimide hydrochloride, N-hydroxysuccinimide, 1,6-hexamethylene diisocyanate, butadiene diepoxide, maleic anhydride, dopamine hydrochloride, and genipin.