Preparation method and application of an amine-functionalized adsorption material with highly dispersed active sites

By creating point defects on amine-functionalized adsorbent materials and introducing additional proton acceptors, combining thermal reduction and plasma treatment, the problem of organic amine agglomeration in amine-functionalized adsorbent materials is solved, and the adsorption capacity and adsorption of carbon dioxide are improved. performance, achieving more efficient carbon dioxide capture.

CN117839657BActive Publication Date: 2024-11-12ZHEJIANG UNIV OF TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410163155.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-02-05
Publication Date
2024-11-12
Estimated Expiration
2044-02-05

AI Technical Summary

Technical Problem

The existing amine-based functionalized adsorbent materials have problems with organic amine agglomeration during carbon dioxide adsorption, resulting in limited adsorption performance and high regeneration energy consumption.

Method used

By creating a large number of point defects on amine-functional adsorbent materials, combining organic amines, introducing additional proton acceptors, and using thermal reduction and plasma treatment methods, the high dispersion and proton transfer of amine-based molecules are achieved, and the amine-based loading is regulated. Improve adsorption performance.

Benefits of technology

It effectively avoids organic amine agglomeration, improves the adsorption capacity and adsorption performance of carbon dioxide, simplifies the adsorption and deprotonation process, and improves the utilization efficiency of amine groups.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117839657B_ABST
    Figure CN117839657B_ABST
Patent Text Reader

Abstract

The present invention discloses a preparation method and application of an amine-functionalized adsorbent material with highly dispersed active sites, comprising: loading a graphene aerogel into a tubular furnace and performing a thermal reduction treatment; loading a thermally reduced sample into a plasma vapor deposition tube, performing a plasma treatment of the sample in different atmospheres under vacuum conditions to obtain a carrier; drying the carrier overnight, taking a polyamino organic amine and the carrier into a reactor, placing them in a blast oven for heating, then taking out the reactants to remove the organic amine attached to the surface, and then soaking them in ethanol, and drying them in a blast oven overnight to obtain the material. The amine-functionalized adsorbent material of the present invention is a material that creates a large number of point defects on a carbon material through thermal reduction and plasma treatment, introduces additional proton receptors, and grafts different organic amines. The preparation method provided by the present invention can prepare an amine-functionalized adsorbent material that can flexibly control the amine loading amount to achieve high dispersion of amine molecules, and strengthen proton transfer to improve adsorption performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of functional material preparation, and specifically relates to a preparation method and application of an amine-functionalized adsorption material with highly dispersed active sites. Background Art

[0002] In recent years, the dual carbon goals have attracted widespread attention from all over the world. The reason for this phenomenon is that people have emitted large amounts of carbon dioxide, causing global warming, resulting in a series of disasters such as rising sea levels, ozone layer depletion, ocean acidification, and unpredictable weather conditions, which have endangered people's lives. Therefore, controlling carbon dioxide emissions and capturing carbon dioxide has become an urgent matter.

[0003] Post-combustion carbon dioxide capture technology is easier to implement in practical applications, and adsorption is the post-combustion carbon dioxide treatment technology that currently receives the most attention. According to the strength of the adsorption effect, the adsorption method can be summarized as physical adsorption and chemical adsorption. The adsorption effect of physical adsorption is relatively weak, so its regeneration energy consumption is low and its selectivity is poor. The adsorption effect of chemical adsorption is strong and has specific selection. It can adsorb a certain substance with high selectivity, but its regeneration energy consumption is relatively high. Amine-functionalized adsorbent materials are a type of adsorbent that is currently used more frequently due to their high carbon dioxide adsorption capacity. The adsorption of CO2 mainly conforms to the zwitterion theory, but there are still some specific factors that affect the adsorption mechanism. For example, when there are no additional proton acceptors, the protons of the zwitterions can only be transferred to the adjacent amine functional groups, causing them to lose the ability to adsorb CO2 molecules, which means that two adsorption sites can capture one CO2 molecule; when there are additional proton acceptors (especially when the proton acceptance capacity is greater than that of the amine functional groups), the zwitterions will preferentially transfer protons to the proton acceptors, thereby achieving the ideal situation of one adsorption site capturing one CO2 molecule, greatly improving the utilization efficiency of the amine groups. Amine-functionalized adsorbents achieve a higher carbon dioxide adsorption capacity by loading a certain amount of organic amines. However, organic amines are prone to agglomeration, resulting in clogging of the pores of the base material.

[0004] The present invention creates a large number of point defects on the amine-functionalized adsorbent material, combines the organic amine with the defects, can flexibly control the amine loading, and achieve a high degree of dispersion of the amine molecules, which greatly improves the problem of easy agglomeration of the organic amine. At the same time, additional proton receptors are introduced to strengthen proton transfer, thereby improving the adsorption performance of the adsorbent material. Summary of the invention

[0005] In view of the shortcomings of the prior art, the present invention provides a preparation method and application of an amine-functionalized adsorption material with highly dispersed active sites. The amine-functionalized adsorption material with highly dispersed active sites is prepared by the following method:

[0006] (1) 10 to 30 mg of graphene aerogel was placed into a corundum tube of a tubular furnace and subjected to thermal reduction treatment to obtain a thermally reduced sample.

[0007] (2) 10 to 30 mg of the sample obtained in step (1) is placed in a plasma vapor deposition tube, and the sample is subjected to plasma treatment in different atmospheres under a vacuum condition with an absolute pressure of less than 30 kPa to obtain a carrier used subsequently.

[0008] (3) Dry the carrier obtained in step (2) overnight. Take 10-50 mL of pure organic amine and 10-30 mg of the carrier and put them into a reaction kettle, and heat them in a 60-100°C forced air oven for 8-15 hours. Then take out the sample and gently dry the organic amine attached to the surface with a paper towel, soak the sample in 150-200 mL of anhydrous ethanol for 10-40 minutes, and dry it in a 60-100°C forced air oven overnight to obtain an amine-functionalized adsorption material with highly dispersed active sites.

[0009] Furthermore, the thermal reduction treatment method in step (1) is: to remove oxygen in the tube by argon-vacuum cycle operation 2 to 3 times, to increase the temperature to 1200 to 1600° C. at a heating rate of 8 to 12° C. (preferably 10° C.) per minute under 10 to 20 mL / min argon protection, maintain for 2 to 3 hours, and then cool naturally.

[0010] Furthermore, the plasma atmosphere in step (2) is argon, helium, hydrogen, or carbon monoxide.

[0011] Furthermore, the plasma treatment method in step (2) is: to remove oxygen in the tube by vacuum cycle operation 2 to 3 times, to increase the temperature to 600 to 900° C. at a heating rate of 8 to 12° C. (preferably 10° C.) per minute under different atmosphere protection of 10 to 20 mL / min, the plasma power is set to 200 W, and the treatment time is 1 to 180 min.

[0012] Furthermore, the polyamino organic amine in step (3) is TETA (triethylenetetramine), TEPA (tetraethylenepentamine) and MMEN (N,N'-dimethylethylenediamine).

[0013] Furthermore, the oven temperature in step (3) is 60-90°C.

[0014] Furthermore, the anhydrous ethanol soaking temperature in step (3) is 30-50°C.

[0015] The present invention also provides an exploration of the amine loading capacity of an amine-functionalized adsorption material with highly dispersed active sites.

[0016] Compared with the prior art, the beneficial effects of the present invention are as follows: the amine-functionalized adsorbent material with highly dispersed active sites prepared by the present invention is a material that produces a large number of point defects on a carbon material through thermal reduction and plasma treatment, and grafts different organic amines. The key point is that enough point defects are produced through plasma treatment to evenly disperse the amine molecules, avoid agglomeration of the organic amines, flexibly control the amine loading, and achieve high dispersion of the amine molecules. At the same time, additional proton receptors are introduced to strengthen proton transfer, thereby improving the adsorption performance of the adsorbent material. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] Figure 1 The spherical aberration corrected electron microscope image of the GA of the present invention before and after plasma treatment;

[0018] Figure 2 This is the XPS full spectrum analysis of dGA and TEPA-dGA of the present invention;

[0019] Figure 3 Raman mapping of rGA, dGA and TEPA-dGA of the present invention (I D / I G );

[0020] Figure 4 High-resolution N1s spectroscopic analysis of dGA and TEPA-dGA of the present invention; DETAILED DESCRIPTION

[0021] The technical solution of the present invention is further described below in conjunction with the accompanying drawings and embodiments.

[0022] The graphene aerogel used in this embodiment is prepared by the following method:

[0023] (1) A graphene oxide aqueous dispersion (12.55 mg / g) and ultrapure water were mixed at a volume ratio of 1:1 and stirred for 10 minutes to prepare a uniform dilution of 6.275 mg / g.

[0024] (2) 16 g of the diluted solution was spread evenly on a plastic petri dish with a diameter of 60 mm, and placed in an oven at 60° C. to dry for 6 hours to obtain graphene oxide flakes.

[0025] (3) Immerse the graphene oxide flakes in a 30 vol% hydrazine hydrate solution at room temperature and allow to foam for 3 hours, until the flakes gradually become fluffy and foamy.

[0026] (4) The foamed sample was completely immersed in 20 mL of anhydrous ethanol for 3 hours. After each time, new anhydrous ethanol was replaced. This step was repeated three times. The above steps were repeated using n-hexane instead of anhydrous ethanol. The sample was placed in a 60°C oven and dried overnight to obtain graphene aerogel.

[0027] Example 1

[0028] The present invention provides a method for preparing a TEPA-modified graphene aerogel, and the specific steps are as follows:

[0029] (1) 20 mg of graphene aerogel was loaded into a corundum tube of a tubular furnace and subjected to thermal reduction treatment (the oxygen in the tube was removed by argon-vacuum cycle operation 3 times, and the temperature was raised to 1400°C at a rate of 10°C per minute under 15 mL / min argon protection, maintained for 2.5 hours, and then naturally cooled to ambient temperature) to obtain rGA.

[0030] (2) 20 mg of the sample obtained in step (1) was taken and placed in a plasma vapor deposition tube, and the sample was treated with argon plasma under vacuum conditions with an absolute pressure of less than 30 kPa (the oxygen in the tube was removed by vacuum cycle operation twice, and the temperature was increased to 750° C. at a rate of 10° C. per minute under the protection of 15 mL / min argon atmosphere, the plasma power was set to 200 W, and the treatment time was 90 min) to obtain dGA.

[0031] (3) Dry the carrier obtained in step (2) overnight for 12 hours. Take 25 mL of pure TEPA and 20 mg of the carrier and put them into a reaction kettle, and heat them in a 90°C forced air oven for 10 hours. Then take out the sample and gently absorb the organic amine attached to the surface with a paper towel, soak the sample in 170 mL of 40°C anhydrous ethanol for 20 minutes, and dry it at 80°C overnight for 12 hours to obtain the adsorption material TEPA-dGA.

[0032] The spherical aberration corrected electron microscope image and XPS spectrum of the graphene aerogel prepared in this example are as follows: Figure 1 , 2 As shown in the figure, after argon plasma treatment, the regular diffraction pattern of rGA is destroyed, and dGA has successfully introduced a large number of point defects. Before TEPA modification, there is almost no nitrogen on the surface of dGA, while the nitrogen content on the surface of TEPA-modified graphene aerogel is 20%. Figure 3 The Raman mapping images of the thermally reduced sample rGA, the carrier dGA after plasma treatment, and TEPA-dGA show that the overall I D / I G The value of dGA is between 0.4 and 0.5. After argon plasma bombardment, dGA significantly increases to 0.6, indicating that a large number of point defects are introduced and evenly distributed on the dGA surface. After TEPA modification, the overall I D / I G The value is reduced to 0.55, indicating that TEPA can accurately and evenly combine with the dispersed sites of point defects.

[0033] Figure 4This is a high-resolution N1s spectrum before and after TEPA modification. The nitrogen element on the surface of TEPA-dGA mainly exists in three forms: pyridinic nitrogen, pyrrolic nitrogen and graphitic nitrogen. The TEPA molecule itself will show the characteristics of pyridinic nitrogen and pyrrolic nitrogen in XPS analysis, and does not contain graphitic nitrogen. Graphitic nitrogen is a form in which one nitrogen atom is bonded to three carbon atoms. Only when the amino functional group of the TEPA molecule is covalently bonded to the point defects on the surface of dGA can this special nitrogen element form be formed. Therefore, TEPA-dGA is determined to be an amine-functionalized adsorption material that meets the requirements of highly dispersed active sites.

[0034] The amino loading of TEPA-dGA prepared in this example was investigated. The TGA curve after TEPA modification had only one weight loss peak, indicating that the loaded amines were all grafted onto the material, and there was no physically adsorbed organic amine. When the argon plasma treatment time was 1, 5, 15, 30, 60, and 180 min, the TEPA loading on TEPA-dGA was 16wt%, 36wt%, 44wt%, 66wt%, 74wt%, and 87wt%, respectively.

[0035] Through DFT calculation, it was found that the TEPA-dGA prepared in this embodiment can complete the CO2 chemical adsorption and deprotonation process simultaneously in just one step, which simplifies the reaction process and makes it easier to help the zwitterions formed after the amino group adsorbs CO2 to complete the deprotonation process, thereby achieving the purpose of improving the CO2 adsorption performance.

[0036] Furthermore, the prepared material can be used for amino group regulation. By changing the duration of argon plasma treatment, the required TEPA loading can be achieved. When used for CO2 adsorption, since TEPA is highly dispersedly bound to the surface of graphene aerogel material, the problem of TEPA easy agglomeration is avoided, and the adsorption performance can be improved. Under 100% CO2 conditions, static adsorption for 30 minutes, the CO2 adsorption capacity is 12mmol / g, and the amine utilization rate can reach 90%.

[0037] Example 2

[0038] The present invention provides a method for preparing TETA-modified graphene aerogel, and the specific steps are as follows:

[0039] (1) 30 mg of graphene aerogel was loaded into a corundum tube of a tubular furnace and subjected to thermal reduction treatment (the oxygen in the tube was removed by argon-vacuum cycle operation twice, and the temperature was raised to 1500°C at a rate of 12°C per minute under 18 mL / min argon protection, maintained for 2 hours, and then naturally cooled to ambient temperature) to obtain rGA.

[0040] (2) 25 mg of the sample obtained in step (1) was taken and placed in a plasma vapor deposition tube, and the sample was treated with argon plasma under vacuum conditions with an absolute pressure of less than 30 kPa (the oxygen in the tube was removed by vacuum cycle operation 3 times, and the temperature was raised to 650° C. at a rate of 8° C. per minute under the protection of 10 mL / min argon atmosphere, the plasma power was set to 200 W, and the treatment time was 150 min) to obtain dGA.

[0041] The carrier obtained in step (2) was dried overnight for 11 hours. 25 mL of pure TETA and 20 mg of the carrier were placed in a reaction kettle and heated in a 90°C forced air oven for 10 hours. The sample was then taken out and the organic amine attached to the surface was gently blotted with a paper towel. The sample was immersed in 170 mL of 35°C anhydrous ethanol for 20 minutes and dried at 80°C overnight for 13 hours to obtain the adsorption material TETA-dGA.

[0042] The TETA loading on the TETA-dGA prepared in this example under different argon treatment times was investigated, with the highest being 54.0 wt %. TETA-dGA was applied to CO2 adsorption, and the CO2 adsorption capacity was 6 mmol / g under 100% CO2 conditions for static adsorption for 30 min.

[0043] Example 3

[0044] The present invention provides a method for preparing MMEN-modified graphene aerogel, and the specific steps are as follows:

[0045] (1) 30 mg of graphene aerogel was loaded into a corundum tube of a tubular furnace and subjected to thermal reduction treatment (the oxygen in the tube was removed by argon-vacuum cycle operation 3 times, and the temperature was raised to 1300°C at a rate of 8°C per minute under 12 mL / min argon protection, maintained for 2 hours, and then naturally cooled to ambient temperature) to obtain rGA.

[0046] (2) 25 mg of the sample obtained in step (1) was taken and placed in a plasma vapor deposition tube, and the sample was treated with hydrogen plasma under vacuum conditions with an absolute pressure of less than 30 kPa (the oxygen in the tube was removed by vacuum cycle operation twice, and the temperature was increased to 850° C. at a rate of 12° C. per minute under the protection of 20 mL / min argon atmosphere, the plasma power was set to 200 W, and the treatment time was 60 min) to obtain dGA.

[0047] (3) The carrier obtained in step (2) was dried overnight for 13 hours. 25 mL of pure MMEN and 20 mg of the carrier were placed in a reaction kettle and heated in a 90°C forced air oven for 10 hours. The sample was then taken out and the organic amine attached to the surface was gently blotted with a paper towel. The sample was immersed in 170 mL of 45°C anhydrous ethanol for 20 minutes and dried at 80°C overnight for 11 hours to obtain the adsorption material MMEN-dGA.

[0048] The MMEN loading on the MMEN-dGA prepared in this example under different hydrogen treatment times was investigated, and the highest was 45.0wt%. The MMEN-dGA was applied to CO2 adsorption, and the CO2 adsorption capacity was 5mmol / g under 100% CO2 conditions for static adsorption for 30min.

[0049] The above description is only a preferred embodiment of the present invention, and therefore cannot be used to limit the scope of the present invention. That is, equivalent changes and modifications made according to the patent scope of the present invention and the contents of the specification should still fall within the scope of the present invention.

Claims

1. A method for preparing an amine-functionalized adsorption material with highly dispersed active sites, characterized in that: The following steps are involved: (1) The graphene aerogel is placed in a tubular furnace and subjected to thermal reduction treatment to obtain a thermally reduced sample; (2) placing the thermally reduced sample obtained in step (1) into a plasma vapor deposition tube, and subjecting the sample to plasma treatment in different atmospheres under vacuum conditions, wherein the atmosphere is argon, helium, hydrogen or carbon monoxide, to obtain a carrier; (3) Dry the carrier obtained in step (2) overnight for 8 to 16 hours, take the polyamino organic amine and the carrier into a reaction kettle, the polyamino organic amine is triethylenetetramine, tetraethylenepentamine or N,N'-dimethylethylenediamine, place it in a 60-100°C forced air oven and heat it for 8 to 15 hours, then take out the reactant to remove the organic amine attached to the surface, then soak it in ethanol for 10 to 40 minutes, and dry it in a 60-100°C forced air oven overnight for 8 to 16 hours to obtain an amine-functionalized adsorption material with highly dispersed active sites.

2. The preparation method according to claim 1, characterized in that: In step (1), the thermal reduction treatment specifically includes: removing oxygen in the tube by argon-vacuum cycle operation 2 to 3 times, raising the temperature to 1200 to 1600°C at a heating rate of 8 to 12°C per minute under the protection of 10 to 20 mL / min argon, maintaining for 2 to 3 hours, and then cooling naturally.

3. The preparation method according to claim 1, characterized in that: In step (2), the sample is subjected to plasma treatment in different atmospheres under vacuum conditions with an absolute pressure of less than 30 kPa.

4. The preparation method according to claim 1, characterized in that: In step (2), the plasma treatment specifically includes: removing oxygen in the tube by vacuum cycle operation 2 to 3 times, heating the temperature to 600 to 900° C. at a heating rate of 8 to 12° C. per minute under different atmosphere protection of 10 to 20 mL / min, setting the plasma power to 180 to 220 W, and the treatment time to 1 to 180 min.

5. The preparation method according to claim 1, characterized in that: In step (3), the oven temperature is 60-90°C.

6. The preparation method according to claim 1, characterized in that: In step (3), the ethanol soaking temperature is 30-50°C.