Polyphenylene sulfide resin microparticles and preparation method thereof
Through the method of polymerization and flash evaporation combined with foam flotation, the problem of large particle size and high cost in the preparation of polyphenylene sulfide resin particles has been solved, and efficient and low-cost preparation of small and narrow particle sizes has been achieved, using by-products As a foaming agent, there is no need to add additional high-pollution agents.
Patent Information
- Application Number
- CN202410016459.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-01-04
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2044-01-04
AI Technical Summary
Existing methods for preparing polyphenylene sulfide resin particles have problems such as large particle size, wide particle size distribution, and high cost. It is difficult to prepare particles with small particle size and narrow particle size distribution efficiently and at low cost.
Polyphenylene sulfide resin with small particle size is obtained by mixing the sulfur source, alkali metal hydroxide solution and polar organic solvent for dehydration, polymerization reaction with dihaloaromatic compounds, followed by flash evaporation and foam flotation. Microparticles use the by-products in the reactants as foaming agents to avoid adding additional high-pollution foaming agents.
It achieves the efficient preparation of polyphenylene sulfide resin particles with small particle size and narrow particle size distribution, reduces production costs, and improves the content of particles and flotation efficiency by controlling the viscosity of the reactants and the solvent removal effect.
Smart Images

Figure CN117843997B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of polymer materials, in particular to polyphenylene sulfide resin particles and a preparation method thereof. Background Art
[0002] Polyphenylene sulfide (PPS) is a special engineering plastic with excellent comprehensive performance, which is widely used in various electronic and electrical components, mechanical components and automotive components. Among them, polyphenylene sulfide resin particles with narrow particle size distribution and small particle size are widely used in coatings, adhesives, dispersants in printing inks and 3D printing. However, the polyphenylene sulfide resin particles are still difficult to be prepared by efficient and low-cost methods.
[0003] At present, the conventional preparation methods of polyphenylene sulfide resin powder or granules are mainly divided into the following two types: First, the cooling crystallization process, which refers to the precipitation of the product by slow cooling, and after filtering or screening, it is divided into a filter cake containing by-product salt and a by-product slurry. The product filter cake is further washed and purified to obtain a granular PPS product. The product of this process contains a small amount of PPS particles mainly composed of low molecular weight PPS. The whole product D 50 Generally, it is above 50μm. For example, patent application US20150105524A1 discloses a manufacturing process in which small PPS particles with a diameter less than 2.38mm are screened out using a screener or classifier, and the remaining large PPS particles are re-crushed and screened again. The screened small PPS particles are further purified and finally solid-liquid separated to obtain a small PPS product with a content of less than 10wt% of the component with particles larger than 2.38mm, indicating that the original product contains a large number of large particles.
[0004] Second, the flash evaporation process refers to flash evaporation of the reaction mixture without cooling it down to normal pressure. During the flash evaporation process, the solvent is vaporized and the product is dried to form a crude product. After further washing and purification, a powdered PPS product is obtained. This product contains a certain amount of PPS particles. 50 Generally, it is above 30 μm. For example, patent application CN111533910A discloses an industrial production process of injection-grade polyphenylene sulfide resin, which produces product particles with a particle size of about 0.2-2 mm.
[0005] It can be seen that in the conventional preparation method of PPS polyphenylene sulfide resin, although the particle size of PPS prepared by the flash evaporation process is lower than that of the product prepared by the cooling crystallization process, it is still larger and has a wider particle size distribution.
[0006] Although there are some methods for preparing PPS particles on the market, such as the method for preparing polyphenylene sulfide resin particles disclosed in patent CN101981091A, PPS resin is dissolved in nitrogen methyl pyrrolidone in an autoclave, and then the high-temperature and high-pressure solution is discharged into a receiving tank filled with cold water through a connecting pipe to obtain a suspension containing NMP of PPS resin particles, and after screening out the coarse particles mixed in a small amount, the suspension is centrifuged, and then washed with water and centrifuged several times to obtain PPS resin particles with an average particle size of about 10μm. Also, patent CN110741032A discloses a method for preparing spherical PPS particles, which melt-blends PPS with water-soluble or water-dispersible polyester (PE) to prepare a PE linear or granular blend in which PPS is dispersed, and then the blend is cooled, and the PPS particles are recovered by dissolving the polyester in water heated to a maximum of 95°C. The D 50 The above patents all use PPS resin products obtained by conventional cooling crystallization or flash evaporation process to further process PPS particles, and the entire production process is complicated and costly. Summary of the invention
[0007] Based on this, it is necessary to provide a polyphenylene sulfide resin microparticle and a preparation method thereof to address the above problems. The preparation method can not only efficiently prepare polyphenylene sulfide resin microparticles with small particle size and narrow particle size distribution, but also has low cost.
[0008] A method for preparing polyphenylene sulfide resin particles, the preparation method comprising the following steps:
[0009] A sulfur source, an alkali metal hydroxide solution and a first polar organic solvent are mixed in the presence or absence of an auxiliary agent and dehydrated to obtain a dehydrated liquid, and then the dehydrated liquid is mixed with a dihalogen aromatic compound and a second polar organic solvent for polymerization reaction to obtain a reactant containing polyphenylene sulfide resin, wherein the viscosity of the reactant is 1Pa·s-5Pa·s, and the ratio of the sum of the molar amounts of the first polar organic solvent and the second polar organic solvent to the molar amount of the sulfur source is 2.8:1-3.3:1; the reactant is flash evaporated to obtain a crude product;
[0010] The crude product is mixed with water to form a mixture, and gas is introduced into the mixture for froth flotation, and polyphenylene sulfide resin particles are separated from the froth phase, wherein the polyphenylene sulfide resin particles have a D 50 ≤20μm, D 90 / D 10 ≤8.
[0011] In one embodiment, the weight average molecular weight of the polyphenylene sulfide resin in the reactant is 15000-30000.
[0012] In one embodiment, the molar ratio of the alkali metal hydroxide solution to the sulfur source is 0.97:1-1.01:1;
[0013] and / or, the molar ratio of the auxiliary agent to the sulfur source is less than or equal to 0.1:1;
[0014] And / or, the molar ratio of water to sulfur in the dehydrated liquid is 1.0:1-1.3:1.
[0015] In one embodiment, the molar ratio of the dihalogen aromatic compound to the sulfur source is 1.03:1-1.06:1.
[0016] In one embodiment, the sulfur source is selected from sodium hydrosulfide and / or potassium hydrosulfide;
[0017] And / or, the alkali metal hydroxide solution is selected from sodium hydroxide solution and / or potassium hydroxide solution;
[0018] And / or, the dihalogen aromatic compound is at least one selected from p-dichlorobenzene, dichloronaphthalene, dichlorofluorene, and dichlorocarbazole;
[0019] And / or, the auxiliary agent is selected from at least one of sodium acetate, sodium benzoate, and sodium of C5-C6 fatty acid;
[0020] And / or, the first polar organic solvent and the second polar organic solvent are both selected from organic amide solvents, and the organic amide solvent is selected from at least one of N-methylpyrrolidone, hexamethylphosphotriamine, and N-methyl-ε-caprolactam.
[0021] In one embodiment, in the step of flash evaporating the reactants, steam is introduced into the flash evaporator, the steam temperature is 270°C-310°C, and the temperature of the reactants is 270°C-290°C;
[0022] And / or, in the step of flash evaporating the reactant, the mass of the steam is 0.1kg-0.5kg based on 1kg of the reactant.
[0023] In one embodiment, in the step of flash evaporating the reactant, after the flash evaporation is completed, the flash evaporation product is further dried until the residual amount of the solvent is less than 0.2wt%, to obtain the crude product;
[0024] And / or, in the step of performing froth flotation, the pH value of the mixture is adjusted to 5-7, and in the step of separating polyphenylene sulfide resin microparticles from the froth phase, the froth phase and water are mixed to form a mixed slurry, and the pH value of the mixed slurry is adjusted to 8-10, and then washed with water to obtain polyphenylene sulfide resin microparticles.
[0025] In one embodiment, in the step of mixing the crude product with water to form a mixture, the mass ratio of polyphenylene sulfide to water in the crude product is 1:4-1:20;
[0026] And / or, in the step of mixing the crude product with water to form a mixture, the crude product and water are firstly slurried, separated and then mixed with water again to form the mixture.
[0027] In one embodiment, in the step of obtaining the foam phase, a mother liquor is also obtained, and the mother liquor is recycled to prepare the mixture;
[0028] Alternatively, a conventional polyphenylene sulfide resin powder product is directly separated from the mother liquor.
[0029] A polyphenylene sulfide resin particle prepared by the method for preparing the polyphenylene sulfide resin particle as described above.
[0030] In the preparation method of polyphenylene sulfide resin microparticles of the present invention, by controlling the viscosity of the reactants and the content of the first polar organic solvent and the second polar organic solvent, and flashing the reactants, the removal effect of the solvent in the reactants during flash evaporation can be improved, and a crude polyphenylene sulfide resin product with a small particle size is obtained, and the content of the polyphenylene sulfide resin microparticles is higher. Since the polyphenylene sulfide resin itself has the characteristic of hydrophobicity, and the polyphenylene sulfide resin microparticles with a small particle size can selectively adhere to the bubbles, thus, the present invention directly mixes the crude product with water to form a mixture and performs foam flotation, so that polyphenylene sulfide resin microparticles with a small particle size and a narrow particle size distribution can be screened out. At the same time, since the crude product contains the main by-products generated during the polymerization reaction (such as dimers of nitrogen-containing sodium methyl butyrate end groups and trimers of nitrogen-containing sodium methyl butyrate end groups), the by-products have high surface activity and can be used as foaming agents, so that in the step of foam flotation, there is no need to add additional highly polluting foaming agents.
[0031] Therefore, the method for preparing polyphenylene sulfide resin microparticles of the present invention can not only efficiently prepare polyphenylene sulfide resin microparticles with small particle size and narrow particle size distribution, but also has low cost. BRIEF DESCRIPTION OF THE DRAWINGS
[0032] Figure 1 The schematic diagram is a flow chart of a method for preparing polyphenylene sulfide resin particles according to one embodiment of the present invention. DETAILED DESCRIPTION
[0033] For ease of understanding of the present invention, the present invention will be described in more detail below. However, it should be understood that the present invention can be implemented in many different forms and is not limited to the embodiments or examples described herein. On the contrary, the purpose of providing these embodiments or examples is to make the understanding of the disclosure of the present invention more thorough and comprehensive.
[0034] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art of the present invention. The terms used in the specification of the present invention herein are only for the purpose of describing specific implementation methods or embodiments and are not intended to limit the present invention.
[0035] Combination Figure 1 As shown, the preparation method of polyphenylene sulfide resin microparticles provided by the present invention comprises the following steps: mixing a sulfur source, an alkali metal hydroxide solution and a first polar organic solvent in the presence or absence of an auxiliary agent and dehydrating the mixture to obtain a dehydrated liquid, and then mixing the dehydrated liquid with a dihalogen aromatic compound and a second polar organic solvent for polymerization reaction to obtain a reactant containing polyphenylene sulfide resin, wherein the viscosity of the reactant is 1Pa·s-5Pa·s, and the molar ratio of the sum of the molar amounts of the first polar organic solvent and the second polar organic solvent to the sulfur source is 2.8:1-3.3:1. Such a configuration enables the reactant to have a low viscosity and a low solvent ratio, which is conducive to the sufficient removal of the solvent during subsequent flash evaporation, thereby obtaining a crude polyphenylene sulfide resin with a small particle size, and wherein the content of polyphenylene sulfide resin microparticles is high.
[0036] Optionally, the molar ratio of the alkali metal hydroxide solution to the sulfur source is 0.96: 1-1.03: 1, and more preferably 0.97: 1-1.01: 1. Such a configuration can further effectively avoid the problem of unbalanced raw material ratio due to sulfur loss, that is, further ensure that the raw material ratio is still within a reasonable range after considering the sulfur loss, so that the subsequent polymerization reaction can be better carried out, and at the same time, it is beneficial to better control the hydrophilicity and hydrophobicity of the polyphenylene sulfide resin particles in the subsequent mixture, and better control the content of the main by-products (such as dimers of nitrogen-containing sodium methylbutyrate end groups and trimers of nitrogen-containing sodium methylbutyrate end groups) in the polymerization reaction, that is, the content of the foaming agent, thereby better improving the flotation efficiency of the polyphenylene sulfide resin particles.
[0037] It should be noted that the structural formula of the dimer of the main byproduct of the polymerization reaction in the present invention, which contains the end groups of sodium nitrogen-containing methylbutyrate, can be The trimer containing the end group of sodium methylbutyrate can be
[0038] Optionally, the molar ratio of water to sulfur in the dehydration liquid is 1.0: 1-1.3: 1. Such a configuration is beneficial to the efficiency of the subsequent polymerization reaction and reduces the heat required for volatilization of water during flash evaporation.
[0039] It can be understood that the sulfur in the dehydrated liquid refers to the sulfur remaining in the dehydrated liquid after the dehydration is completed and the sulfur loss is taken into account.
[0040] Optionally, the weight average molecular weight of the polyphenylene sulfide resin in the reactant is 15000-30000. This configuration can further control the viscosity of the reactant to be 1Pa·s-5Pa·s, which is beneficial to further improve the solvent removal effect during flash evaporation, and make the particle size of the polyphenylene sulfide resin after flash evaporation small and the content of polyphenylene sulfide resin particles high.
[0041] Optionally, the molar ratio of the auxiliary agent to the sulfur source is less than or equal to 0.1: 1. This configuration can better control the viscosity of the reactants, which is beneficial to improving the subsequent flash evaporation effect.
[0042] Optionally, the auxiliary agent is selected from at least one of sodium acetate, sodium benzoate, and sodium of C5-C6 fatty acid.
[0043] Considering that the addition of auxiliary agents such as sodium acetate, C5-C6 fatty acid, sodium benzoate, etc. will increase the viscosity of the subsequent reactants, in order to further control the viscosity of the reactants, the present invention preferably does not add auxiliary agents during the dehydration process. Specifically, in the dehydration step, the sulfur source, alkali metal hydroxide solution and the first polar organic solvent are mixed and dehydrated. Such an arrangement can better control the viscosity of the subsequent reactants, improve the removal effect of the solvent during the subsequent flash evaporation, and then reduce the particle size of the polyphenylene sulfide resin particles after flash evaporation, and increase the content of the polyphenylene sulfide resin microparticles.
[0044] Optionally, the molar ratio of the dihalogen aromatic compound to the sulfur source is 1.03: 1-1.06: 1. Such an arrangement can further control and ensure that the weight average molecular weight of the polyphenylene sulfide resin in the reactant is 15000-30000, thereby better controlling the viscosity of the reactant, reducing the particle size of the polyphenylene sulfide resin particles after flash evaporation, and increasing the content of the polyphenylene sulfide resin microparticles.
[0045] Optionally, in the polymerization step, the reaction temperature is 240° C.-265° C., and the reaction time is 0.5 h-5 h. This arrangement enables each component to undergo a better polymerization reaction.
[0046] Optionally, the sulfur source is selected from sodium hydrosulfide and / or potassium hydrosulfide.
[0047] Optionally, the alkali metal hydroxide solution is selected from sodium hydroxide solution and / or potassium hydroxide solution, preferably sodium hydroxide solution.
[0048] Optionally, the dihalogen aromatic compound is selected from at least one of p-dichlorobenzene, dichloronaphthalene, dichlorofluorene, and dichlorocarbazole, preferably p-dichlorobenzene.
[0049] Optionally, the first polar organic solvent and the second polar organic solvent are both selected from organic amide solvents, and the organic amide solvent is selected from at least one of N-methylpyrrolidone, hexamethylphosphotriamine, and N-methyl-ε-caprolactam, preferably N-methylpyrrolidone.
[0050] It should be noted that the specific types of the first polar organic solvent and the second polar organic solvent may be the same or different. In the present invention, it is preferred that the specific types of the first polar organic solvent and the second polar organic solvent are the same.
[0051] In the method for preparing polyphenylene sulfide resin microparticles of the present invention, the reactant obtained above is flash evaporated to remove the solvent in the reactant to obtain a crude product. Specifically, the reactant is heated to 270°C-290°C, preferably 280°C-290°C, and then flash evaporated. Such an arrangement can effectively prevent the reactant from decomposing due to excessive temperature.
[0052] Optionally, in the step of flash evaporating the reactant, steam is introduced into the flash evaporator, and the steam temperature is 270°C-310°C; based on 1kg of the reactant, the mass of the steam is 0.1kg-0.5kg. Such an arrangement can further improve the removal effect of the solvent in the reactant, reduce the particle size of the polyphenylene sulfide resin particles after flash evaporation, and increase the content of the polyphenylene sulfide resin microparticles; at the same time, it avoids the increase in production costs due to excessive steam consumption.
[0053] Optionally, in the step of flash evaporating the reactant, after the flash evaporation is completed, the steam is stopped from being introduced, and the flash evaporation product is further dried until the residual amount of the solvent is less than 0.2 wt %, to obtain the crude product. This arrangement can further reduce the loss of polar organic solvents.
[0054] It should be noted that the solvent in the residual amount of the solvent being less than 0.2 wt % refers to a mixture of the remaining water in the flash product, the first polar solvent and the second polar solvent.
[0055] In the preparation method of polyphenylene sulfide resin microparticles of the present invention, the crude product is mixed with water to form a mixture, gas is introduced into the mixture for froth flotation, and polyphenylene sulfide resin microparticles are separated from the froth phase, wherein the D 50 ≤20μm, D 90 / D 10 ≤8.
[0056] Specifically, in addition to polyphenylene sulfide resin particles and by-product sodium chloride, the crude product also contains major by-products produced during the polymerization reaction, such as dimers of nitrogen-containing sodium methylbutyrate end groups and trimers of nitrogen-containing sodium methylbutyrate end groups. The by-products have high surface activity and can be used as foaming agents. Under the action of gas, a large number of bubbles are generated in the mixture and a foam phase is formed. Since the polyphenylene sulfide resin itself has hydrophobic properties, and small-size polyphenylene sulfide resin microparticles can selectively adhere to the bubbles, the present invention directly performs foam flotation on the crude product to screen out polyphenylene sulfide resin microparticles with small particle size and narrow particle size distribution. The method is simple and efficient.
[0057] At the same time, since the by-products in the crude product can be directly used as a foaming agent, the present invention does not need to add additional highly polluting foaming agents in the froth flotation step, which is economical, environmentally friendly and low in cost.
[0058] In one embodiment, the crude product obtained above is mixed with water to form a mixture, the mixture is placed in a froth flotation machine, and gas is introduced into the mixture for flotation treatment to obtain a foam phase, and then the foam phase is mixed with water to form a mixed slurry, and the polyphenylene sulfide resin particles are obtained by separation after defoaming.
[0059] Optionally, in the step of mixing the crude product with water to form a mixture, the mass ratio of polyphenylene sulfide to water in the crude product is 1:4-1:20. Such an arrangement can facilitate the subsequent formation of a foam phase consisting of gas, liquid and solid phases, thereby facilitating the flotation effect of polyphenylene sulfide resin particles.
[0060] In one embodiment, in the step of mixing the crude product with water to form a mixture, the crude product is first mixed with water for pulping, separated by suction filtration or the like, and then mixed with water to form a mixture. When adding water twice, the mass ratio of polyphenylene sulfide to water in the crude product is independently selected from 1:4-1:20. This arrangement can further remove impurities and improve the subsequent flotation efficiency.
[0061] It should be noted that the pulping treatment can be carried out at normal pressure and room temperature, or at high temperature. The high-temperature pulping treatment is specifically as follows: after mixing the crude product with water, the temperature is raised to between 150°C and 220°C, kept warm for 20min-40min, and then dropped to room temperature.
[0062] Optionally, in the step of froth flotation, the pH value of the mixture is adjusted to 5-7, preferably 5-6.5, and then, in the step of separating the polyphenylene sulfide resin microparticles from the foam phase, the foam phase and water are mixed to form a mixed slurry, and the pH value of the mixed slurry is adjusted to 8-10, preferably 9-10, and then washed with water to obtain polyphenylene sulfide resin microparticles. Such an arrangement can further improve the hydrophobicity and foaming effect of the polyphenylene sulfide resin microparticles, and at the same time, it is beneficial to defoam the foam phase, thereby improving the flotation effect of the polyphenylene sulfide resin microparticles.
[0063] In one embodiment, the step of washing with water can be performed at room temperature or at high temperature. The present invention prefers high temperature washing, which is as follows: the mixed slurry is heated to 150°C-220°C, kept warm for 20min-100min, preferably 30min, and then cooled, filtered, rinsed and dried to obtain polyphenylene sulfide resin microparticles with small particle size and narrow particle size distribution.
[0064] High-temperature water washing device In the present invention, in the step of obtaining the foam phase, a mother liquor is also obtained, and the mother liquor can be treated in the following two ways.
[0065] The first treatment method is to recycle the mother liquor for preparing the mixture. This arrangement can further improve the yield of the polyphenylene sulfide resin particles.
[0066] The second treatment method is to directly separate and obtain a conventional polyphenylene sulfide resin powder product from the mother liquor.
[0067] Optionally, in the step of directly separating a conventional polyphenylene sulfide resin powder product from the mother liquor, the pH value of the mother liquor is adjusted to 8-10, then the temperature is raised to 150°C-220°C and kept for 20min-100min, then the temperature is lowered, filtered and dried to obtain a conventional polyphenylene sulfide resin powder product.
[0068] Therefore, the method for preparing polyphenylene sulfide resin microparticles of the present invention can not only efficiently prepare polyphenylene sulfide resin microparticles with small particle size and narrow particle size distribution, but also has low cost.
[0069] The present invention also provides polyphenylene sulfide resin particles prepared by the method for preparing polyphenylene sulfide resin particles as described above. 50 ≤20μm, D 90 / D 10 ≤8, which enables it to be better used in coatings, adhesives, dispersants and 3D printing fields.
[0070] Hereinafter, the polyphenylene sulfide resin particles and the preparation method thereof will be further described through the following specific examples.
[0071] It should be noted that the raw materials and reagents involved in all the embodiments and comparative examples of the present invention can be purchased from the market. At the same time, the equipment involved in the embodiments of the present invention, including the froth flotation machine, the reactor and the high-temperature water washing device, are all conventional equipment in the prior art.
[0072] In addition, it should be noted that the specific test method for the particle size and particle size distribution range of the polyphenylene sulfide resin microparticles prepared in the embodiments and comparative examples of the present invention is as follows: 0.2 g of the sample is put into 20 mL of water, and after ultrasonic dispersion for 5 minutes, it is added to the sample injection system of the Microtrac S3500 particle size measuring instrument, and the automatic test is started. The default refractive index of the particles is 1.81, and the particle size distribution test is completed, and the D 10 , D 50 and D 90 Data results. Moreover, the weight average molecular weight of the polyphenylene sulfide resin in the reactants in the embodiments and comparative examples of the present invention was measured by gel permeation chromatography using narrow distribution polystyrene as a standard sample, the solvent was α-chloronaphthalene, and the column temperature was 210°C. In addition, the viscosity test of the reactants in the embodiments and comparative examples of the present invention was measured by a rotational rheometer MARS60 high pressure module at 260°C, with a shear rate of 20s -1 .
[0073] Example 1
[0074] In a 100L reactor, 19.8kg (200.0mol) of N-methylpyrrolidone, 9.7kg (97mol) of 40% sodium hydroxide aqueous solution, and 14.01kg (100.0mol) of 40% sodium hydrosulfide aqueous solution were added, and the temperature was raised to 130°C at a rate of 2.0°C / min under nitrogen protection at a stirring speed of 300rpm, then to 160°C at a rate of 0.5°C / min, and finally to 210°C at a rate of 1°C / min, and 14.16kg of aqueous solution (water content 98.0%) was removed. After the removal and dehydration was completed, the temperature was lowered to 160°C. At this time, the amount of sulfur in the system was 98.0mol and the water content was 117.6mol.
[0075] 15.14 kg (103.0 mol) of p-dichlorobenzene and 10.2 kg (103 mol) of NMP were added into the above-mentioned reactor, and the temperature was raised to 260° C. at a rate of 0.5° C. / min. After keeping the temperature for 3 hours, a reactant containing polyphenylene sulfide resin was obtained, wherein the weight average molecular weight of the polyphenylene sulfide resin in the reactant was 20,000, and the viscosity of the reactant was 1.5 Pa.s.
[0076] Then the reactant is heated to 290°C, discharged into a normal pressure flash evaporator, and 290°C superheated steam is introduced. The steam consumption per 1kg of reactant discharged is 0.5kg. After the flash evaporation is completed, the reaction mixture is dried until the residual amount of the solvent is less than 0.2wt%, and then the temperature is lowered to obtain 20.9kg of crude product. 60kg of deionized water is added to the crude product, and after stirring for 3 hours, a primary filter cake is obtained after suction filtration. An appropriate amount of the primary filter cake is dried and sieved with a 150-mesh screen, and the content of the screened material is measured to be 35wt%. The remaining primary filter cake is slurried with 50kg of deionized water to obtain a mixture, acetic acid is added to the mixture to adjust the pH to 6, and then the mixture is sent to a foam flotation machine for cyclic flotation to obtain a foam phase. Add 10 kg of deionized water to the foam phase, add an appropriate amount of NaOH to adjust the pH to 9.5, transfer to a high-temperature water washing device after defoaming, heat to 200 ° C, keep warm for 30 minutes, cool down, filter and dry to obtain 1.5 kg of polyphenylene sulfide resin particles, of which D 50 15μm, D 90 / D 10 is 7.
[0077] Example 2
[0078] The difference between Example 2 and Example 1 is that the mixture is not subjected to acid treatment, and the mixed slurry is not subjected to alkaline treatment. That is, the obtained mixture (pH is 10.9) is directly sent to the froth flotation machine for cyclic flotation to obtain a froth phase. The other conditions are the same, and 0.74 kg of polyphenylene sulfide resin particles are obtained, wherein D 50 10μm, D 90 / D 10 is 6.
[0079] Example 3
[0080] The difference between Example 3 and Example 1 is that acetic acid is added to the mixture to adjust the pH to 4, and then the mixture is sent to a froth flotation machine for cyclic flotation to obtain a froth phase. 10 kg of deionized water is added to the froth phase, and an appropriate amount of NaOH is added to adjust the pH to 9.5. After defoaming, the mixture is transferred to a high-temperature water washing device, heated to 200°C, kept warm for 30 minutes, cooled, filtered, and dried to obtain 0.45 kg of polyphenylene sulfide resin particles, wherein D 50 8μm, D 90 / D 10 is 5.
[0081] Example 4
[0082] The difference between Example 4 and Example 1 is that acetic acid is added to the mixture to adjust the pH to 8, and then the mixture is sent to a froth flotation machine for cyclic flotation to obtain a froth phase. 10 kg of deionized water is added to the froth phase, and an appropriate amount of NaOH is added to adjust the pH to 9.5. After defoaming, the mixture is transferred to a high-temperature water washing device, heated to 200°C, kept warm for 30 minutes, cooled, filtered, and dried to obtain 1.2 kg of polyphenylene sulfide resin particles, wherein D 50 14μm, D 90 / D 10 It is 6.8.
[0083] Example 5
[0084] The only difference between Example 5 and Example 1 is that 15.14 kg (103.0 mol) of p-dichlorobenzene and 8.2 kg (83 mol) of NMP are added to the above-mentioned reactor, and the temperature is raised to 260° C. at a rate of 0.5° C. / min. After keeping warm for 3 hours, a reactant containing polyphenylene sulfide resin is obtained, and the weight average molecular weight of the polyphenylene sulfide resin in the reactant is 21000, and the viscosity of the reactant is 1.8 Pa.s.
[0085] Then the reactants were heated to 290°C and discharged into a normal pressure flash tank. Superheated steam at 290°C was introduced. The steam consumption for each kg of reactants discharged was 0.5 kg. After the flash evaporation, the reaction was dried until the residual amount of the solvent was less than 0.2 wt%. Then, the reaction was cooled to obtain 20.9 kg of crude product. 60 kg of deionized water was added to the crude product. After stirring for 3 hours, a primary filter cake was obtained after suction filtration. An appropriate amount of the primary filter cake was dried and sieved with a 150-mesh sieve. The content of the sieve was measured to be 30 wt%. The remaining primary filter cake was slurried with 50 kg of deionized water to obtain a mixture. The other conditions were the same to obtain 1.2 kg of polyphenylene sulfide resin particles, wherein D 50 16μm, D 90 / D 10 It is 7.2.
[0086] Example 6
[0087] The only difference between Example 6 and Example 1 is that 15.14 kg (103.0 mol) of p-dichlorobenzene and 13.2 kg (133 mol) of NMP NMP are added to the above-mentioned reactor, the temperature is raised to 260°C at a rate of 0.5°C / min, and after keeping warm for 3 hours, a reactant containing polyphenylene sulfide resin is obtained, the weight average molecular weight of the polyphenylene sulfide resin in the reactant is 19500, and the viscosity of the reactant is 1.2 Pa.s.
[0088] Then the reactants were heated to 290°C and discharged into a normal pressure flash tank. Superheated steam at 290°C was introduced. The steam consumption for each kg of reactants discharged was 0.5 kg. After the flash evaporation, the reaction was dried until the residual amount of the solvent was less than 0.2 wt%. Then, the reaction was cooled to obtain 20.9 kg of crude product. 60 kg of deionized water was added to the crude product. After stirring for 3 hours, a primary filter cake was obtained after suction filtration. An appropriate amount of the primary filter cake was dried and sieved with a 150-mesh sieve. The content of the sieve was 34 wt%. The remaining primary filter cake was slurried with 50 kg of deionized water to obtain a mixture. The other conditions were the same to obtain 1.4 kg of polyphenylene sulfide resin particles, of which D 50 14μm, D 90 / D 10 is 7.
[0089] Example 7
[0090] Compared with Example 1, Example 7 is different from Example 1 only in that 19.8 kg (200.0 mol) of N-methylpyrrolidone, 10.1 kg (101 mol) of 40% sodium hydroxide aqueous solution, and 14.01 kg (100.0 mol) of 40% sodium hydrosulfide aqueous solution are added to a 100 L reactor, and the temperature is raised to 130° C. at a stirring speed of 300 rpm and under nitrogen protection at a rate of 2.0° C. / min, then raised to 160° C. at a rate of 0.5° C. / min, and finally raised to 210° C. at a rate of 1° C. / min, 14.4 kg of aqueous solution (water content 98.0%) is removed, and after the removal and dehydration are completed, the temperature is lowered to 160° C. At this time, the amount of sulfur in the system is 98 mol, and the water content is 117.6 mol.
[0091] 15.14 kg (103.0 mol) of p-dichlorobenzene and 10.2 kg (103 mol) of NMP were added to the above reactor, and the temperature was raised to 260° C. at a rate of 0.5° C. / min. After being kept warm for 3 hours, a reactant containing polyphenylene sulfide resin was obtained, wherein the weight average molecular weight of the polyphenylene sulfide resin in the reactant was 20500, and the viscosity of the reactant was 1.6 Pa.s. The other conditions were the same, and 1.6 kg of polyphenylene sulfide resin particles were obtained, wherein D 50 18μm, D 90 / D 10 It is 7.5.
[0092] Example 8
[0093] Compared with Example 1, Example 8 is different from Example 1 only in that 19.8 kg (200.0 mol) of N-methylpyrrolidone, 10.4 kg (104 mol) of 40% sodium hydroxide aqueous solution, 14.01 kg (100.0 mol) of 40% sodium hydrosulfide aqueous solution, and 1 kg (5 mol) of 41% sodium acetate aqueous solution are added to a 100 L reactor, and the temperature is raised to 130° C. at a stirring speed of 300 rpm and under nitrogen protection at a rate of 2.0° C. / min, then raised to 160° C. at a rate of 0.5° C. / min, and finally raised to 210° C. at a rate of 1° C. / min, 14.58 kg of aqueous solution (water content 98.0%) is removed, and after the removal and dehydration are completed, the temperature is lowered to 160° C. At this time, the amount of sulfur in the system is 98 mol, and the water content is 117.6 mol.
[0094] 15.14 kg (103.0 mol) of p-dichlorobenzene and 10.2 kg (103 mol) of NMP were added into the above-mentioned reactor, and the temperature was raised to 260° C. at a rate of 0.5° C. / min. After keeping the temperature for 3 hours, a reactant containing polyphenylene sulfide resin was obtained, wherein the weight average molecular weight of the polyphenylene sulfide resin in the reactant was 21,000, and the viscosity of the reactant was 1.7 Pa.s.
[0095] Then the reactant is heated to 290°C and discharged into a normal pressure flash evaporator, and 290°C superheated steam is introduced. The steam consumption for each 1kg of reactant discharged is 0.5kg. After the flash evaporation is completed, the drying is continued until the residual amount of the polar organic solvent is less than 0.2wt%, and the temperature is lowered to obtain 20.9kg of crude product. 60kg of deionized water is added to the crude product, and after stirring for 3 hours, a primary filter cake is obtained after suction filtration. An appropriate amount of the primary filter cake is dried and sieved with a 150-mesh sieve, and the content of the sieve is measured to be 32wt%. The remaining primary filter cake is added with 50kg of deionized water to make a pulp to obtain a mixture. The other conditions are the same to obtain 1.1kg of polyphenylene sulfide resin particles, wherein D 50 13μm, D 90 / D 10 is 6.
[0096] Example 9
[0097] Compared with Example 1, Example 9 is different from Example 1 in that 19.8 kg (200.0 mol) of N-methylpyrrolidone, 9.7 kg (97 mol) of 40% sodium hydroxide aqueous solution, 14.01 kg (100.0 mol) of 40% sodium hydrosulfide aqueous solution, and 1 kg (5 mol) of 41% sodium acetate aqueous solution are added to a 100 L reactor, and the temperature is raised to 130° C. at a stirring speed of 300 rpm and under nitrogen protection at a rate of 2.0° C. / min, then raised to 160° C. at a rate of 0.5° C. / min, and finally raised to 210° C. at a rate of 1° C. / min, 14.76 kg of aqueous solution (water content 98.0%) is removed, and after the removal and dehydration are completed, the temperature is lowered to 160° C. At this time, the amount of sulfur in the system is 198 mol, and the water content is 117.6 mol.
[0098] 15.14 kg (103.0 mol) of p-dichlorobenzene and 10.2 kg (103 mol) of NMP were added into the above-mentioned reactor, and the temperature was raised to 260° C. at a rate of 0.5° C. / min. After keeping the temperature for 3 hours, a reactant containing polyphenylene sulfide resin was obtained, wherein the weight average molecular weight of the polyphenylene sulfide resin in the reactant was 26,000, and the viscosity of the reactant was 3 Pa.s.
[0099] Then the reactant is heated to 290°C and discharged into a normal pressure flash evaporator, while superheated steam at 290°C is introduced. The steam consumption for each 1kg of reactant discharged is 0.5kg. After the flash evaporation is completed, the reaction is dried until the residual amount of the polar organic solvent is less than 0.2wt%, and then the temperature is lowered to obtain 21.3kg of crude product. 60kg of deionized water is added to the crude product, and after stirring for 3 hours, a primary filter cake is obtained after suction filtration. An appropriate amount of the primary filter cake is dried and sieved with a 150-mesh sieve, and the content of the sieve is measured to be 24wt%. The remaining primary filter cake is slurried with 50kg of deionized water to obtain a mixture. The other conditions are the same to obtain 1kg of polyphenylene sulfide resin particles, wherein D 50 20μm, D 90 / D 10 It is 7.8.
[0100] Example 10
[0101] The only difference between Example 10 and Example 1 is that 14.85 kg (101.0 mol) of p-dichlorobenzene and 10.2 kg (103 mol) of NMP are added to the above-mentioned reactor, and the temperature is raised to 260° C. at a rate of 0.5° C. / min. After keeping warm for 3 hours, a reactant containing polyphenylene sulfide resin is obtained, wherein the weight average molecular weight of the polyphenylene sulfide resin in the reactant is 25800, and the viscosity of the reactant is 2.7 Pa.s.
[0102] Then the reactant is heated to 290°C and discharged into a normal pressure flash evaporator, while superheated steam at 290°C is introduced. The steam consumption for each 1kg of reactant discharged is 0.5kg. After the flash evaporation is completed, the reaction is dried until the residual amount of the polar organic solvent is less than 0.2wt%, and then the temperature is lowered to obtain 20.9kg of crude product. 60kg of deionized water is added to the crude product, and after stirring for 3 hours, a primary filter cake is obtained after suction filtration. An appropriate amount of the primary filter cake is dried and sieved with a 150-mesh sieve, and the content of the sieve is measured to be 26wt%. The remaining primary filter cake is slurried with 50kg of deionized water to obtain a mixture. The other conditions are the same to obtain 1.1kg of polyphenylene sulfide resin particles, wherein D 50 20μm, D 90 / D 10 is 8.0.
[0103] Embodiment 11
[0104] Example 11 is different from Example 1 only in that 19.8 kg (200.0 mol) of N-methylpyrrolidone, 9.7 kg (97 mol) of 40% sodium hydroxide aqueous solution, and 14.01 kg (100.0 mol) of 40% sodium hydrosulfide aqueous solution are added to a 100 L reactor, and the temperature is raised to 130° C. at a stirring speed of 300 rpm and under nitrogen protection at a rate of 2.0° C. / min, then raised to 160° C. at a rate of 0.5° C. / min, and finally raised to 203° C. at a rate of 1° C. / min, 13.44 kg of aqueous solution (water content 98.0%) is removed, and after the removal and dehydration are completed, the temperature is lowered to 160° C. At this time, the amount of sulfur in the system is 98 mol, and the water content is 156.8 mol.
[0105] 15.14 kg (103.0 mol) of p-dichlorobenzene and 10.2 kg (103 mol) of NMP were added into the above-mentioned reactor, and the temperature was raised to 260° C. at a rate of 0.5° C. / min. After keeping the temperature for 3 hours, a reactant containing polyphenylene sulfide resin was obtained, wherein the weight average molecular weight of the polyphenylene sulfide resin in the reactant was 18,000, and the viscosity of the reactant was 1.3 Pa.s.
[0106] Then the reactants were heated to 290°C and discharged into a normal pressure flash evaporator, where superheated steam at 290°C was introduced. The steam consumption for each kg of reactants discharged was 0.5 kg. After the flash evaporation was completed, the reaction mixture was dried until the residual amount of the solvent was less than 0.2 wt %, and then the temperature was lowered to obtain 20.9 kg of crude product. 60 kg of deionized water was added to the crude product, and after stirring for 3 hours, a primary filter cake was obtained after suction filtration. An appropriate amount of the primary filter cake was dried and sieved with a 150-mesh sieve, and the content of the sieve was measured to be 28 wt %. The remaining primary filter cake was slurried with 50 kg of deionized water to obtain a mixture. The remaining conditions were the same, and 1.2 kg of polyphenylene sulfide resin particles were obtained, wherein D 50 14μm, D 90 / D 10 It is 6.5.
[0107] Example 12
[0108] Compared with Example 1, Example 12 differs only in that the reactants are heated to 290°C, discharged into a normal pressure flash evaporator, and superheated steam at 290°C is introduced. The amount of steam consumed for each 1 kg of reactant discharged is 0.25 kg. Drying is continued after the flash evaporation is completed until the residual amount of the solvent is less than 0.2 wt%, and cooling is started to obtain 20.9 kg of crude product. 60 kg of deionized water is added to the crude product, stirred for 3 hours, and filtered to obtain a primary filter cake. Take an appropriate amount of the primary filter cake, dry it, and sieve it with a 150-mesh sieve. The content of the sieve is measured to be 20 wt%. The remaining primary filter cakes are added with 50 kg of deionized water to make pulp to obtain a mixture. The other conditions are the same to obtain 0.8 kg of polyphenylene sulfide resin particles, wherein D 50 20μm, D 90 / D 10 is 6.
[0109] Example 13
[0110] Compared with Example 1, Example 13 differs only in that the reactants are heated to 270°C, discharged into a normal pressure flash evaporator, and superheated steam at 290°C is introduced. The amount of steam consumed for each 1 kg of reactant discharged is 0.25 kg. Drying is continued after the flash evaporation is completed until the residual amount of the solvent is less than 0.2 wt%, and cooling is started to obtain 20.9 kg of crude product. 60 kg of deionized water is added to the crude product, stirred for 3 hours, and filtered to obtain a primary filter cake. Take an appropriate amount of the primary filter cake, dry it, and sieve it with a 150-mesh sieve. The content of the sieve is measured to be 27 wt%. The remaining primary filter cakes are added with 50 kg of deionized water to make pulp to obtain a mixture. The other conditions are the same to obtain 1.15 kg of polyphenylene sulfide resin particles, wherein D 50 14μm, D 90 / D 10 It is 6.4.
[0111] Comparative Example 1
[0112] In a 100L reactor, 19.8kg (200.0mol) of N-methylpyrrolidone, 9.7kg (97mol) of 40% sodium hydroxide aqueous solution, 14.01kg (100.0mol) of 40% sodium hydrosulfide aqueous solution, and 4kg (20.0mol) of 41% anhydrous sodium acetate aqueous solution were added, and the mixture was heated to 130°C at a rate of 2.0°C / min under nitrogen protection at a stirring speed of 300rpm, then to 160°C at a rate of 0.5°C / min, and finally to 210°C at a rate of 1°C / min, and 16.56kg of aqueous solution (water content 98.0%) was removed. After the removal and dehydration was completed, the temperature was lowered to 160°C. At this time, the amount of sulfur in the system was 98.0mol, and the water content was 117.6mol.
[0113] 14.99 kg (102.0 mol) of p-dichlorobenzene and 14.2 kg (143 mol) of NMP were added into the above-mentioned reactor, and the temperature was raised to 260° C. at a rate of 0.5° C. / min. After keeping warm for 3 hours, a reactant containing polyphenylene sulfide resin was obtained, wherein the weight average molecular weight of the polyphenylene sulfide resin in the reactant was 40,000, and the viscosity of the reactant was 6 Pa.s.
[0114] Then the temperature was raised to 290°C and discharged into a normal pressure flash evaporator. After the flash evaporation was completed, the material was dried until the residual amount of the solvent was less than 0.2wt%, and then the temperature was lowered to obtain 22.5kg of crude product. 60kg of deionized water was added to the crude product, and then stirred for 3 hours, and filtered to obtain a primary filter cake. An appropriate amount of the primary filter cake was dried and sieved with a 150-mesh sieve. The content of the material under the sieve was measured to be 10wt%. 50kg of deionized water was added, the temperature was raised to 200°C, and the temperature was kept for 30 minutes before being cooled to room temperature. After filtration and drying, 0.3kg of polyphenylene sulfide resin particles were obtained, of which D 50 28μm, D 90 / D 10 is 8.
[0115] Comparative Example 2
[0116] Comparative Example 2 is compared with Example 1, except that 16.13 kg (103.0 mol) of p-dichlorobenzene and 10.2 kg (103 mol) of NMP are added to the above-mentioned reactor, and the temperature is raised to 260° C. at a rate of 0.5° C. / min. After keeping warm for 3 hours, a reactant containing polyphenylene sulfide resin is obtained, wherein the weight average molecular weight of the polyphenylene sulfide resin in the reactant is 14000, and the viscosity of the reactant is 0.8 Pa.s.
[0117] Then the reactant is heated to 290°C and discharged into a normal pressure flash evaporator, while superheated steam at 290°C is introduced. The steam consumption for each 1kg of reactant discharged is 0.5kg. After the flash evaporation is completed, the reaction is dried until the residual amount of the polar organic solvent is less than 0.2wt%, and then the temperature is lowered to obtain 20.9kg of crude product. 60kg of deionized water is added to the crude product, and after stirring for 3 hours, a primary filter cake is obtained after suction filtration. An appropriate amount of the primary filter cake is dried and sieved with a 150-mesh sieve, and the content of the sieve is measured to be 40wt%. The remaining primary filter cake is slurried with 50kg of deionized water to obtain a mixture. The other conditions are the same to obtain 1.8kg of polyphenylene sulfide resin particles, wherein D 50 12μm, D 90 / D 10 It is 8.2.
[0118] Comparative Example 3
[0119] Comparative Example 3 is different from Example 1 in that the obtained mixture is directly transferred to a high-temperature water washing device without flotation, heated to 200°C, kept warm for 30 minutes, cooled, filtered, and dried to obtain 9.95 kg of polyphenylene sulfide resin particles, wherein D 50 50μm, D 90 / D 10 is 14.
[0120] Comparative Example 4
[0121] Comparative Example 4 is different from Example 1 only in that 15.14 kg (103.0 mol) of p-dichlorobenzene and 20.05 kg (253 mol) of NMP are added to the above reactor, and the temperature is raised to 260° C. at a rate of 0.5° C. / min. After being kept warm for 3 hours, a reactant containing polyphenylene sulfide resin is obtained, wherein the weight average molecular weight of the polyphenylene sulfide resin in the reactant is 19000, and the viscosity of the reactant is 0.8 Pa.s. The other conditions are the same, and 0.15 kg of polyphenylene sulfide resin particles are obtained, wherein D 50 25μm, D 90 / D 10 It is 7.5.
[0122] The D of the polyphenylene sulfide resin particles of Examples 1-13 and the polyphenylene sulfide resin particles of Comparative Examples 1-4 50 , D 90 / D 10The data show that by controlling the viscosity of the reactants and the molar ratio of NMP to the sulfur source in the reaction, and optimizing the process parameters during flash evaporation of the reactants, the removal effect of the solvent in the reactants during flash evaporation can be improved, and a crude polyphenylene sulfide resin product with a small particle size can be obtained, and the content of polyphenylene sulfide resin microparticles is higher. Since the polyphenylene sulfide resin itself has hydrophobic properties, and small-sized polyphenylene sulfide resin microparticles can selectively adhere to bubbles, the present invention directly performs foam flotation on the crude product to screen out polyphenylene sulfide resin microparticles with a small particle size and a narrow particle size distribution.
[0123] At the same time, since the crude product contains the main by-products produced in the polymerization reaction (such as dimers of nitrogen-containing sodium methylbutyrate end groups and trimers of nitrogen-containing sodium methylbutyrate end groups), the by-products have high surface activity and can be used as foaming agents. Therefore, in the froth flotation step, there is no need to add additional highly polluting foaming agents.
[0124] Therefore, the method for preparing polyphenylene sulfide resin microparticles of the present invention can not only efficiently prepare polyphenylene sulfide resin microparticles with small particle size and narrow particle size distribution, but also has low cost.
[0125] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.
[0126] The above-mentioned embodiments only express several implementation methods of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, and these all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.
Claims
1. A method for preparing polyphenylene sulfide resin particles, characterized in that: The preparation method comprises the following steps: A sulfur source, an alkali metal hydroxide solution and a first polar organic solvent are mixed in the presence or absence of an auxiliary agent and dehydrated to obtain a dehydrated liquid, and then the dehydrated liquid is mixed with a dihalogen aromatic compound and a second polar organic solvent for polymerization reaction to obtain a reactant containing polyphenylene sulfide resin, wherein the viscosity of the reactant is 1Pa·s-5Pa·s, the weight average molecular weight of the polyphenylene sulfide resin in the reactant is 15000-30000, the ratio of the sum of the molar amounts of the first polar organic solvent and the second polar organic solvent to the molar amount of the sulfur source is 2.8:1-3.3:1, the first polar organic solvent and the second polar organic solvent are both selected from organic amide solvents, and the dihalogen aromatic compound is selected from p-dichlorobenzene; Flash distilling the reactant to obtain a crude product; The crude product is mixed with water to form a mixture, and gas is introduced into the mixture for froth flotation, and polyphenylene sulfide resin particles are separated from the froth phase, wherein the polyphenylene sulfide resin particles have a D 50 ≤20μm, D 90 / D 10 ≤8.
2. The method for preparing polyphenylene sulfide resin particles according to claim 1, characterized in that: The weight average molecular weight of the polyphenylene sulfide resin in the reactants is 18000-30000.
3. The method for preparing polyphenylene sulfide resin particles according to claim 1, characterized in that: The molar ratio of the alkali metal hydroxide solution to the sulfur source is 0.97:1-1.01:1; and / or, the molar ratio of the auxiliary agent to the sulfur source is less than or equal to 0.1:1; And / or, the molar ratio of water to sulfur in the dehydrated liquid is 1.0:1-1.3:
1.
4. The method for preparing polyphenylene sulfide resin particles according to claim 1, characterized in that: The molar ratio of the dihalogen aromatic compound to the sulfur source is 1.03:1-1.06:
1.
5. The method for preparing polyphenylene sulfide resin particles according to claim 1, characterized in that: The sulfur source is selected from sodium hydrosulfide and / or potassium hydrosulfide; And / or, the alkali metal hydroxide solution is selected from sodium hydroxide solution and / or potassium hydroxide solution; And / or, the auxiliary agent is selected from at least one of sodium acetate, sodium benzoate, and sodium of C5-C6 fatty acid; And / or, the organic amide solvent is at least one selected from N-methylpyrrolidone, hexamethylphosphotriamine, and N-methyl-ε-caprolactam.
6. The method for preparing polyphenylene sulfide resin particles according to claim 1, characterized in that: In the step of flash evaporating the reactants, steam is introduced into the flash evaporator, the steam temperature is 270°C-310°C, and the temperature of the reactants is 270°C-290°C; And / or, in the step of flash evaporating the reactant, the mass of the steam is 0.1kg-0.5kg based on 1kg of the reactant.
7. The method for preparing polyphenylene sulfide resin particles according to claim 1, characterized in that: In the step of flash evaporating the reactant, after the flash evaporation is completed, the flash evaporation product is further dried until the residual amount of the solvent is less than 0.2wt%, to obtain the crude product; And / or, in the step of performing froth flotation, the pH value of the mixture is adjusted to 5-7, and in the step of separating polyphenylene sulfide resin microparticles from the froth phase, the froth phase and water are mixed to form a mixed slurry, and the pH value of the mixed slurry is adjusted to 8-10, and then washed with water to obtain the polyphenylene sulfide resin microparticles.
8. The method for preparing polyphenylene sulfide resin particles according to claim 1, characterized in that: In the step of mixing the crude product with water to form a mixture, the mass ratio of polyphenylene sulfide to water in the crude product is 1:4-1:20; And / or, in the step of mixing the crude product with water to form a mixture, the crude product and water are firstly slurried, separated and then mixed with water again to form the mixture.
9. The method for preparing polyphenylene sulfide resin particles according to any one of claims 1 to 8, characterized in that: In the step of obtaining the foam phase, a mother liquor is also obtained, and the mother liquor is recycled for preparing the mixture; Alternatively, a conventional polyphenylene sulfide resin powder product is directly separated from the mother liquor.
10. Polyphenylene sulfide resin microparticles prepared by the method for preparing polyphenylene sulfide resin microparticles according to any one of claims 1 to 9.
Citation Information
Patent Citations
Process for producing fine particles of polyphenylene sulfide resin, fine particles of polyphenylene sulfide resin, and dispersion thereof
CN101981091A
Process for preparing particles of polyphenylene sulfide polymer
CN110741032A
Industrial production process and device of injection molding grade polyphenylene sulfide resin
CN111533910A
Method of Improving the Melt Properties of Poly(Arylene Sulfide) Polymers
US20150105524A1
Clean production process of polyphenylene sulfide and treatment method of polyphenylene sulfide reaction liquid
CN114479082A