Ferroalloy slag-based filling material for iron ore and preparation method thereof

By preparing ferroalloy slag-based filling materials and utilizing solid wastes such as ferroalloy slag and water-quenched blast furnace granulated slag, the problem of ferroalloy slag storage is solved, the cost of mine filling is reduced, and the mechanical properties and environmental protection of the filling materials are improved, achieving Collaborative utilization and environmental protection of various solid wastes.

CN117865626BActive Publication Date: 2024-10-01TANGSHAN COLLEGE
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410089914.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-01-23
Publication Date
2024-10-01
Estimated Expiration
2044-01-23

AI Technical Summary

Technical Problem

The large-scale utilization of ferroalloy slag has not yet been realized, resulting in a large amount of land resources occupied and damage to the ecological environment. The cost of existing mine filling materials is high and it is difficult to realize the coordinated utilization of various industrial solid wastes.

Method used

Ferroalloy slag-based filling material is used. The cementitious material part is composed of industrial solid waste such as low-carbon ferrochromium slag, ferronickel slag, water-quenched blast furnace granulated slag, soda ash white mud and modified desulfurization ash. It is quenched by water, crushed and ground. And mixed preparation, combined with iron tailings to form cementitious materials, reducing production costs and improving the compactness and environmental protection of filling materials.

Benefits of technology

It realizes the resource utilization of ferroalloy slag, reduces filling costs, improves the mechanical properties and environmental protection of filling materials, reduces the impact of solid waste storage on the environment, and has significant social and environmental benefits.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The present invention discloses a ferroalloy slag-based filling material for iron ore and a preparation method thereof, wherein the cementitious material part is respectively composed of 25% to 50% low-carbon ferrochrome slag, 10% to 15% ferronickel slag from blast furnace, 5% to 10% high-carbon ferrochrome slag, 15% to 30% water-quenched blast furnace granulated slag, 5% to 10% soda ash white mud, and 6% to 12% modified desulfurized ash in percentage by mass; the aggregate is iron tailings. The ferroalloy slag-based filling material provided by the present invention can solve the environmental problems and waste of land resources caused by the large-scale storage of various industrial solid wastes by organically combining ferroalloy smelting waste slag, chemical solid waste and iron tailings that are difficult to use alone to prepare filling materials for iron ore mining. At the same time, the prepared filling material has low production cost and stable mechanical properties, can effectively improve the recovery rate of iron ore, has significant economic and environmental benefits, and has broad market prospects.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of mine filling material preparation technology and comprehensive utilization of solid waste, and in particular to a ferroalloy slag-based filling material for iron ore and a preparation method thereof. Background Art

[0002] Ferroalloy slag includes ferrochrome slag, ferronickel slag, silicon-manganese slag and many other types. Large-scale storage occupies land resources and causes damage to the ecological environment. At present, my country's utilization of ferroalloy slag is mainly concentrated on a single type, which is difficult to achieve large-scale utilization. Ferrochrome slag is a gray-black metallurgical slag emitted when smelting carbon ferrochrome alloy. It is a metallurgical waste slag formed after chromite is reduced at 1700°C in a blast furnace with carbon as a reducing agent. Ferronickel slag is a light green metallurgical waste slag produced after humus-type laterite ore is reduced and smelted with nickel iron in an electric furnace or blast furnace.

[0003] Mine filling material is a kind of backfill material for mine goaf made of cementitious materials, tailings and water, which can improve resource utilization and achieve safe, efficient and green mining. At present, most mines use cement-based or slag-based cementitious materials, and the cost of mine filling remains high.

[0004] At present, various types of ferroalloy slag are mainly disposed of by landfill, and only a very small amount is used in cement mixed materials. There is still a blank in the preparation of cementitious materials based on the coupling of various types of ferroalloy slag and chemical slag for use in mine filling. Therefore, the ferroalloy slag-based filling material for iron ore proposed in the present invention has a simple process and low cost, and can also achieve the coordinated utilization of various industrial solid wastes, and has good social and environmental benefits. Summary of the invention

[0005] The object of the present invention is to provide a ferroalloy slag-based filling material for iron ore and a preparation method thereof, so as to reduce the cost of iron ore mining and filling, realize the resource utilization of various solid wastes, and reduce the impact of large-scale storage of ferroalloy slag on the environment.

[0006] To achieve the above object, the present invention is implemented by adopting the following technical solutions:

[0007] A ferroalloy slag-based filling material for iron ore, wherein the cementitious material part comprises, by mass percentage, 25%-50% of low-carbon ferrochrome slag, 10%-15% of blast furnace ferronickel slag, 5%-10% of high-carbon ferrochrome slag, 15%-30% of water-quenched blast furnace granulated slag, 5%-10% of soda ash white mud, 6%-12% of modified desulfurized ash, and the aggregate is iron tailings. The cementitious material and the iron tailings are mixed in a mass ratio of 1:4-1:8.

[0008] Furthermore, the CaO and SiO in the low-carbon ferrochrome slag 2 Mass percentage ≥70%, Cr 2 O3 ≤3%.

[0009] Furthermore, the mass percentage of the main chemical components of the blast furnace nickel-iron slag meets the following requirements: SiO 2 ≥30%,Al 2 O 3 ≥18%, CaO≥26%, Cr 2 O 3 ≤3%.

[0010] Furthermore, the mass percentage of the main chemical components of the soda ash mud meets the following requirements: CaCl 2 ≥15%, CaSO 4 ≥10%, moisture content<5%.

[0011] Furthermore, the modified desulfurization ash is a semi-dry desulfurization ash with the addition of catalyst Fe 2 O 3 The catalyst was baked at 110℃, and the amount of the catalyst added was 2% of the total mass, CaSO 3 The conversion rate is greater than 2.5%.

[0012] Furthermore, the water-quenched blast furnace granulated slag is granulated blast furnace slag powder that complies with GB / T18046-2008 "Granulated blast furnace slag powder for cement and concrete".

[0013] A method for preparing a ferroalloy slag-based filling material for iron ore, comprising the above-mentioned ferroalloy slag-based filling material for iron ore, and the specific steps are as follows:

[0014] Step S1. The ferroalloy slag is subjected to primary and secondary water quenching through a water quenching system, and a slag flushing treatment is performed on the typical ferroalloy slag on the slag flushing tank.

[0015] Step S2. The ferroalloy slag obtained after water quenching in step S1 is placed in a cone crusher for crushing, so that the particle size of the crushed metallurgical slag particles is less than 2.5 mm, and is placed in a jig for screening;

[0016] Step S3. Weigh 25%-50% of low-carbon ferrochrome slag, 10%-15% of blast furnace ferronickel slag, 5%-10% of high-carbon ferrochrome slag, 15%-30% of water-quenched blast furnace granulated slag, 5%-10% of soda ash mud, and 6%-12% of modified desulfurization ash, respectively, and grind them into powder to obtain low-carbon ferrochrome slag powder, high-carbon ferrochrome slag powder, blast furnace ferronickel slag powder, water-quenched blast furnace granulated slag powder, soda ash mud powder, and modified desulfurization ash powder, and mix them to obtain a cementitious material.

[0017] Step S4. The cementitious material obtained in step S3 is mixed evenly with iron tailings in a mass ratio of 1:4 to 1:8 to obtain a ferroalloy slag-based filling material for iron ore.

[0018] Furthermore, the particle size of the ferroalloy slag crushed in step S2 is less than 3 mm, and then grinding is performed, which can effectively reduce the grinding energy consumption and improve the grinding fineness.

[0019] Furthermore, the specific surface areas of the low-carbon ferrochrome slag powder, blast furnace ferronickel slag powder, and high-carbon ferrochrome slag powder in step S3 are all ≥430 m 2 / kg, the specific surface area of ​​water-quenched blast furnace granulated slag powder is ≥520m 2 / kg, the mud content of the iron tailings in step S4 is less than 8%.

[0020] The beneficial effects of the present invention are as follows:

[0021] 1. The raw materials used in the ferroalloy slag-based filling material for iron ore provided by the present invention are mainly metallurgical and chemical solid wastes such as ferroalloy slag, soda ash white mud and modified desulfurization ash. Its production cost is lower than that of cement-based materials or slag-based cementitious materials, and it can also solve the environmental problems caused by the large-scale storage of such industrial solid wastes.

[0022] 2. The present invention utilizes the main chemical components of low-carbon ferrochrome slag, CaO and SiO 2 The main mineral components are dicalcium silicate and a small amount of calcite, which are similar to the mineral composition of cement clinker. The main mineral components of blast furnace nickel-iron slag are also dicalcium silicate and magnesium-aluminum spinel, which are highly active mineral components. The blast furnace water-quenched granulated slag provides high-quality silicon and aluminum components for the gelling system. Under the synergistic stimulation of soda ash white mud and modified desulfurization ash, several solid wastes are organically coupled to ensure the formation of stable CSH gel, CASH gel and AFt in the gelling system. There are more types of complex salt minerals in the hydration product, making the hydration product particles smaller and combining with the active SiO 2 A reaction occurs, thereby increasing the density of the interface reaction transition zone and making the bonding network structure inside the filling material denser.

[0023] 3. The ferroalloy slag-based filling material for iron ore of the present invention uses cementitious materials that are all industrial solid waste, which are more low-carbon and environmentally friendly than cement-based materials; the aggregate used is tailings sand, which not only solves the problem of land resource waste caused by tailings storage, but also reduces the risk of surface subsidence in the goaf. DETAILED DESCRIPTION

[0024] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and understandable, the specific embodiments of the present invention are described in detail. In the following description, many specific details are set forth to facilitate a full understanding of the present invention. However, the present invention can be implemented in many other ways different from those described herein, and those skilled in the art can make similar improvements without violating the connotation of the present invention, so the present invention is not limited by the specific implementation disclosed below.

[0025] A ferroalloy slag-based filling material for iron ore, wherein the cementitious material part is respectively composed of 25% to 50% low-carbon ferrochrome slag, 10% to 15% ferronickel slag from blast furnace, 5% to 10% high-carbon ferrochrome slag, 15% to 30% water-quenched blast furnace granulated slag, 5% to 10% soda ash white mud, and 6% to 12% modified desulfurized ash, wherein the aggregate is iron tailings, and the obtained cementitious material and the iron tailings are mixed uniformly in a mass ratio of (1:4) to (1:8) to obtain the ferroalloy slag-based filling material for iron ore. Among them, CaO and SiO in the low-carbon ferrochrome slag are 2 Mass percentage ≥70%, Cr 2 O 3 ≤3%, the mass percentage of the main chemical components of blast furnace nickel-iron slag meets the following requirements: SiO 2 ≥30%,Al 2 O 3 ≥18%, CaO≥26%, Cr 2 O 3 ≤3%, the mass percentage of the main chemical components of soda ash mud meets the following requirements: CaCl 2 ≥15%, CaSO 4 ≥10%, moisture content <5%, water-quenched blast furnace granulated slag is granulated blast furnace slag powder that conforms to GB / T18046-2008 "Granulated blast furnace slag powder for cement and concrete". Embodiment 1:

[0026] The method for preparing a ferroalloy slag-based filling material for iron ore in the present invention comprises the following specific steps:

[0027] Step S1. The ferroalloy slag is subjected to primary and secondary water quenching through a water quenching system, and a slag flushing treatment is performed on the typical ferroalloy slag on the slag flushing tank.

[0028] Step S2. The ferroalloy slag obtained after water quenching is placed in a cone crusher for crushing so that the particle size of the crushed metallurgical slag particles is less than 2.5 mm, and is placed in a jig for screening;

[0029] Step S3. Weigh 50% of low-carbon ferrochrome slag, 10% of blast furnace ferronickel slag, 10% of high-carbon ferrochrome slag, 15% of water-quenched blast furnace granulated slag, 5% of soda ash mud, and 10% of modified desulfurization ash, and grind them into powder to obtain low-carbon ferrochrome slag powder, high-carbon ferrochrome slag powder, blast furnace ferronickel slag powder, water-quenched blast furnace granulated slag powder, soda ash mud powder, and modified desulfurization ash powder, and mix them to obtain a cementitious material.

[0030] Step S4. The cementitious material obtained in step S3 is mixed evenly with iron tailings in a mass ratio of 1:4 to obtain a ferroalloy slag-based filling material for iron ore. Embodiment 2:

[0031] The method for preparing a ferroalloy slag-based filling material for iron ore in the present invention comprises the following specific steps:

[0032] Step S1. The ferroalloy slag is subjected to primary and secondary water quenching through a water quenching system, and a slag flushing treatment is performed on the typical ferroalloy slag on the slag flushing tank.

[0033] Step S2. The ferroalloy slag obtained after water quenching is placed in a cone crusher for crushing so that the particle size of the crushed metallurgical slag particles is less than 2.5 mm, and is placed in a jig for screening;

[0034] Step S3. Weigh 45% of low-carbon ferrochrome slag, 10% of blast furnace ferronickel slag, 10% of high-carbon ferrochrome slag, 20% of water-quenched blast furnace granulated slag, 5% of soda ash mud, and 10% of modified desulfurization ash, respectively, and grind them into powder to obtain low-carbon ferrochrome slag powder, high-carbon ferrochrome slag powder, blast furnace ferronickel slag powder, water-quenched blast furnace granulated slag powder, soda ash mud powder, and modified desulfurization ash powder, and mix them to obtain a cementitious material.

[0035] Step S4. The cementitious material obtained in step S3 is mixed evenly with iron tailings in a mass ratio of 1:4 to obtain a ferroalloy slag-based filling material for iron ore. Embodiment 3:

[0036] The method for preparing a ferroalloy slag-based filling material for iron ore in the present invention comprises the following specific steps:

[0037] Step S1. The ferroalloy slag is subjected to primary and secondary water quenching through a water quenching system, and a slag flushing treatment is performed on the typical ferroalloy slag on the slag flushing tank.

[0038] Step S2. The ferroalloy slag obtained after water quenching is placed in a cone crusher for crushing so that the particle size of the crushed metallurgical slag particles is less than 2.5 mm, and is placed in a jig for screening;

[0039] Step S3. Weigh 40% of low-carbon ferrochrome slag, 15% of blast furnace ferronickel slag, 10% of high-carbon ferrochrome slag, 20% of water-quenched blast furnace granulated slag, 5% of soda ash mud, and 10% of modified desulfurization ash, respectively, and grind them into powder to obtain low-carbon ferrochrome slag powder, high-carbon ferrochrome slag powder, blast furnace ferronickel slag powder, water-quenched blast furnace granulated slag powder, soda ash mud powder, and modified desulfurization ash powder, and mix them to obtain a cementitious material.

[0040] Step S4. The cementitious material obtained in step S3 is mixed evenly with iron tailings in a mass ratio of 1:4 to obtain a ferroalloy slag-based filling material for iron ore. Embodiment 4:

[0041] The method for preparing a ferroalloy slag-based filling material for iron ore in the present invention comprises the following specific steps:

[0042] Step S1. The ferroalloy slag is subjected to primary and secondary water quenching through a water quenching system, and a slag flushing treatment is performed on the typical ferroalloy slag on the slag flushing tank.

[0043] Step S2. The ferroalloy slag obtained after water quenching is placed in a cone crusher for crushing so that the particle size of the crushed metallurgical slag particles is less than 2.5 mm, and is placed in a jig for screening;

[0044] Step S3. Weigh 35% of low-carbon ferrochrome slag, 15% of blast furnace ferronickel slag, 10% of high-carbon ferrochrome slag, 25% of water-quenched blast furnace granulated slag, 5% of soda ash mud, and 10% of modified desulfurization ash, respectively, and grind them into powder to obtain low-carbon ferrochrome slag powder, high-carbon ferrochrome slag powder, blast furnace ferronickel slag powder, water-quenched blast furnace granulated slag powder, soda ash mud powder, and modified desulfurization ash powder, and mix them to obtain a cementitious material.

[0045] Step S4. The cementitious material obtained in step S3 is mixed evenly with iron tailings in a mass ratio of 1:4 to obtain a ferroalloy slag-based filling material for iron ore. Embodiment 5:

[0046] The method for preparing a ferroalloy slag-based filling material for iron ore in the present invention comprises the following specific steps:

[0047] Step S1. The ferroalloy slag is subjected to primary and secondary water quenching through a water quenching system, and a slag flushing treatment is performed on the typical ferroalloy slag on the slag flushing tank.

[0048] Step S2. The ferroalloy slag obtained after water quenching is placed in a cone crusher for crushing so that the particle size of the crushed metallurgical slag particles is less than 2.5 mm, and is placed in a jig for screening;

[0049] Step S3. Weigh 30% of low-carbon ferrochrome slag, 15% of blast furnace ferronickel slag, 10% of high-carbon ferrochrome slag, 25% of water-quenched blast furnace granulated slag, 8% of soda ash mud, and 12% of modified desulfurization ash, respectively, and grind them into powder to obtain low-carbon ferrochrome slag powder, high-carbon ferrochrome slag powder, blast furnace ferronickel slag powder, water-quenched blast furnace granulated slag powder, soda ash mud powder, and modified desulfurization ash powder, and mix them to obtain a cementitious material.

[0050] Step S4. The cementitious material obtained in step S3 is mixed evenly with iron tailings in a mass ratio of 1:4 to obtain a ferroalloy slag-based filling material for iron ore. Embodiment 6:

[0051] The method for preparing a ferroalloy slag-based filling material for iron ore in the present invention comprises the following specific steps:

[0052] Step S1. The ferroalloy slag is subjected to primary and secondary water quenching through a water quenching system, and a slag flushing treatment is performed on the typical ferroalloy slag on the slag flushing tank.

[0053] Step S2. The ferroalloy slag obtained after water quenching is placed in a cone crusher for crushing so that the particle size of the crushed metallurgical slag particles is less than 2.5 mm, and is placed in a jig for screening;

[0054] Step S3. Weigh 30% of low-carbon ferrochrome slag, 10% of blast furnace ferronickel slag, 10% of high-carbon ferrochrome slag, 30% of water-quenched blast furnace granulated slag, 8% of soda ash mud, and 12% of modified desulfurization ash, respectively, and grind them into powder to obtain low-carbon ferrochrome slag powder, high-carbon ferrochrome slag powder, blast furnace ferronickel slag powder, water-quenched blast furnace granulated slag powder, soda ash mud powder, and modified desulfurization ash powder, and mix them to obtain a cementitious material.

[0055] Step S4. The cementitious material obtained in step S3 is mixed evenly with iron tailings in a mass ratio of 1:4 to obtain a ferroalloy slag-based filling material for iron ore.

[0056] Experimental comparison demonstration

[0057] The ferroalloy slag-based filling material for iron ore obtained in Examples 1-6 was mixed with water in a mass ratio of 3:7 to obtain a filling material that meets the needs of filling mining.

[0058] Comparative Example 1

[0059] A cement-based filling material is selected, and the cementitious material of the filling material is composed of the following raw materials by mass fraction: 40% fly ash, 35% slag powder, and 25% cement, wherein the fly ash is Grade I ash in accordance with GB / T1596-2017 "Fly ash used in cement and concrete", and the slag powder is Grade S95 with a specific surface area of ​​420 m 2 / kg, the aggregate is iron tailings.

[0060] The cement-based filling material and water are prepared in a mass ratio of 3:7 to obtain a filling material that meets the needs of filling mining.

[0061] Comparative Example 2

[0062] The cementitious material obtained in step S3 of Example 6 was mixed evenly with iron tailings in a mass ratio of 1:5 to obtain a ferroalloy slag-based filling material for iron ore, and the filling material and water were prepared in a mass ratio of 3:7 to obtain a filling material that meets the needs of filling mining.

[0063] Comparative Example 3

[0064] The cementitious material obtained in step S3 of Example 6 was mixed evenly with iron tailings in a mass ratio of 1:6 to obtain a ferroalloy slag-based filling material for iron ore, and the filling material and water were prepared in a mass ratio of 3:7 to obtain a filling material that meets the needs of filling mining.

[0065] Comparative Example 4

[0066] The cementitious material obtained in step S3 of Example 6 was mixed evenly with iron tailings in a mass ratio of 1:7 to obtain a ferroalloy slag-based filling material for iron ore, and the filling material and water were prepared in a mass ratio of 3:7 to obtain a filling material that meets the needs of filling mining.

[0067] Comparative Example 5

[0068] The cementitious material obtained in step S3 of Example 6 was mixed evenly with iron tailings in a mass ratio of 1:8 to obtain a ferroalloy slag-based filling material for iron ore, and the filling material and water were prepared in a mass ratio of 3:7 to obtain a filling material that meets the needs of filling mining.

[0069] The raw materials in Examples 1-6 and Comparative Examples 1-5 were placed in a fully automatic mortar mixer and stirred evenly, and injected into a 70mm×70mm×70mm mold at a temperature of 20±5°C and a relative humidity of not less than 60%, and their relevant properties were tested; the prepared test blocks were placed under standard curing conditions of a curing temperature of 20°C±2°C and a relative humidity of not less than 95%, and then continued to be placed in a constant temperature and humidity curing box at a curing temperature of 20°C±2°C and a relative humidity of not less than 95% for curing to 7d and 28d, and the compressive strength of the test blocks was tested. The above test results are shown in Table 1:

[0070] Table 1

[0071] serial number Mortar-sand ratio Mass concentration / % Fluidity / mm Water seepage rate / % 7d compressive strength / MPa 28d compressive strength / MPa Example 1 1:4 70 245 17.2 3.22 5.65 Example 2 1:4 70 245 16.8 3.36 5.73 Example 3 1:4 70 255 16.3 3.39 5.67 Example 4 1:4 70 260 15.7 3.55 5.88 Example 5 1:4 70 265 14.2 3.71 6.13 Example 6 1:4 70 265 13.5 4.25 6.67 Comparative Example 1 1:4 70 260 26.6 3.63 4.96 Comparative Example 2 1:5 70 260 15.6 3.06 5.66 Comparative Example 3 1:6 70 265 18.3 2.87 4.93 Comparative Example 4 1:7 70 260 20.2 2.66 4.39 Comparative Example 5 1:8 70 270 23.7 2.03 3.87

[0072] As can be seen from Table 1, the working performance and mechanical properties of the ferroalloy slag-based filling material for iron ore of the present invention are significantly improved compared with cement-based filling materials, and its specific addition amount can be adjusted according to the design parameters of filling mining. The above specific embodiments are only preferred, but not limiting to the implementation methods.

[0073] In summary: the ferroalloy slag-based filling material for iron ore provided by the present invention can replace cement-based filling materials, play a role in reducing carbon emissions, and at the same time can improve the mechanical properties of the filling body to ensure the safety of filling and mining work. The advantage of ferroalloy slag-based filling materials over other types of filling materials sold on the market is that the raw material cost is lower and the mechanical properties of the filling body are better. At the same time, relying on the utilization method of the made filling material to achieve its large-scale resource utilization, it can solve the environmental impact brought about by the storage of such solid wastes, and has more obvious social and environmental benefits.

[0074] The basic principles and main features of the present invention and the advantages of the present invention are shown and described above. For those skilled in the art, it is obvious that the present invention is not limited to the details of the above exemplary embodiments, and the present invention can be implemented in other specific forms without departing from the spirit or basic features of the present invention; therefore, no matter from which point of view, the embodiments should be regarded as exemplary and non-restrictive. The scope of the present invention is limited by the appended claims rather than the above description, and it is intended that all changes within the meaning and scope of the equivalent elements of the claims are included in the present invention.

Claims

1. A ferroalloy slag-based filling material for iron ore, characterized in that: The cementitious materials are as follows in percentage by mass: 25% to 50% low-carbon ferrochrome slag, 10% to 15% ferronickel slag from blast furnace, 5% to 10% high-carbon ferrochrome slag, 15% to 30% water-quenched blast furnace granulated slag, 5% to 10% soda ash mud, 6% to 12% modified desulfurized ash, and the aggregate is iron tailings. The cementitious materials and iron tailings are mixed in a mass ratio of 1:4 to 1:

8. The modified desulfurization ash is obtained by adding catalyst Fe2O3 to semi-dry desulfurization ash and baking it at a low temperature of 110°C, wherein the amount of catalyst added is 2% of the total mass, and the conversion rate of CaSO3 is greater than 2.5%.

2. The ferroalloy slag-based filling material for iron ore according to claim 1, characterized in that: The mass percentage of CaO and SiO2 in the low-carbon ferrochrome slag is ≥70%, and the mass percentage of Cr2O3 is ≤3%.

3. The ferroalloy slag-based filling material for iron ore according to claim 1, characterized in that: The mass percentages of the main chemical components of the blast furnace nickel-iron slag meet the following requirements: SiO2≥30%, Al2O3≥18%, CaO≥26%, and Cr2O3≤3%.

4. The ferroalloy slag-based filling material for iron ore according to claim 1, characterized in that: The mass percentages of the main chemical components of the soda ash mud meet the following requirements: CaCl2≥15%, CaSO4≥10%, and water content<5%.

5. A method for preparing the ferroalloy slag-based filling material for iron ore according to any one of claims 1 to 4, characterized in that: The specific steps are as follows: Step S1, subjecting the ferroalloy slag to primary and secondary water quenching through a water quenching system, and subjecting the typical ferroalloy slag on the slag flushing tank to slag flushing treatment; Step S2, placing the ferroalloy slag obtained after water quenching in step S1 into a cone crusher for crushing, so that the particle size of the crushed metallurgical slag particles is less than 2.5 mm, and placing it into a jig for screening; Step S3, respectively weighing 25%-50% of low-carbon ferrochrome slag, 10%-15% of blast furnace ferronickel slag, 5%-10% of high-carbon ferrochrome slag, 15%-30% of water-quenched blast furnace granulated slag, 5%-10% of soda ash white mud, and 6%-12% of modified desulfurization ash, and grinding them into powders to obtain low-carbon ferrochrome slag powder, high-carbon ferrochrome slag powder, blast furnace ferronickel slag powder, water-quenched blast furnace granulated slag powder, soda ash white mud powder, and modified desulfurization ash powder, and mixing them to obtain a cementitious material; Step S4, uniformly mixing the cementitious material obtained in step S3 with iron tailings in a mass ratio of 1:4 to 1:8 to obtain a ferroalloy slag-based filling material for iron ore.

6. The method for preparing a ferroalloy slag-based filling material for iron ore according to claim 5, characterized in that: The ferroalloy slag crushed in step S2 has a particle size of less than 3 mm and is then ground.

7. The method for preparing a ferroalloy slag-based filling material for iron ore according to claim 5, characterized in that: The specific surface areas of the low-carbon ferrochrome slag powder, blast furnace ferronickel slag powder and high-carbon ferrochrome slag powder in step S3 are all ≥430m 2 / kg, the specific surface area of ​​water-quenched blast furnace granulated slag powder is ≥520m 2 / kg, the mud content of the iron tailings in step S4 is less than 8%.