A method for preparing construction solid waste recycled sand powder concrete

By treating construction solid waste sand powder with alkali excitation and mixing it with cement and other materials, a recycled sand powder concrete with high early strength and crack resistance is prepared, which solves the problem of insufficient strength and durability of existing recycled concrete and improves its performance. application value.

CN117865582BActive Publication Date: 2024-10-25SUQIAN MUNICIPAL BUILDING MATERIALS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410125855.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-01-30
Publication Date
2024-10-25
Estimated Expiration
2044-01-30

AI Technical Summary

Technical Problem

The existing recycled concrete has low strength and poor durability, and is limited by its application fields, resulting in low utilization rate.

Method used

Use an alkali activator to treat construction solid waste sand powder to form regenerated sand powder, and mix it with cement, aggregate, fly ash, and water-reducing agent. Concrete is prepared after stirring and curing. A sodium silicate & zinc aluminum tartrate composite solution is used as the Alkaline activator to improve the early strength of concrete and slow down dry shrinkage cracking.

Benefits of technology

It improves the early strength and crack resistance of concrete, slows down the phenomenon of dry shrinkage and cracking, and significantly improves the mechanical properties of recycled sand powder concrete.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
Patent Text Reader

Abstract

The present invention relates to a construction solid waste recycled sand powder concrete and a preparation method thereof, comprising the following steps: step 1, collecting construction solid waste materials, and obtaining solid waste sand powder after crushing; step 2, subjecting the solid waste sand powder to alkali excitation treatment under the action of an alkali activator to obtain recycled sand powder; step 3, mixing the recycled sand powder with cement, aggregate, fly ash, a water reducer and water, and then stirring evenly to form a mixed slurry; step 4, preparing recycled sand powder concrete. The present invention treats construction solid waste materials and then uses them in the preparation of concrete. Among them, the treatment process for construction solid waste materials is mainly alkali excitation treatment, and the alkali activator sodium silicate & zinc aluminum tartrate composite solution used in the present invention, the solid waste sand powder treated by the present invention is used in concrete, which can not only enable the concrete to maintain the advantage of high early strength, but also overcome the defect that traditional alkali excitation treatment is prone to cracking.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of concrete, and in particular to a method for preparing construction solid waste recycled sand powder concrete. Background Art

[0002] With the advancement of urbanization, the construction waste as a by-product is also increasing. The amount of waste concrete demolished each year is huge, and the accompanying construction waste is increasing day by day.

[0003] The construction waste formed by the concrete of abandoned buildings is crushed to form recycled concrete for recycling, which not only handles a large amount of construction waste, but also saves construction materials. However, the recycled concrete aggregate obtained after the waste concrete and abandoned bricks are crushed has too many edges and corners, and most of the recycled aggregates are needle-shaped. In addition, tiny cracks will appear inside the aggregate during the crushing process of the recycled aggregate. At the same time, a part of the old mortar is generally adhered to the surface of the recycled aggregate, which makes the recycled aggregate have the characteristics of large crushing index, high water absorption rate, large porosity, and low apparent density compared with natural aggregate. These characteristics of recycled aggregates lead to low strength and poor durability of recycled concrete. Therefore, recycled concrete is currently mostly used in non-structural and non-load-bearing concrete fields such as backfill and roadbed. Due to the limitation of application fields, the utilization rate of recycled concrete is very low. The low mechanical properties of recycled concrete have become a bottleneck restricting the application of recycled concrete. Summary of the invention

[0004] In view of the problems existing in the prior art, the purpose of the present invention is to provide a method for preparing recycled sand powder concrete from construction solid waste.

[0005] The purpose of the present invention is achieved by the following technical solutions:

[0006] In a first aspect, the present invention discloses a method for preparing construction solid waste recycled sand powder concrete, comprising the following steps:

[0007] Step 1, collecting construction solid waste materials and crushing them to obtain solid waste sand powder;

[0008] Step 2, subjecting the solid waste sand powder to an alkali excitation treatment under the action of an alkali exciter to obtain regenerated sand powder;

[0009] Step 3, mixing the regenerated sand powder with cement, aggregate, fly ash, water reducing agent and water, and then stirring evenly to form a mixed slurry;

[0010] Step 4, pour the mixed slurry into a mold, knock to remove bubbles, let it stand for 2-3 days, then remove the mold, and cure for 7-14 days to obtain recycled sand powder concrete.

[0011] Preferably, the solid waste sand powder obtained in step 1 has a median particle size of 27.6 μm, the content of particles with a particle size less than 75 μm is 83.74%, the content of particles with a particle size less than 40 μm is 57.52%, and the content of particles with a particle size less than 10 μm is 23.25%.

[0012] Preferably, the crushing process in step 1 comprises: first using a crusher to crush the collected solid construction waste materials into particles with a size less than 5 mm, placing them in an oven for treatment until they are dry, and then finely grinding them in a ball mill to a desired particle size.

[0013] Preferably, in step 2, the process of treating solid waste sand powder with an alkali activator includes: mixing the solid waste sand powder and the alkali activator in a mixer, stirring at a speed of 100-200 r / min for 15-30 min, and then drying in an oven to obtain regenerated sand powder.

[0014] Preferably, the alkaline activator in step 2 is a sodium silicate & zinc aluminum tartrate composite solution, and the preparation process is as follows:

[0015] (1) weighing tartaric acid and deionized water, mixing, adding a silane coupling agent, and stirring thoroughly to obtain a tartaric acid solution;

[0016] (2) mixing zinc chloride and aluminum chloride into deionized water, and mixing and stirring thoroughly to obtain a zinc-aluminum mixed solution;

[0017] (3) mixing the tartaric acid solution and the zinc-aluminum mixed solution, heating to 110-120° C., reacting for 2-3 hours, cooling to 40-50° C., collecting the filtrate by filtration, adjusting the pH of the reaction solution to 7.0-8.0, and drying to obtain zinc-aluminum tartrate;

[0018] (4) Sodium silicate and deionized water are mixed, and then zinc aluminum tartrate is added and fully dispersed to form an alkaline activator.

[0019] Preferably, in step (1), the tartaric acid is DL-tartaric acid, and the silane coupling agent is one of KH-550, KH-560, and KH-570.

[0020] Preferably, in the tartaric acid solution of step (1), the mass ratio of tartaric acid, silane coupling agent and deionized water is 1.5-3:0.2-0.4:20-30.

[0021] Preferably, in the zinc-aluminum mixed solution of step (2), the mass ratio of zinc chloride, aluminum chloride and deionized water is 1.36-2.72:0.67-1.33:20-40.

[0022] Preferably, in step (3), the mass ratio of tartaric acid solution to zinc-aluminum mixed solution is 1.5-2:1.

[0023] Preferably, in step (4), the mass ratio of sodium silicate, zinc aluminum tartrate and deionized water is 1.8-3.6:0.2-0.8:10.

[0024] Preferably, in step 3, the mass ratio of cement, aggregate, regenerated sand powder, fly ash, water reducer and water is 100-150:278-426:29-58:30-50:3-8:180-260.

[0025] Preferably, in step 3, the aggregate includes coarse aggregate and fine aggregate, the coarse aggregate is stone with a particle size of 4.75-9.5 mm, the fine aggregate is gravel with a particle size less than 4.75 mm, and the mass ratio of coarse aggregate to fine aggregate is 1.5-1.8:1.

[0026] Preferably, in step 3, the cement is ordinary silicate cement PO42.5, the fly ash type is grade I, and the water reducer is naphthalene-based high-efficiency water reducer SY-05.

[0027] Preferably, in step 4, the curing is performed by covering the surface with a plastic film having a thickness of 0.1 mm, avoiding direct sunlight, and spraying water to replenish moisture when necessary.

[0028] In a second aspect, the present invention discloses a construction solid waste recycled sand powder concrete, which is prepared by the above method.

[0029] The beneficial effects of the present invention are:

[0030] 1. The present invention processes construction solid waste materials and then uses them in the preparation of concrete. The process of treating construction solid waste materials is mainly alkali activation treatment. The alkali activator sodium silicate & zinc aluminum tartrate composite solution used in the present invention is used in concrete. The solid waste sand powder treated by the present invention can not only make the concrete maintain the advantage of high early strength, but also overcome the defect of easy cracking in traditional alkali activation treatment.

[0031] 2. The materials treated with alkali activation can increase the early strength and drying time of concrete when used in concrete, but they have the defects of large brittleness and low toughness, which makes them prone to shrinkage and cracking. In order to improve this phenomenon, the present invention adds a certain amount of zinc aluminum tartrate to the conventional sodium silicate solution. The presence of zinc aluminum tartrate can act as a buffer. On the one hand, during the mixing of the alkali activator and the sand powder, zinc aluminum tartrate can be coated on the surface of the sand powder, which alleviates the reaction between the sand powder and the alkali to a certain extent. On the other hand, zinc and aluminum in zinc aluminum tartrate are both amphoteric metals, which can consume a certain amount of alkali during the concrete curing process, slowing down the generation of expanded gel.

[0032] 3. The alkaline activator used in the present invention uses amphoteric metals zinc and aluminum. The tartrates of the two metals are highly water-soluble and can be dispersed more evenly in the solvent. If insoluble metals such as calcium are used, the dispersibility and stability of the alkaline activator will be reduced, thereby affecting its performance. In addition, the present invention also found that the tartrate obtained by using a certain ratio of zinc and aluminum has better performance than pure aluminum tartrate or zinc tartrate. DETAILED DESCRIPTION

[0033] The technical solution of the present invention is described below through specific examples. It should be understood that the one or more method steps mentioned in the present invention do not exclude the existence of other method steps before and after the combination step or the insertion of other method steps between these explicitly mentioned steps; it should also be understood that these embodiments are only used to illustrate the present invention and are not used to limit the scope of the present invention. Moreover, unless otherwise specified, the numbering of each method step is only a convenient tool for identifying each method step, and is not intended to limit the order of arrangement of each method step or to limit the scope of the present invention. The change or adjustment of the relative relationship thereof shall also be regarded as the scope of the present invention without substantially changing the technical content.

[0034] In order to better understand the above technical scheme, the exemplary embodiments of the present invention are described in more detail below. Although exemplary embodiments of the present invention are shown, it should be understood that the present invention can be implemented in various forms and should not be limited by the embodiments set forth herein. On the contrary, these embodiments are provided in order to enable a more thorough understanding of the present invention and to enable the scope of the present invention to be fully communicated to those skilled in the art.

[0035] The present invention will be further described below in conjunction with the following examples.

[0036] Example 1

[0037] A method for preparing construction solid waste recycled sand powder concrete comprises the following steps:

[0038] Step 1, collecting construction solid waste materials, first using a crusher to crush the collected construction solid waste materials into particles with a size less than 5 mm, placing them in an oven to dry, and then finely grinding them in a ball mill to a desired particle size, to obtain solid waste sand powder with a median particle size of 27.6 μm, a content of particles with a particle size less than 75 μm of 83.74%, a content of particles with a particle size less than 40 μm of 57.52%, and a content of particles with a particle size less than 10 μm of 23.25%;

[0039] The composition of solid waste sand powder is shown in Table 1 below:

[0040] Table 1 Composition and content of solid waste sand powder

[0041]

[0042] Step 2, mixing the solid waste sand powder and the alkali activator into a mixer, stirring at a speed of 100-200 r / min for 15-30 min, and then drying in an oven to obtain regenerated sand powder;

[0043] Among them, the alkaline activator is a sodium silicate & zinc aluminum tartrate composite solution, and the preparation process is as follows:

[0044] (1) Weigh DL-tartaric acid and deionized water, mix them, and then add silane coupling agent KH-550, the mass ratio of tartaric acid, silane coupling agent and deionized water is 2.2:0.3:25, and after sufficient stirring, a tartaric acid solution is obtained;

[0045] (2) mixing zinc chloride and aluminum chloride into deionized water, wherein the mass ratio of zinc chloride, aluminum chloride and deionized water is 2.04:1:30, and mixing and stirring thoroughly to obtain a zinc-aluminum mixed solution;

[0046] (3) mixing a tartaric acid solution and a zinc-aluminum mixed solution in a mass ratio of 1.8:1, heating to 120° C., reacting for 2 hours, cooling to 45° C., collecting the filtrate by filtration, adjusting the pH of the reaction solution to 7.0-8.0, and drying to obtain zinc-aluminum tartrate;

[0047] (4) Sodium silicate and deionized water are mixed, and then zinc aluminum tartrate is added. The mass ratio of sodium silicate, zinc aluminum tartrate and deionized water is 2.7:0.5:10. After being fully dispersed, an alkaline activator is formed.

[0048] Step 3, mixing the regenerated sand powder with cement, aggregate, fly ash, water reducer and water, wherein the mass ratio of cement, aggregate, regenerated sand powder, fly ash, water reducer and water is 120:358:43:40:5:220, and then stirring evenly to form a mixed slurry;

[0049] Among them, the aggregates include coarse aggregate and fine aggregate. The coarse aggregate is stone with a particle size of 4.75-9.5mm, and the fine aggregate is gravel with a particle size less than 4.75mm. The mass ratio of coarse aggregate to fine aggregate is 1.6:1; the cement is ordinary Portland cement PO42.5, the fly ash model is Grade I, and the water reducer is naphthalene-based high-efficiency water reducer SY-05.

[0050] Step 4, pour the mixed slurry into the mold, knock to remove the bubbles, let it stand for 2-3 days, then remove the mold, and then cover it with a 0.1mm thick plastic film for curing for 7-14 days, avoid direct sunlight, and spray water to replenish moisture when necessary to obtain recycled sand powder concrete.

[0051] Example 2

[0052] A method for preparing construction solid waste recycled sand powder concrete, which is different from Example 1 in that the preparation process of the alkali activator in step 2 is slightly different, and the alkali activator is a sodium silicate & zinc aluminum tartrate composite solution, and the preparation process is as follows:

[0053] (1) Weigh DL-tartaric acid and deionized water, mix them, and then add silane coupling agent KH-560, the mass ratio of tartaric acid, silane coupling agent and deionized water is 1.5:0.2:20, and after sufficient stirring, a tartaric acid solution is obtained;

[0054] (2) mixing zinc chloride and aluminum chloride into deionized water, wherein the mass ratio of zinc chloride, aluminum chloride and deionized water is 1.36:0.67:20, and mixing and stirring thoroughly to obtain a zinc-aluminum mixed solution;

[0055] (3) mixing the tartaric acid solution and the zinc-aluminum mixed solution in a mass ratio of 1.5:1, heating to 110° C., reacting for 2 hours, cooling to 40° C., collecting the filtrate by filtration, adjusting the pH of the reaction solution to 7.0-8.0, and drying to obtain zinc-aluminum tartrate;

[0056] (4) Sodium silicate and deionized water are mixed, and then zinc aluminum tartrate is added. The mass ratio of sodium silicate, zinc aluminum tartrate and deionized water is 1.8:0.2:10. After being fully dispersed, an alkaline activator is formed.

[0057] Example 3

[0058] A method for preparing construction solid waste recycled sand powder concrete, which is different from Example 1 in that the preparation process of the alkali activator in step 2 is slightly different, and the alkali activator is a sodium silicate & zinc aluminum tartrate composite solution, and the preparation process is as follows:

[0059] (1) Weigh DL-tartaric acid and deionized water, mix them, and then add silane coupling agent KH-570, the mass ratio of tartaric acid, silane coupling agent and deionized water is 3:0.4:30, and after sufficient stirring, a tartaric acid solution is obtained;

[0060] (2) mixing zinc chloride and aluminum chloride into deionized water, wherein the mass ratio of zinc chloride, aluminum chloride and deionized water is 2.72:1.33:40, and mixing and stirring thoroughly to obtain a zinc-aluminum mixed solution;

[0061] (3) mixing a tartaric acid solution and a zinc-aluminum mixed solution in a mass ratio of 2:1, heating to 120° C., reacting for 3 hours, cooling to 50° C., collecting the filtrate by filtration, adjusting the pH of the reaction solution to 7.0-8.0, and drying to obtain zinc-aluminum tartrate;

[0062] (4) Sodium silicate and deionized water are mixed, and then zinc aluminum tartrate is added. The mass ratio of sodium silicate, zinc aluminum tartrate and deionized water is 3.6:0.8:10. After being fully dispersed, an alkaline activator is formed.

[0063] Example 4

[0064] A method for preparing recycled sand powder concrete from construction solid waste, which is different from Example 1 in that the content of each component in step 3 is slightly different. In step 3, the mass ratio of cement, aggregate, recycled sand powder, fly ash, water reducer and water is 100:278:29:30:3:180.

[0065] Example 5

[0066] A method for preparing construction solid waste recycled sand powder concrete, which is different from Example 1 in that the content of each component in step 3 is slightly different. In step 3, the mass ratio of cement, aggregate, recycled sand powder, fly ash, water reducer and water is 150:426:58:50:8:260.

[0067] Comparative Example 1

[0068] A method for preparing construction solid waste recycled sand powder concrete, the difference from Example 1 is that the alkali activator in step 2 is different. The alkali activator used in this comparative example is sodium silicate solution. The preparation process is as follows:

[0069] Sodium silicate and deionized water are mixed in a mass ratio of 2.7:10. After being fully dispersed, an alkali activator is formed.

[0070] Comparative Example 2

[0071] A method for preparing construction solid waste recycled sand powder concrete, the difference from Example 1 is that the alkali activator in step 2 is different. The alkali activator used in this comparative example is a sodium silicate & zinc tartrate composite solution, and the preparation process is as follows:

[0072] (1) Weigh DL-tartaric acid and deionized water, mix them, and then add silane coupling agent KH-550, the mass ratio of tartaric acid, silane coupling agent and deionized water is 2.2:0.3:25, and after sufficient stirring, a tartaric acid solution is obtained;

[0073] (2) mixing zinc chloride into deionized water in a mass ratio of zinc chloride to deionized water of 3.04:30, and mixing and stirring thoroughly to obtain zinc solution;

[0074] (3) mixing the tartaric acid solution and the zinc solution in a mass ratio of 1.8:1, heating to 120° C., reacting for 2 h, cooling to 45° C., collecting the filtrate by filtration, adjusting the pH of the reaction solution to 7.0-8.0, and drying to obtain zinc tartrate;

[0075] (4) Sodium silicate and deionized water are mixed, and then zinc tartrate is added. The mass ratio of sodium silicate, zinc tartrate and deionized water is 2.7:0.5:10. After being fully dispersed, an alkaline activator is formed.

[0076] Comparative Example 3

[0077] A method for preparing construction solid waste recycled sand powder concrete, the difference from Example 1 is that the alkali activator in step 2 is different. The alkali activator used in this comparative example is a sodium silicate & aluminum tartrate composite solution, and the preparation process is as follows:

[0078] (1) Weigh DL-tartaric acid and deionized water, mix them, and then add silane coupling agent KH-550, the mass ratio of tartaric acid, silane coupling agent and deionized water is 2.2:0.3:25, and after sufficient stirring, a tartaric acid solution is obtained;

[0079] (2) mixing aluminum chloride with deionized water in a mass ratio of aluminum chloride to deionized water of 3.04:30, and mixing and stirring thoroughly to obtain aluminum liquid;

[0080] (3) mixing tartaric acid solution and aluminum liquid in a mass ratio of 1.8:1, heating to 120° C., reacting for 2 h, cooling to 45° C., collecting the filtrate by filtration, adjusting the pH of the reaction solution to 7.0-8.0, and drying to obtain aluminum tartrate;

[0081] (4) Sodium silicate and deionized water are mixed, and then aluminum tartrate is added. The mass ratio of sodium silicate, aluminum tartrate and deionized water is 2.7:0.5:10. After being fully dispersed, an alkaline activator is formed.

[0082] Experimental example

[0083] The performance of the recycled sand powder concrete prepared in Example 1 and Comparative Examples 1-3 was tested and compared. The crack resistance grade was referenced to JGJ / T 193-2009 "Concrete Durability Test and Evaluation Standard", the compressive strength and flexural strength were referenced to GB / T50081-2002 "Ordinary Concrete Mechanical Properties Test Method Standard", and the shrinkage rate was referenced to GB / T 50082-2009 "Ordinary Concrete Long-term Performance and Durability Test Method Standard", and the results are shown in Table 2:

[0084] Table 2 Performance test of recycled sand powder concrete

[0085]

[0086] It can be seen from Table 2 that the recycled sand powder concrete prepared in Example 1 has a higher crack resistance grade, and both strength and shrinkage resistance are more excellent, indicating that it has better performance than conventional alkali-activated concrete.

[0087] In the description of this specification, the description with reference to the terms "one embodiment", "some embodiments", "example", "specific example", or "some examples" etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms should not be understood as necessarily being directed to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described may be combined in any one or more embodiments or examples in a suitable manner. In addition, those skilled in the art may combine and combine different embodiments or examples described in this specification.

[0088] Although the embodiments of the present invention have been shown and described above, it is to be understood that the above embodiments are exemplary and are not to be construed as limitations of the present invention. A person skilled in the art may change, modify, replace and vary the above embodiments within the scope of the present invention.

Claims

1. A method for preparing recycled sand powder concrete from construction solid waste, characterized in that: The following steps are involved: Step 1, collecting construction solid waste materials and crushing them to obtain solid waste sand powder; Step 2, subjecting the solid waste sand powder to alkali excitation treatment under the action of an alkali exciter to obtain regenerated sand powder; Step 3, mixing the regenerated sand powder with cement, aggregate, fly ash, water reducing agent and water, and then stirring evenly to form a mixed slurry; Step 4, pour the mixed slurry into a mold, knock to remove bubbles, let it stand for 2-3 days, then remove the mold, and cure for 7-14 days to obtain recycled sand powder concrete; The alkaline activator in step 2 is a sodium silicate & zinc aluminum tartrate composite solution, and the preparation process is as follows: (1) Weigh tartaric acid and deionized water, mix them, add a silane coupling agent, and stir them thoroughly to obtain a tartaric acid solution; (2) Mixing zinc chloride and aluminum chloride into deionized water, and mixing and stirring thoroughly to obtain a zinc-aluminum mixed solution; (3) Mix the tartaric acid solution and the zinc-aluminum mixed solution, raise the temperature to 110-120°C, react for 2-3 hours, then cool to 40-50°C, collect the filtrate by filtration, adjust the pH of the reaction solution to 7.0-8.0, and dry to obtain zinc-aluminum tartrate; (4) Mixing sodium silicate and deionized water, adding zinc aluminum tartrate, and fully dispersing them to form an alkaline activator; Wherein, in step (1), the mass ratio of tartaric acid, silane coupling agent and deionized water is 1.5-3:0.2-0.4:20-30; in the zinc-aluminum mixed solution of step (2), the mass ratio of zinc chloride, aluminum chloride and deionized water is 1.36-2.72:0.67-1.33:20-40; in step (3), the mass ratio of tartaric acid solution and zinc-aluminum mixed solution is 1.5-2:1; in step (4), the mass ratio of sodium silicate, zinc aluminum tartrate and deionized water is 1.8-3.6:0.2-0.8:

10.

2. The method for preparing construction solid waste recycled sand powder concrete according to claim 1, characterized in that: The solid waste sand powder obtained in step 1 has a median particle size of 27.6 μm, a content of particles with a particle size less than 75 μm of 83.74%, a content of particles with a particle size less than 40 μm of 57.52%, and a content of particles with a particle size less than 10 μm of 23.25%.

3. The method for preparing construction solid waste recycled sand powder concrete according to claim 1, characterized in that: In step 2, the process of treating the solid waste sand powder with an alkali activator includes: mixing the solid waste sand powder and the alkali activator in a mixer, stirring at a speed of 100-200 r / min for 15-30 minutes, and then drying in an oven to obtain regenerated sand powder.

4. The method for preparing construction solid waste recycled sand powder concrete according to claim 1, characterized in that: In step (1), the tartaric acid is DL-tartaric acid, and the silane coupling agent is one of KH-550, KH-560, and KH-570.

5. The method for preparing construction solid waste recycled sand powder concrete according to claim 1, characterized in that: In step 3, the mass ratio of cement, aggregate, regenerated sand powder, fly ash, water reducing agent and water is 100-150:278-426:29-58:30-50:3-8:180-260.

6. The method for preparing construction solid waste recycled sand powder concrete according to claim 5, characterized in that: In step 3, the aggregate includes coarse aggregate and fine aggregate, the coarse aggregate is stone with a particle size of 4.75-9.5 mm, the fine aggregate is gravel with a particle size less than 4.75 mm, and the mass ratio of the coarse aggregate to the fine aggregate is 1.5-1.8:

1.

7. The method for preparing construction solid waste recycled sand powder concrete according to claim 6, characterized in that: In the step 3, the cement is ordinary silicate cement PO42.5, the fly ash model is grade I, and the water reducer is naphthalene-based high-efficiency water reducer SY-05.

8. The method for preparing construction solid waste recycled sand powder concrete according to claim 1, characterized in that: In step 4, the maintenance is performed by covering with a plastic film with a thickness of 0.1 mm, avoiding direct sunlight, and spraying water to replenish moisture.

9. A construction solid waste recycled sand powder concrete, characterized in that: The method according to claim 1 is used to prepare the product.