Control method of edge crack of hot rolled plate and hot rolled steel coil

By using technical means such as forward and reverse electromagnetic stirring, heating treatment and edge heating during continuous casting and hot rolling of silicon steel, the problem of edge crack defects in the hot rolling process of silicon steel is solved, and the edge portion of hot rolled steel coil is realized Improve quality and material yield.

CN117900266BActive Publication Date: 2024-12-06HUNAN VALIN LIANYUAN IRON & STEEL CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202410060055.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-01-15
Publication Date
2024-12-06
Estimated Expiration
2044-01-15

AI Technical Summary

Technical Problem

Silicon steel is prone to edge crack defects during hot rolling, and the prior art is difficult to reduce edge cracking problems of hot rolled steel coils from the source.

Method used

During the continuous casting process, the continuous casting blank is heated and rolled equally, and the intermediate blank is heated before finishing rolling to control rolling parameters such as temperature, current, Frequency and heating rate to reduce columnar crystal ratio and grain size, and improve the edge quality of continuous cast billets and hot-rolled steel coils.

Benefits of technology

By reducing the columnar crystal ratio and grain size and uniform deformation, the edge cracking problems of continuous casting billets and hot-rolled steel coils are significantly reduced, and the material yield and production efficiency are improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117900266B_ABST
    Figure CN117900266B_ABST
Patent Text Reader

Abstract

The present application discloses a control method for edge cracks of hot-rolled plates and hot-rolled steel coils. The method comprises: continuous casting, continuously casting molten steel to obtain continuous casting billets, electromagnetically stirring the molten steel in a crystallizer, the electromagnetic stirring adopts a forward and reverse alternating stirring mode, the forward and reverse alternating time is 15‑25s, the current of the electromagnetic stirring is 260‑360A, and the frequency of the electromagnetic stirring is 8‑15Hz; heating treatment, heating the continuous casting billets in a heating furnace to obtain heated continuous casting billets; rolling, rolling the heated continuous casting billets in an equal-width rolling manner, wherein rolling includes rough rolling and finish rolling, and the edge of the intermediate billet is heated before finish rolling. The control method of the present application can improve the quality of the continuous casting billets and the edge quality of the hot-rolled steel coils, and reduce the edge cracks of the hot-rolled steel coils from the source.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of steel smelting, and in particular to a method for controlling edge cracks of hot-rolled plates and a hot-rolled steel coil. Background Art

[0002] Silicon steel is widely used in the manufacture of transformer cores and is an important functional soft magnetic material. The silicon element is very sensitive to the magnetic properties of silicon steel. As the silicon content in the steel increases, the resistivity increases, the eddy current loss decreases, and the iron loss also decreases. However, as the silicon content increases, the brittleness of the steel increases, and edge cracks are very likely to occur during the hot rolling process. Optimizing the rolling process cannot reduce the problem of edge cracks in hot-rolled steel coils from the source. Summary of the invention

[0003] The embodiments of the present application provide a method for controlling edge cracks of hot-rolled plates and a hot-rolled steel coil, which can improve the quality of continuous casting ingots and improve the edge quality of hot-rolled steel coils, thereby reducing the edge crack problem of hot-rolled steel coils from the source.

[0004] In the first aspect, an embodiment of the present application proposes a method for controlling edge cracks of a hot-rolled plate, the control method comprising: continuous casting, continuously casting molten steel to obtain a continuously cast billet, and electromagnetically stirring the molten steel in a crystallizer, wherein the electromagnetic stirring adopts a forward and reverse alternating stirring mode, the forward and reverse alternating time is 15-25s, the electromagnetic stirring current is 260-360A, and the electromagnetic stirring frequency is 8-15Hz; heating treatment, heating the continuously cast billet in a heating furnace to obtain a heated continuously cast billet; rolling, rolling the heated continuously cast billet by equal-width rolling, wherein rolling includes rough rolling and finish rolling, and the edge of the intermediate billet is heated before finish rolling.

[0005] According to one aspect of an embodiment of the present application, in the rolling step, the edge heating area is 8-15 mm of the edge of the intermediate billet; the heating temperature of the edge heating is 90-120°C.

[0006] According to one aspect of an embodiment of the present application, in the step of heating treatment, the heating treatment includes a preheating section, a first heating section and a second heating section; the initial temperature of the continuous casting billet is 600-750°C, the temperature of the preheating section is 600-750°C, the temperature of the first heating section is 750-900°C, the temperature of the second heating section is 900-1150°C, and the heating rate of the heating treatment is ≤6.5°C / min.

[0007] According to one aspect of an embodiment of the present application, in the rolling step, the width reduction of the continuous casting billet is ≤5 mm.

[0008] According to one aspect of the embodiment of the present application, the temperature of rough rolling is 1050-1150°C, and the temperature of finish rolling is 900-1000°C.

[0009] According to one aspect of an embodiment of the present application, in the rolling step, the reduction amount of a single pass of rough rolling is 15-35 mm; the number of rolling passes of the rough rolling is 5 or 7 passes.

[0010] According to one aspect of the embodiment of the present application, in the continuous casting step, the columnar crystal thickness in the triangular region of the continuous casting billet is less than 30 mm.

[0011] According to one aspect of an embodiment of the present application, the control method also includes laminar cooling and coiling after rolling.

[0012] In a second aspect, an embodiment of the present application provides a hot-rolled steel coil, which is prepared by the control method of the first aspect of the present application.

[0013] According to another aspect of the embodiment of the present application, the thickness of the hot-rolled steel coil is 2-3.5 mm; the edge crack ratio of the hot-rolled steel coil is ≤0.1%, and the edge shearing ratio of the hot-rolled steel coil is ≤10%.

[0014] The embodiments of the present application reduce the proportion of columnar crystals in the continuous casting billet by performing electromagnetic stirring on the molten steel in a crystallizer in alternating forward and reverse directions, controlling the time of the alternating forward and reverse directions within the range of 15-25s, the current of the electromagnetic stirring within the range of 260-360A, and controlling the frequency of the electromagnetic stirring within the range of 8-15Hz. During the rolling process of the continuous casting billet, the grain size is reduced, the deformation of the continuous casting billet is made more uniform, and the probability of the continuous casting billet generating holes is reduced. The continuous casting billet is heated and rolled in an equal-width rolling manner, and the edge of the intermediate billet is heated before finish rolling, thereby improving the quality of the continuous casting billet and the edge quality of the hot-rolled steel coil, thereby reducing the edge cracking of the hot-rolled steel coil from the source. BRIEF DESCRIPTION OF THE DRAWINGS

[0015] The features, advantages and technical effects of exemplary embodiments of the present application will be described below with reference to the accompanying drawings.

[0016] Figure 1 The iron-carbon phase diagram of Si and Fe alloys;

[0017] Figure 2 A schematic flow chart of a method for controlling edge cracks of hot-rolled plates provided in an embodiment of the present application;

[0018] Figure 3 This is a cross-sectional view of the edge structure of the ingot of Example 3;

[0019] Figure 4 This is a cross-sectional view of the edge structure of the ingot of Comparative Example 1;

[0020] Figure 5 This is a cross-sectional morphology diagram of the edge of the hot-rolled steel coil of Example 3;

[0021] Figure 6This is a cross-sectional morphology of the edge of the hot-rolled steel coil of Comparative Example 1;

[0022] Figure 7 This is the edge morphology of the hot-rolled steel coil of Example 3;

[0023] Figure 8 This is the edge morphology of the hot-rolled steel coil in comparative example 1. DETAILED DESCRIPTION

[0024] The features and exemplary embodiments of various aspects of the present application will be described in detail below. In the detailed description below, many specific details are proposed to provide a comprehensive understanding of the present application. However, it is obvious to those skilled in the art that the present application can be implemented without the need for some of these specific details. The following description of the embodiments is only to provide a better understanding of the present application by illustrating examples of the present application. In the accompanying drawings and the following description, at least some of the known structures and technologies are not shown to avoid unnecessary ambiguity in the present application; and, for clarity, the size of some structures may be exaggerated. In addition, the features, structures or characteristics described below may be combined in one or more embodiments in any suitable manner.

[0025] It should be noted that, in this application, the term "comprises" or any other variant thereof is intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also includes other elements not explicitly listed, or also includes elements inherent to such process, method, article or device. In the absence of further restrictions, the elements defined by the sentence "comprises..." do not exclude the existence of other identical elements in the process, method, article or device including the elements.

[0026] Unless otherwise specified, the values ​​of the parameters mentioned in this application can be measured by various measurement methods commonly used in the art (for example, they can be tested according to the methods given in the examples of this application). Unless otherwise specified, the test temperature of the parameters mentioned in this application is 25° C. and the test pressure is standard atmospheric pressure.

[0027] The temperature range of the austenite and ferrite phases of oriented silicon steel is 770-1220℃. Figure 1 The iron-carbon phase diagram of Si and Fe alloys with Si mass content of 3.25% is shown in Figure 1As shown in the figure, oriented silicon steel is rolled in the two-phase region during the entire hot rolling process. Due to the different resistance of austenite and ferrite to deformation, holes are easily generated at the interface between ferrite and austenite under the same rolling force. At the same time, since the sub-surface material at the edge of the strip is in the free expansion stage and the deformation is large, the probability of holes in these parts will also increase. However, due to the decarburization of the surface area of ​​the strip during the heating process, it is in the ferrite single-phase region during the entire hot rolling process, and the probability of holes is reduced. Therefore, the sub-surface of the edge of the strip is the area most likely to generate holes. When these areas expand freely during the slab rolling process, the holes will be enlarged and extended to the edge of the strip, thereby forming edge crack defects. If there is a serious edge crack on the edge of the entire steel coil, there is a risk of tearing the steel coil during the cold rolling process. Therefore, the entire steel coil must be trimmed before cold rolling, which will affect the yield rate and production efficiency of the strip.

[0028] In order to reduce the problem of edge cracks in hot-rolled steel coils, most of the measures adopted in related technologies are to optimize the hot rolling process, but no measures are taken to address the fundamental cause of edge cracks in oriented silicon steel hot-rolled coils.

[0029] Figure 2 A schematic flow chart of a method for controlling edge cracks of hot-rolled plates provided in an embodiment of the present application.

[0030] like Figure 2 As shown, the embodiment of the present application proposes a method for controlling edge cracks of hot-rolled plates. The control method comprises the following steps:

[0031] S10: continuous casting, continuously casting the molten steel to obtain a continuous casting billet, and electromagnetically stirring the molten steel in the crystallizer, wherein the electromagnetic stirring adopts a forward and reverse alternating stirring mode, the forward and reverse alternating time is 15-25s, the electromagnetic stirring current is 260-360A, and the electromagnetic stirring frequency is 8-15Hz;

[0032] S20: heating treatment, heating the continuous casting billet in a heating furnace to obtain a heated continuous casting billet;

[0033] S30: rolling, rolling the heated continuous casting billet by equal width rolling, wherein the rolling includes rough rolling and finish rolling, and the edge of the intermediate billet is heated before the finish rolling.

[0034] The embodiments of the present application reduce the proportion of columnar crystals in the continuous casting billet by performing electromagnetic stirring on the molten steel in a crystallizer in alternating forward and reverse directions, controlling the time of the alternating forward and reverse directions within the range of 15-25s, the current of the electromagnetic stirring within the range of 260-360A, and controlling the frequency of the electromagnetic stirring within the range of 8-15Hz. During the rolling process of the continuous casting billet, the grain size is reduced, the deformation of the continuous casting billet is made more uniform, and the probability of the continuous casting billet generating holes is reduced. The continuous casting billet is heated and rolled in an equal-width rolling manner, and the edge of the intermediate billet is heated before finish rolling, thereby improving the quality of the continuous casting billet and the edge quality of the hot-rolled steel coil, thereby reducing the edge cracking of the hot-rolled steel coil from the source.

[0035] The columnar crystals in the ingot are slender, with a length of 5-10mm, and the equiaxed crystals are equiaxed, with a size of 0.4-1.2mm. In addition, the specific surface area of ​​the equiaxed crystals is greater than that of the columnar crystals. The triangular area of ​​the continuous casting ingot of oriented silicon steel is almost entirely columnar crystals. The continuous casting ingot is in the two-phase region at 770-1220℃, that is, the continuous casting ingot is rolled in the two-phase region during the entire hot rolling process. Austenite and ferrite have different deformation resistances. Under the same rolling force, ferrite deforms more and austenite deforms less, and it is very easy to produce holes at the interface between the ferrite and austenite two-phase regions. During the continuous casting process, the molten steel is subjected to alternating electromagnetic stirring in forward and reverse directions, and the alternating time of forward and reverse directions is controlled within the range of 15-25s, the current of electromagnetic stirring is within the range of 260-360A, and the frequency of electromagnetic stirring is controlled within the range of 8-15Hz, which can rapidly reduce the number of columnar crystals, increase the number of equiaxed crystals, and increase the grain boundary area. Therefore, when the continuous casting billet is rolled in the two-phase region, the grain size is reduced and the deformation is more uniform, which reduces the probability of holes, especially large holes, in the continuous casting billet.

[0036] In some optional embodiments, the device for electromagnetically stirring the molten steel may include an electromagnetic stirring regulator, and the molten steel may be caused to rotate in a specific direction in the crystallizer through the regulation of the electromagnetic stirring regulator.

[0037] The intensity of stirring can be adjusted by changing the intensity of the input current of the electromagnetic stirring regulator. In addition, the stirring direction of the molten steel can be changed by changing the magnetic field direction of the electromagnetic stirring regulator. The molten steel is stirred alternately in positive and negative directions, that is, the molten steel is stirred in a clockwise direction and in a counterclockwise direction.

[0038] The continuous casting billet that enters the rolling process is called the intermediate billet. In the embodiment of the present application, the vertical roller mill can be used to roll the heated continuous casting billet. During the rolling process, the surface quality of the vertical roller may decrease, scraping the edge of the intermediate billet, thereby causing the holes in the sub-surface of the edge to expand, resulting in the deterioration of the quality of the edge of the intermediate billet. In the embodiment of the present application, equal-width rolling is used to reduce the pressure between the intermediate billet and the surface of the vertical roller during the rolling process, thereby improving the quality of the edge of the intermediate billet.

[0039] In some optional embodiments, in the continuous casting step, the columnar crystal thickness in the triangular region of the continuous casting billet is less than 30 mm. The columnar crystal thickness in the triangular region here refers to the thickness of the entire columnar crystal region.

[0040] The triangular area of ​​the continuous casting billet refers to the triangular area formed by the two diagonal lines starting from the corner of the slab in the cross section and the narrow side at an angle of 30-40 degrees.

[0041] By controlling the thickness of the columnar crystals in the triangular area of ​​continuous casting within the range of <30 mm, the grain size can be further reduced, making the deformation of the continuous casting billet more uniform, thereby reducing the probability of holes in the continuous casting billet.

[0042] In some optional embodiments, in the heating treatment step, the initial temperature of the continuous casting billet can be 600-750°C, the temperature of the preheating section can be 600-750°C, the temperature of the first heating section can be 750-900°C, and the temperature of the second heating section can be 900-1150°C.

[0043] The initial temperature of the continuous casting billet is the temperature of the continuous casting billet when it enters the heating furnace. The embodiment of the present application can reduce the edge corner cracks generated during the cooling process of the continuous casting billet in the air by increasing the initial temperature of the continuous casting billet, thereby reducing the edge cracks of the continuous casting billet caused by thermal stress, and further reducing the edge cracks of the hot-rolled steel coil.

[0044] In some optional embodiments, the heating rate of the heating treatment may be ≤6.5°C / min.

[0045] When the intermediate billet is in the preheating section and the first heating section, the temperature is ≤900°C. At this time, the thermoplasticity of the intermediate billet is poor. Therefore, the thermal stress on the intermediate billet can be reduced by reducing the heating rate of the heating treatment, so that the intermediate billet has good edge quality.

[0046] The heating rate in the embodiment of the present application may be the heating rate of the preheating section, the heating rate of the first heating section, or the heating rate of the second heating section.

[0047] In some optional embodiments, the rolling step may include rough rolling and finish rolling. Exemplarily, the rough rolling process may use a reversible rough rolling mill, and the finish rolling process may use a conventional finish rolling mill.

[0048] In some optional embodiments, the temperature of rough rolling may be 1050-1150°C, and the temperature of finish rolling may be 900-1000°C.

[0049] In some optional embodiments, in the rolling step, the width reduction of the continuous casting billet is ≤5 mm.

[0050] The width reduction in the embodiment of the present application may be the width reduction of rough rolling, and the width reduction of rough rolling is the absolute value of the difference between the width of the intermediate billet before and after rough rolling.

[0051] The embodiments of the present application can reduce the width reduction of the continuous casting billet during the rolling process, thereby reducing the proportion of edge cracks caused by large deformation of the continuous casting billet during the rolling process, thereby further improving the quality of the continuous casting billet and the edge quality of the hot-rolled steel coil.

[0052] In some optional embodiments, in the rolling step, the reduction amount of a single pass of rough rolling can be 15-35 mm.

[0053] In some optional embodiments, the maximum pass reduction of rough rolling can be 25-35 mm.

[0054] The embodiment of the present application can reduce the deformation and free flow variables of the intermediate billet during the pressing process by reducing the single-pass pressing amount of rough rolling, thereby reducing the holes in the continuous casting billet and further reducing the proportion of edge cracks caused by large deformation of the continuous casting billet during the rolling process.

[0055] In some optional embodiments, the rough rolling may be performed 5 times or 7 times.

[0056] In some optional embodiments, in the rolling step, the edge of the intermediate billet is heated before finish rolling, and the edge heating area is 8-15 mm of the edge of the intermediate billet.

[0057] In some optional embodiments, the temperature of the edge heating may be 90-120°C.

[0058] In the embodiment of the present application, the edge of the intermediate billet is heated to 90-120° C., so that the temperature of the edge of the intermediate billet can be ≥ 900° C. At this temperature, the intermediate billet has good thermoplasticity.

[0059] In the embodiment of the present application, an edge heater is arranged before the finishing mill to heat the edge of the intermediate billet.

[0060] The intermediate billet after rough rolling is in the shape of a strip, with a length of more than 100 meters. During the rolling process of the intermediate billet, the temperature drop of the edge is greater than that of the middle part. Under normal circumstances, the temperature of the edge is 80-100°C lower than that of the middle. The thermoplasticity of steel materials is closely related to their temperature. Within a certain temperature range, the higher the temperature, the better its processing and deformation ability. The edge temperature is low, and its processing and deformation ability is poor, and the probability of generating holes during the rolling process increases sharply. The function of the edge heater is to heat and compensate the edge temperature of the intermediate billet to be consistent with the middle temperature. On the one hand, it can improve its own thermoplasticity, and on the other hand, it can simultaneously improve its ability to resist deformation, thereby reducing the risk of edge cracking. The embodiment of the present application can further reduce the proportion of edge cracks caused by large deformation of the cast billet during the rolling process by heating the edge of the intermediate billet.

[0061] The edge heater for heating the edge of the intermediate billet includes, but is not limited to, an electromagnetic induction heating type edge heater.

[0062] In some optional embodiments, the control method may further include laminar cooling and coiling after rolling.

[0063] For example, a coiler may be used to coil the hot-rolled steel into a coil.

[0064] In a second aspect, an embodiment of the present application provides a hot-rolled steel coil, which is prepared by the control method of the first aspect of the present application.

[0065] In some optional embodiments, the thickness of the hot rolled steel coil may be 2-3.5 mm.

[0066] In some optional embodiments, the edge crack ratio of the hot-rolled steel coil is ≤0.1%, and the edge shear ratio of the hot-rolled steel coil is ≤10%. The yield rate of the hot-rolled steel coil can be increased by 2.3%-2.5% compared with the yield rate of the steel coil obtained by the conventional preparation method.

[0067] According to the present application, since the hot-rolled steel coil is prepared according to the control method of the present application, it has the beneficial effects of any implementation of the control method of the present application.

[0068] Example

[0069] The following examples describe the disclosure of the present application in more detail, and these examples are for illustrative purposes only, as various modifications and variations within the scope of the disclosure of the present application are apparent to those skilled in the art. Unless otherwise stated, all parts, percentages, and ratios reported in the following examples are by mass, and all reagents used in the examples are commercially available or synthesized according to conventional methods and can be used directly without further treatment, and the instruments used in the examples are commercially available.

[0070] Example 1

[0071] (1) Continuous casting: Molten steel is continuously cast to obtain a continuous casting billet. The molten steel is electromagnetically stirred in a crystallizer. The electromagnetic stirring adopts a forward and reverse alternating stirring mode. The forward and reverse alternating time is 16 s. The current of the electromagnetic stirring is 359 A. The frequency of the electromagnetic stirring is 14 Hz. The thickness of the columnar crystal in the triangular area of ​​the continuous casting billet is about 25 mm.

[0072] (2) Heating treatment: The continuous casting billet is heated in a heating furnace. The initial temperature of the continuous casting billet is 608°C, the temperature of the preheating section is 732°C, the temperature of the first heating section is 891°C, the temperature of the second heating section is 1144°C, and the heating rate is 6.1°C / min.

[0073] (3) Rolling: The heated continuous casting billet is rolled by equal-width rolling. During the rough rolling process: the width reduction of the continuous casting billet is 1.6 mm, the single-pass reduction of the rough rolling is 27 mm; the number of rough rolling passes is 5, the rough rolling temperature is 1060-1110°C, and the edge of the intermediate billet is heated before finishing rolling. The edge heating area is 13 mm of the edge of the intermediate billet, and the edge heating temperature is 98°C. The finishing rolling temperature is 900-980°C.

[0074] (4) The intermediate billet after rolling is laminar-cooled and coiled to obtain a hot-rolled steel coil.

[0075] The differences between the hot rolled steel coils prepared in Examples 1-8 and Comparative Examples 1-3 are shown in Table 1.

[0076] Table 1

[0077]

[0078]

[0079] Examples 1-8 and Comparative Examples 1-3 all produced 10 steel coils, and the finished product thickness, total length of the finished product, total number of edge cracks, total length of edge cracks, edge crack ratio, number of trimmed steel coils and trimmed ratio of the 10 steel coils were statistically analyzed. The statistical results are shown in Table 2.

[0080] Table 2

[0081]

[0082] Figure 3 This is a cross-sectional view of the edge structure of the ingot of Example 3. Figure 4 The cross-sectional view of the edge structure of the ingot of comparative example 1 is shown in FIG. Figure 3 and Figure 4It can be seen that electromagnetic stirring of molten steel in the crystallizer using a forward and reverse alternating stirring mode can reduce the number of columnar crystals, increase the number of equiaxed crystals, and increase the grain boundary area.

[0083] Figure 5 This is a cross-sectional morphology of the edge of the hot-rolled steel coil of Example 3. Figure 6 The cross-sectional morphology of the edge of the hot-rolled steel coil of Comparative Example 1 is shown in FIG. Figure 5 and Figure 6 It can be seen that electromagnetic stirring of the molten steel in the crystallizer and the use of a forward and reverse alternating stirring mode can reduce the occurrence of edge crack defects in the steel coil.

[0084] Figure 7 This is the edge morphology of the hot-rolled steel coil in Example 3. Figure 8 The edge morphology of the hot-rolled steel coil of comparative example 1 is shown in FIG. Figure 5 and Figure 6 It can be seen that electromagnetic stirring of the molten steel in the crystallizer and the use of a forward and reverse alternating stirring mode can reduce the occurrence of edge crack defects in the steel coil.

[0085] It can be seen from Examples 1-8 and Comparative Examples 1-3 of the present application that Examples 1-8 reduce the proportion of columnar crystals in the continuous casting billet by performing electromagnetic stirring of the molten steel in the crystallizer in alternating forward and reverse directions, controlling the time of the alternating forward and reverse directions within the range of 15-25s, the current of the electromagnetic stirring within the range of 260-360A, and controlling the frequency of the electromagnetic stirring within the range of 8-15Hz. During the rolling process of the continuous casting billet, the grain size is reduced, the deformation of the continuous casting billet is more uniform, and the probability of the continuous casting billet generating holes is reduced. The continuous casting billet is heated and rolled in an equal-width rolling manner, and the edge of the intermediate billet is heated before the finish rolling, thereby improving the quality of the continuous casting billet and the edge quality of the hot-rolled steel coil, and reducing the edge cracks of the hot-rolled steel coil from the source. The edge crack ratio of the hot-rolled steel coil in the examples of the present application is ≤0.1%, and the shearing ratio of the hot-rolled steel coil is ≤10%.

[0086] It can also be seen from Examples 1-8 of the present application and Comparative Examples 1-3 that Comparative Example 1 did not use electromagnetic stirring, the hot rolling process of Comparative Example 2 was different from that of Examples 1-8, and Comparative Example 3 did not use edge heating. The total number of edge cracks, total length of edge cracks, edge crack ratio, number of trimmed steel coils, and trimming ratio of Examples 1-8 were significantly better than those of Comparative Examples 1-3.

[0087] Although the present application has been described with reference to preferred embodiments, various modifications may be made thereto and parts thereof may be replaced with equivalents without departing from the scope of the present application. In particular, the various technical features mentioned in the various embodiments may be combined in any manner as long as there are no structural conflicts. The present application is not limited to the specific embodiments disclosed herein, but includes all technical solutions falling within the scope of the claims.

Claims

1. A method for controlling edge cracks of hot-rolled plates, characterized in that: The control method comprises: Continuous casting, continuously casting molten steel to obtain a continuous casting billet, and electromagnetically stirring the molten steel in a crystallizer, wherein the electromagnetic stirring adopts a forward and reverse alternating stirring mode, the forward and reverse alternating time is 15-25s, the current of the electromagnetic stirring is 260-360A, the frequency of the electromagnetic stirring is 8-15Hz, and the thickness of the columnar crystal in the triangular area of ​​the continuous casting billet is less than 30mm; Heating treatment, heating the continuous casting billet in a heating furnace to obtain a heated continuous casting billet; the heating treatment includes a preheating section, a first heating section and a second heating section; the initial temperature of the continuous casting billet is 600-750°C, the temperature of the preheating section is 600-750°C, the temperature of the first heating section is 750-900°C, the temperature of the second heating section is 900-1150°C, and the heating rate of the heating treatment is ≤6.5°C / min; Rolling, rolling the heated continuous casting billet by equal-width rolling, wherein the rolling includes rough rolling and finish rolling, and the intermediate billet is edge-heated before the finish rolling, the edge heating area is 8-15 mm of the edge of the intermediate billet, the edge heating temperature is 90-120° C., and the width reduction of the continuous casting billet is ≤5 mm; The material of the hot-rolled plate is oriented silicon steel.

2. The control method according to claim 1, characterized in that: The temperature of the rough rolling is 1050-1150°C, and the temperature of the finish rolling is 900-1000°C.

3. The control method according to claim 1, characterized in that: In the rolling step, the single pass reduction of the rough rolling is 15-35 mm; The rough rolling is performed in 5 or 7 passes.

4. The control method according to claim 1, characterized in that: The control method also includes laminar cooling and coiling after rolling.

5. A hot rolled steel coil, characterized in that: It is prepared by the control method according to any one of claims 1 to 4.

6. The hot rolled steel coil according to claim 5, characterized in that: The thickness of the hot-rolled steel coil is 2-3.5 mm; The edge crack ratio of the hot-rolled steel coil is ≤0.1%, and the edge shearing ratio of the hot-rolled steel coil is ≤10%.

Citation Information

Patent Citations

  • High-elongation flange steel plate and preparation method thereof

    CN109202028A