A viscous composite phase change material, a viscous composite phase change sheet, and a preparation method and application thereof

By adding high melting point regulators and nucleating agents to the polystyrene/fatty acid methyl ester system, the problem of volume changes in viscous composite phase change materials during thermal cycles is solved, and better temperature regulation effects and stability are achieved.

CN117924848BActive Publication Date: 2024-10-01PHASE CHANGE ENERGY STORAGE (BEIJING) TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410167089.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-02-06
Publication Date
2024-10-01
Estimated Expiration
2044-02-06

Smart Images

  • Figure BDA0004699981570000041
    Figure BDA0004699981570000041
  • Figure BDA0004699981570000051
    Figure BDA0004699981570000051
  • Figure BDA0004699981570000071
    Figure BDA0004699981570000071
Patent Text Reader

Abstract

The present invention provides a viscous composite phase change material, a viscous composite phase change sheet, and a preparation method and application thereof. The raw materials for preparing the viscous composite phase change material include the following components by weight: 20 to 40 parts of polystyrene, 30 to 60 parts of fatty acid methyl ester, 5 to 15 parts of hydrogenated styrene olefin thermoplastic elastomer, 5 to 30 parts of high melting point regulator and 0.1 to 2 parts of nucleating agent. The viscous composite phase change material of the present invention effectively adjusts the volume expansion rate and contraction rate of the composite phase change material system by adjusting the addition amount of the high melting point regulator and the nucleating agent.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of temperature regulating materials, and in particular to a viscous composite phase change material, a viscous composite phase change sheet material, and a preparation method and application thereof. Background Art

[0002] Phase change energy storage materials have the ability to absorb or release a large amount of thermal energy when changing their physical state, storing and releasing energy by melting and solidifying at a certain temperature. Therefore, phase change energy storage materials have attracted attention for their wide applications in the fields of heat storage and thermal protection, especially in the thermal protection and heat dissipation of electronic devices.

[0003] Viscous composite phase change materials will have great application prospects in the fields of thermal protection and heat dissipation of electronic equipment, functional fabrics, etc. However, during the heat absorption / release cycle, the viscous composite phase change material is generally accompanied by volume expansion / contraction changes, which affects the temperature control performance of the composite phase change material. At present, no scientific researchers have conducted systematic research in this area.

[0004] CN116496763A discloses a composite phase change material and a preparation method thereof and a method for adjusting the phase change temperature of the phase change material. The composite phase change material comprises the following components by weight: 30 to 80 parts of phase change material, 15 to 55 parts of supporting material, 3 to 20 parts of softening aid and 0.1 to 10 parts of ultra-high molecular weight polyethylene. By adding a certain amount of ultra-high molecular weight polyethylene to the system of the phase change material, a synergistic effect can be produced with the supporting material of the composite phase change material. Although the composite phase change material has the ability to adjust the phase change temperature, it does not have the ability to adjust the volume change of the composite phase change material.

[0005] CN114892307A discloses an elastic phase-change temperature-regulating fiber and a preparation method thereof. The elastic phase-change temperature-regulating fiber is mainly made of the following components: 20-60 parts of phase-change material, 5-30 parts of elastomer, 5-50 parts of thermoplastic resin, 3-15 parts of thermal conductive material and 0-5 parts of auxiliary agent. Although the invention improves the flexibility and mechanical strength of the elastic phase-change temperature-regulating fiber by adding a specific proportion of elastomer, thermoplastic resin and thermal conductive material to the phase-change material, it cannot adjust the volume change of the composite phase-change material.

[0006] In view of this, the present invention is proposed. Summary of the invention

[0007] One of the purposes of the present invention is to provide a viscous composite phase change material, wherein the raw materials for preparing the viscous composite phase change material include the following components by weight: 20-40 parts of polystyrene, 30-60 parts of fatty acid methyl ester, 5-15 parts of hydrogenated styrene olefin thermoplastic elastomer, 5-30 parts of high melting point regulator and 0.1-2 parts of nucleating agent. The viscous composite phase change material of the present invention is a polystyrene / fatty acid methyl ester system, and the high melting point regulator and nucleating agent are added at the same time, which has a synergistic effect, can effectively adjust the volume shrinkage / expansion performance of the phase change composite material, so that the viscous phase change composite material achieves a better temperature control effect.

[0008] The second object of the present invention is to provide a method for preparing the viscous composite phase change material, which comprises the following steps: mixing polystyrene, fatty acid methyl ester, hydrogenated styrene olefin thermoplastic elastomer, high melting point regulator and nucleating agent, and kneading to obtain the viscous composite phase change material.

[0009] The third object of the present invention is to provide a viscous composite phase change sheet, which is obtained by pressing the viscous composite phase change material as mentioned above.

[0010] A fourth object of the present invention is to provide a method for preparing the viscous composite phase change sheet, which comprises the following steps: pressing the above-mentioned viscous composite phase change material into sheets to obtain the viscous composite phase change sheet.

[0011] A fifth object of the present invention is to provide an application of the viscous composite phase change material or the viscous composite phase change sheet in the preparation of a temperature regulating material.

[0012] In order to achieve the above-mentioned purpose of the present invention, the following technical solutions are particularly adopted:

[0013] In a first aspect, the present invention provides a viscous composite phase change material, wherein the raw materials for preparing the viscous composite phase change material include the following components in parts by weight:

[0014] 20-40 parts of polystyrene, 30-60 parts of fatty acid methyl ester, 5-15 parts of hydrogenated styrene olefin thermoplastic elastomer, 5-30 parts of high melting point regulator and 0.1-2 parts of nucleating agent.

[0015] In the present invention, a system using polystyrene / fatty acid methyl ester as phase change material and simultaneously adding a high melting point regulator and a nucleating agent has a synergistic effect and can effectively adjust the volume shrinkage / expansion properties of the phase change composite material, so that the viscous phase change composite material achieves a better temperature regulation effect.

[0016] Among them, the high melting point regulator crystallizes at a higher temperature, restricting the movement of the polymer chain in the system, so that the polymer skeleton structure can be maintained, and the system's encapsulation performance for phase change materials is improved. The nucleating agent accelerates the crystallization rate of the high melting point regulator, refines the grain structure, and is conducive to improving the rigidity of the product, thereby affecting the change in its volume before and after the phase change.

[0017] In the raw materials for preparing the viscous composite phase change material, the added amount of polystyrene is 20 to 40 parts, for example, it can be 20 parts, 22 parts, 24 parts, 26 parts, 28 parts, 30 parts, 32 parts, 34 parts, 36 parts, 38 parts, 40 parts, etc.

[0018] In the preparation raw materials of the viscous composite phase change material, the added amount of fatty acid methyl ester is 30 to 60 parts, for example, it can be 30 parts, 32 parts, 34 parts, 36 parts, 38 parts, 40 parts, 42 parts, 44 parts, 46 parts, 48 ​​parts, 50 parts, 52 parts, 54 parts, 56 parts, 58 parts, 60 parts, etc.

[0019] In the raw materials for preparing the viscous composite phase change material, the addition amount of hydrogenated styrene-based thermoplastic elastomer is 5 to 15 parts, for example, it can be 5 parts, 6 parts, 7 parts, 8 parts, 9 parts, 10 parts, 11 parts, 12 parts, 13 parts, 14 parts, 15 parts, etc.

[0020] In the preparation raw materials of the viscous composite phase change material, the added amount of the high melting point regulator is 5 to 30 parts, for example, it can be 5 parts, 6 parts, 7 parts, 8 parts, 9 parts, 10 parts, 12 parts, 14 parts, 15 parts, 16 parts, 18 parts, 20 parts, 22 parts, 24 parts, 25 parts, 26 parts, 28 parts, 30 parts, etc.

[0021] In the raw materials for preparing the viscous composite phase change material, the added amount of the nucleating agent is 0.1 to 2 parts, for example, it can be 0.1 parts, 0.2 parts, 0.4 parts, 0.6 parts, 0.8 parts, 1 parts, 1.2 parts, 1.4 parts, 1.6 parts, 1.8 parts, 2 parts, etc.

[0022] In the present invention, the volume expansion / contraction rate of the composite phase change material system can be effectively adjusted by adjusting the addition amount of the high melting point regulator and the nucleating agent.

[0023] Preferably, the weight average molecular weight of the polystyrene is 6×10 4 ~10×10 4 g / mol, for example, 6×10 4 g / mol, 6.5×10 4 g / mol, 7×10 4 g / mol, 7.5×10 4 g / mol, 8×104 g / mol, 8.5×10 4 g / mol, 9×10 4 g / mol, 9.5×10 4 g / mol, 10×10 4 g / mol, etc.

[0024] Preferably, the melt index of the polystyrene is 3 to 8 g / 10 min, for example, 3 g / mol, 3.5 g / mol, 4 g / mol, 4.5 g / mol, 5 g / mol, 5.5 g / mol, 6 g / mol, 6.5 g / mol, 7 g / mol, 7.5 g / mol, 8 g / mol, etc.

[0025] Preferably, the structural formula of the fatty acid methyl ester is as shown in Formula I below:

[0026]

[0027] Among them, R1 is selected from a straight chain or branched alkyl group with a carbon number of 10 or more (for example, 10, 12, 14, 16, 18, 20, 22, 24, 26, 28, 30, etc.), preferably a C12-C24 straight chain or branched alkyl group, and more preferably a C14-C18 straight chain or branched alkyl group.

[0028] As some embodiments of the present invention, the fatty acid methyl esters include but are not limited to methyl dodecanoate (methyl caprate), methyl dodecanoate (methyl laurate), methyl tetradecanoate (methyl myristic acid), methyl hexadecanoate (methyl palmitate), methyl octadecanoate (methyl stearate), methyl eicosanoate (methyl arachidate), methyl docosanoate (methyl behenate), etc.

[0029] Preferably, the fatty acid methyl ester is selected from any one of methyl stearate, methyl palmitate or methyl myristic acid, or a combination of at least two thereof.

[0030] Preferably, the hydrogenated styrene olefin-based thermoplastic elastomer is selected from any one or a combination of at least two of a hydrogenated styrene-butadiene-styrene triblock polymer, a hydrogenated styrene-isoprene-styrene triblock polymer, a styrene-isoprene-styrene triblock copolymer, a hydrogenated styrene-isoprene diblock polymer, a star-shaped styrene-ethylene-butylene-styrene block copolymer or a hydrogenated styrene-isoprene triblock polymer.

[0031] Preferably, the high melting point regulator is selected from long-chain fatty acids and / or long-chain fatty alcohols.

[0032] Preferably, the structural formula of the long-chain fatty acid is as shown in Formula II below:

[0033]

[0034] Among them, R2 is selected from C12~C24 (for example, it can be 12, 14, 16, 18, 20, 22, 24, etc.) straight chain or branched alkyl, preferably C16~C20 straight chain or branched alkyl.

[0035] Preferably, the long-chain fatty acid is stearic acid.

[0036] Preferably, the structural formula of the long-chain fatty alcohol is as shown in Formula III below:

[0037] R3-CH2-OH

[0038] Formula III

[0039] Among them, R3 is selected from C12~C24 (for example, it can be 12, 14, 16, 18, 20, 22, 24, etc.) straight chain or branched alkyl, preferably C16~C20 straight chain or branched alkyl.

[0040] Preferably, the long-chain fatty alcohol is stearyl alcohol.

[0041] Preferably, the nucleating agent is selected from stearate, carbonate or ultra high molecular weight polyethylene.

[0042] Preferably, the stearate is selected from zinc stearate and / or calcium stearate.

[0043] Preferably, the carbonate is zinc carbonate and / or calcium carbonate.

[0044] Preferably, the weight average molecular weight of the ultra-high molecular weight polyethylene is 1×10 7 ~10×10 7 g / mol, for example, 1×10 7 g / mol, 2×10 7 g / mol, 3×10 7 g / mol, 4×10 7 g / mol, 5×10 7 g / mol, 6×10 7 g / mol, 7×10 7 g / mol, 8×10 7 g / mol, 9×10 7 g / mol, 10×10 7 g / mol, etc.

[0045] Preferably, the molecular weight distribution width index of the ultra-high molecular weight polyethylene is 10-15, for example, it can be 10, 11, 12, 13, 14, 15, etc.

[0046] In a second aspect, the present invention provides a method for preparing the viscous composite phase change material as described in the first aspect, the preparation method comprising the following steps:

[0047] The viscous composite phase change material is obtained by mixing polystyrene, fatty acid methyl ester, hydrogenated styrene olefin thermoplastic elastomer, high melting point regulator and nucleating agent, and performing banburying.

[0048] Preferably, the banburying temperature is 180-200°C, for example, 180°C, 185°C, 190°C, 195°C, 200°C, etc.

[0049] Preferably, the kneading time is 0.5 to 2 h, for example, it can be 0.5 h, 0.6 h, 0.8 h, 1 h, 1.2 h, 1.4 h, 1.6 h, 1.8 h, 2 h, etc.

[0050] In a third aspect, the present invention provides a viscous composite phase change sheet, wherein the viscous composite phase change sheet is obtained by pressing the viscous composite phase change material as described in the first aspect.

[0051] Preferably, the thickness of the adhesive composite phase change sheet is 1 to 3 mm, for example, it may be 1 mm, 1.2 mm, 1.4 mm, 1.6 mm, 1.8 mm, 2 mm, 2.2 mm, 2.4 mm, 2.6 mm, 2.8 mm, 3 mm, etc.

[0052] Preferably, the thermal expansion coefficient of the viscous composite phase change sheet is 1.0-1.7%, for example, it may be 1.0%, 1.1%, 1.2%, 1.3%, 1.4%, 1.5%, 1.6%, 1.7%, etc.

[0053] Preferably, the thermal shrinkage rate of the adhesive composite phase change sheet is 0.9-1.6%, for example, it can be 0.9%, 1.0%, 1.1%, 1.2%, 1.3%, 1.4%, 1.5%, 1.6%, etc.

[0054] In a fourth aspect, the present invention provides a method for preparing the viscous composite phase change sheet, the method for preparing the viscous composite phase change sheet comprising the following steps:

[0055] The viscous composite phase change material is pressed into sheets to obtain the viscous composite phase change sheet.

[0056] Preferably, the tableting is carried out in a vulcanizing press.

[0057] Preferably, the tabletting pressure is 1 to 3 MPa, for example, 1 MPa, 1.2 MPa, 1.4 MPa, 1.6 MPa, 1.8 MPa, 2 MPa, 2.2 MPa, 2.4 MPa, 2.6 MPa, 2.8 MPa, 3 MPa, etc.

[0058] In a fifth aspect, the present invention provides a use of the viscous composite phase change material or the viscous composite phase change sheet in the preparation of a temperature regulating material.

[0059] Compared with the prior art, the present invention has the following beneficial effects:

[0060] (1) The present invention limits the movement of polymer chains in the system by adding a high melting point regulator to crystallize at a higher temperature, thereby maintaining the polymer skeleton structure and improving the system's encapsulation performance for phase change materials;

[0061] (2) The present invention accelerates the crystallization rate of the high melting point modifier by adding a nucleating agent, refines the grain structure, and is beneficial to improving the rigidity of the product, thereby affecting the change in volume before and after the phase change;

[0062] (3) The present invention can effectively adjust the volume expansion / contraction rate of the composite phase change material system by adjusting the addition amount of the high melting point regulator and the nucleating agent. DETAILED DESCRIPTION

[0063] Unless otherwise defined herein, scientific and technical terms used in conjunction with the present invention shall have the meanings commonly understood by those of ordinary skill in the art. The meaning and scope of the terms should be clear, however, in the case of any potential ambiguity, the definitions provided herein take precedence over any dictionary or external definitions. In this application, unless otherwise stated, the use of "or" means "and / or". In addition, the use of the term "including" and other forms is non-limiting.

[0064] It should be noted that specific details are described in the following description to facilitate a full understanding of the present invention. However, the present invention can be implemented in a variety of other ways different from those described herein, and those skilled in the art can make similar generalizations without violating the connotation of the present invention. Therefore, the present invention is not limited to the specific embodiments disclosed below.

[0065] Example 1

[0066] This embodiment provides a viscous composite phase change material, and a sheet prepared therefrom;

[0067] The viscous composite phase change material comprises the following components by weight:

[0068]

[0069]

[0070] The above-mentioned viscous composite phase change sheet is prepared by the following steps:

[0071] S1. Preparation of viscous composite phase change material:

[0072] The polystyrene, fatty acid methyl ester, hydrogenated styrene olefin thermoplastic elastomer, high melting point regulator and nucleating agent are mixed in a high speed mixer according to a proportion, placed in an internal mixer, heated to 190° C., and internally kneaded for 1 hour to obtain the viscous composite phase change material.

[0073] S2. Preparation of viscous composite phase change sheet:

[0074] The above-mentioned viscous composite phase change material was pressed into a sheet in a vulcanizer, with the hot plate temperature being room temperature and the pressure being 2 MPa, to obtain a viscous composite phase change sheet with a thickness of 2 mm.

[0075] Example 2

[0076] This embodiment provides a viscous composite phase change material, and a sheet prepared therefrom;

[0077] The viscous composite phase change material comprises the following components by weight:

[0078]

[0079] The above-mentioned viscous composite phase change sheet is prepared by the following steps:

[0080] S1. Preparation of viscous composite phase change material:

[0081] The polystyrene, fatty acid methyl ester, hydrogenated styrene olefin thermoplastic elastomer, high melting point regulator and nucleating agent are mixed in a high speed mixer according to a proportion, placed in an internal mixer, heated to 190° C., and internally kneaded for 1 hour to obtain the viscous composite phase change material.

[0082] S2. Preparation of viscous composite phase change sheet:

[0083] The above-mentioned viscous composite phase change material was pressed into a sheet in a vulcanizer, with the hot plate temperature being room temperature and the pressure being 2 MPa, to obtain a viscous composite phase change sheet with a thickness of 2 mm.

[0084] Example 3

[0085] This embodiment provides a viscous composite phase change material, and a sheet prepared therefrom;

[0086] The viscous composite phase change material comprises the following components by weight:

[0087]

[0088] The above-mentioned viscous composite phase change sheet is prepared by the following steps:

[0089] S1. Preparation of viscous composite phase change material:

[0090] The polystyrene, fatty acid methyl ester, hydrogenated styrene olefin thermoplastic elastomer, high melting point regulator and nucleating agent are mixed in a high speed mixer according to a proportion, placed in an internal mixer, heated to 190° C., and internally kneaded for 1 hour to obtain the viscous composite phase change material.

[0091] S2. Preparation of viscous composite phase change sheet:

[0092] The above-mentioned viscous composite phase change material was pressed into a sheet in a vulcanizer, with the hot plate temperature being room temperature and the pressure being 2 MPa, to obtain a viscous composite phase change sheet with a thickness of 2 mm.

[0093] Example 4

[0094] This embodiment provides a viscous composite phase change material, and a sheet prepared therefrom;

[0095] The viscous composite phase change material comprises the following components by weight:

[0096]

[0097] The above-mentioned viscous composite phase change sheet is prepared by the following steps:

[0098] S1. Preparation of viscous composite phase change material:

[0099] The polystyrene, fatty acid methyl ester, hydrogenated styrene olefin thermoplastic elastomer, high melting point regulator and nucleating agent are mixed in a high speed mixer according to a proportion, placed in an internal mixer, heated to 190° C., and internally kneaded for 1 hour to obtain the viscous composite phase change material.

[0100] S2. Preparation of viscous composite phase change sheet:

[0101] The above-mentioned viscous composite phase change material was pressed into a sheet in a vulcanizer, with the hot plate temperature being room temperature and the pressure being 2 MPa, to obtain a viscous composite phase change sheet with a thickness of 2 mm.

[0102] Example 5

[0103] This embodiment provides a viscous composite phase change material, and a sheet prepared therefrom;

[0104] The viscous composite phase change material comprises the following components by weight:

[0105]

[0106]

[0107] The above-mentioned viscous composite phase change sheet is prepared by the following steps:

[0108] S1. Preparation of viscous composite phase change material:

[0109] The polystyrene, fatty acid methyl ester, hydrogenated styrene olefin thermoplastic elastomer, high melting point regulator and nucleating agent are mixed in a high speed mixer according to a proportion, placed in an internal mixer, heated to 190° C., and internally kneaded for 1 hour to obtain the viscous composite phase change material.

[0110] S2. Preparation of viscous composite phase change sheet:

[0111] The above-mentioned viscous composite phase change material was pressed into a sheet in a vulcanizer, with the hot plate temperature being room temperature and the pressure being 2 MPa, to obtain a viscous composite phase change sheet with a thickness of 2 mm.

[0112] Example 6

[0113] This embodiment provides a viscous composite phase change material, and a sheet prepared therefrom;

[0114] The viscous composite phase change material comprises the following components by weight:

[0115]

[0116] The above-mentioned viscous composite phase change sheet is prepared by the following steps:

[0117] S1. Preparation of viscous composite phase change material:

[0118] The polystyrene, fatty acid methyl ester, hydrogenated styrene olefin thermoplastic elastomer, high melting point regulator and nucleating agent are mixed in a high speed mixer according to a proportion, placed in an internal mixer, heated to 190° C., and internally kneaded for 1 hour to obtain the viscous composite phase change material.

[0119] S2. Preparation of viscous composite phase change sheet:

[0120] The above-mentioned viscous composite phase change material was pressed into a sheet in a vulcanizer, with the hot plate temperature being room temperature and the pressure being 2 MPa, to obtain a viscous composite phase change sheet with a thickness of 2 mm.

[0121] Example 7

[0122] This embodiment provides a viscous composite phase change material, and a sheet prepared therefrom;

[0123] The viscous composite phase change material comprises the following components by weight:

[0124]

[0125] The above-mentioned viscous composite phase change sheet is prepared by the following steps:

[0126] S1. Preparation of viscous composite phase change material:

[0127] The polystyrene, fatty acid methyl ester, hydrogenated styrene olefin thermoplastic elastomer, high melting point regulator and nucleating agent are mixed in a high speed mixer according to a proportion, placed in an internal mixer, heated to 190° C., and internally kneaded for 1 hour to obtain the viscous composite phase change material.

[0128] S2. Preparation of viscous composite phase change sheet:

[0129] The above-mentioned viscous composite phase change material was pressed into a sheet in a vulcanizer, with the hot plate temperature being room temperature and the pressure being 2 MPa, to obtain a viscous composite phase change sheet with a thickness of 2 mm.

[0130] Example 8

[0131] This embodiment provides a viscous composite phase change material, and a sheet prepared therefrom;

[0132] The viscous composite phase change material comprises the following components by weight:

[0133]

[0134] The above-mentioned viscous composite phase change sheet is prepared by the following steps:

[0135] S1. Preparation of viscous composite phase change material:

[0136] The polystyrene, fatty acid methyl ester, hydrogenated styrene olefin thermoplastic elastomer, high melting point regulator and nucleating agent are mixed in a high speed mixer according to a proportion, placed in an internal mixer, heated to 190° C., and internally kneaded for 1 hour to obtain the viscous composite phase change material.

[0137] S2. Preparation of viscous composite phase change sheet:

[0138] The above-mentioned viscous composite phase change material was pressed into a sheet in a vulcanizer, with the hot plate temperature being room temperature and the pressure being 2 MPa, to obtain a viscous composite phase change sheet with a thickness of 2 mm.

[0139] Example 9

[0140] This embodiment provides a viscous composite phase change material, and a sheet prepared therefrom;

[0141] The viscous composite phase change material comprises the following components by weight:

[0142]

[0143] The above-mentioned viscous composite phase change sheet is prepared by the following steps:

[0144] S1. Preparation of viscous composite phase change material:

[0145] The polystyrene, fatty acid methyl ester, hydrogenated styrene olefin thermoplastic elastomer, high melting point regulator and nucleating agent are mixed in a high speed mixer according to a proportion, placed in an internal mixer, heated to 190° C., and internally kneaded for 1 hour to obtain the viscous composite phase change material.

[0146] S2. Preparation of viscous composite phase change sheet:

[0147] The above-mentioned viscous composite phase change material was pressed into a sheet in a vulcanizer, with the hot plate temperature being room temperature and the pressure being 2 MPa, to obtain a viscous composite phase change sheet with a thickness of 2 mm.

[0148] Example 10

[0149] This embodiment provides a viscous composite phase change material, and a sheet prepared therefrom;

[0150] The viscous composite phase change material comprises the following components by weight:

[0151]

[0152]

[0153] The above-mentioned viscous composite phase change sheet is prepared by the following steps:

[0154] S1. Preparation of viscous composite phase change material:

[0155] The polystyrene, fatty acid methyl ester, hydrogenated styrene olefin thermoplastic elastomer, high melting point regulator and nucleating agent are mixed in a high speed mixer according to a proportion, placed in an internal mixer, heated to 190° C., and internally kneaded for 1 hour to obtain the viscous composite phase change material.

[0156] S2. Preparation of viscous composite phase change sheet:

[0157] The above-mentioned viscous composite phase change material was pressed into a sheet in a vulcanizer, with the hot plate temperature being room temperature and the pressure being 2 MPa, to obtain a viscous composite phase change sheet with a thickness of 2 mm.

[0158] Comparative Example 1

[0159] This comparative example provides a viscous composite phase change material, and a sheet prepared therefrom;

[0160] The viscous composite phase change material comprises the following components by weight:

[0161]

[0162] The above-mentioned viscous composite phase change sheet is prepared by the following steps:

[0163] S1. Preparation of viscous composite phase change material:

[0164] The polystyrene, fatty acid methyl ester, hydrogenated styrene olefin thermoplastic elastomer and high melting point regulator are mixed in a high speed mixer according to a proportion, placed in an internal mixer, heated to 190° C., and internally kneaded for 1 hour to obtain the viscous composite phase change material.

[0165] S2. Preparation of viscous composite phase change sheet:

[0166] The above-mentioned viscous composite phase change material was pressed into a sheet in a vulcanizer, with the hot plate temperature being room temperature and the pressure being 2 MPa, to obtain a viscous composite phase change sheet with a thickness of 2 mm.

[0167] Comparative Example 2

[0168] This comparative example provides a viscous composite phase change material, and a sheet prepared therefrom;

[0169] The viscous composite phase change material comprises the following components by weight:

[0170]

[0171] The above-mentioned viscous composite phase change sheet is prepared by the following steps:

[0172] S1. Preparation of viscous composite phase change material:

[0173] The polystyrene, fatty acid methyl ester, hydrogenated styrene olefin thermoplastic elastomer and nucleating agent are mixed in a high-speed mixer according to a proportion, placed in an internal mixer, heated to 190° C., and internally kneaded for 1 hour to obtain the viscous composite phase change material.

[0174] S2. Preparation of viscous composite phase change sheet:

[0175] The above-mentioned viscous composite phase change material was pressed into a sheet in a vulcanizer, with the hot plate temperature being room temperature and the pressure being 2 MPa, to obtain a viscous composite phase change sheet with a thickness of 2 mm.

[0176] Comparative Example 3

[0177] This comparative example provides a viscous composite phase change material, and a sheet prepared therefrom;

[0178] The viscous composite phase change material comprises the following components by weight:

[0179]

[0180] The above-mentioned viscous composite phase change sheet is prepared by the following steps:

[0181] S1. Preparation of viscous composite phase change material:

[0182] The polystyrene, fatty acid methyl ester, hydrogenated styrene olefin thermoplastic elastomer, high melting point regulator and nucleating agent are mixed in a high speed mixer according to a proportion, placed in an internal mixer, heated to 190° C., and internally kneaded for 1 hour to obtain the viscous composite phase change material.

[0183] S2. Preparation of viscous composite phase change sheet:

[0184] The above-mentioned viscous composite phase change material was pressed into a sheet in a vulcanizer, with the hot plate temperature being room temperature and the pressure being 2 MPa, to obtain a viscous composite phase change sheet with a thickness of 2 mm.

[0185] Comparative Example 4

[0186] This comparative example provides a viscous composite phase change material and a sheet prepared therefrom; the only difference from Example 10 is that polystyrene is replaced with polyethylene of equal mass, and the contents of other components and the preparation method are exactly the same as those in Example 10.

[0187] Comparative Example 5

[0188] This comparative example provides a viscous composite phase change material and a sheet prepared therefrom; the only difference from Example 10 is that methyl stearate is replaced with an equal mass of octadecane, and the contents of other components and the preparation method are exactly the same as those in Example 10.

[0189] Comparative Example 6

[0190] This comparative example provides a viscous composite phase change material and a sheet prepared therefrom; the only difference from Implementation 10 is that methyl stearate is replaced with ethyl stearate of equal mass, and the contents of other components and the preparation method are exactly the same as those in Example 10.

[0191] Test Case

[0192] Test samples: the viscous composite phase change sheets provided in Examples 1 to 10, and the viscous composite phase change sheets provided in Comparative Examples 1 to 6;

[0193] Test method:

[0194] (1) Cut a sheet with a side length of 20×20×2 mm; put it into a high and low temperature cycle box, control the temperature at the phase change temperature ±20°C, cycle it 100 times, and observe the leakage on the sheet surface;

[0195] (2) Cut a sheet with a side length of 20×20×2 mm; place it on the aluminum foil and mark the four sides with a marker; place it on a heated hot plate or oven at a temperature of phase change temperature + 20°C for 10 min; cool it to a temperature of -20°C; measure the longitudinal and latitudinal dimensions of the sheet after the test; and calculate the thermal expansion rate and thermal contraction rate.

[0196] The specific test results are shown in Table 1:

[0197] Table 1

[0198]

[0199]

[0200] As can be seen from the test data in Table 1, after the viscous composite phase change sheet of the present invention has been subjected to 100 high and low temperature cycles at a phase change temperature of ±20°C, there is no powdery substance on the surface of the sheet and no leakage; and the thermal expansion rate of the viscous composite phase change sheet can be controlled to be 0.6-1.4% by adjusting the content of the high melting point regulator and the nucleating agent; the thermal shrinkage rate of the viscous composite phase change sheet is 0.9-1.6%, which effectively adjusts the volume expansion / contraction rate of the composite phase change material system.

[0201] From the comparison between Example 1 and Comparative Example 1, it can be seen that without adding a nucleating agent, even if the content of the high melting point regulator is increased, powdery substances will appear on the surface of the sheet after high and low temperature cycles, and leakage will occur; in addition, not adding a nucleating agent will also lead to a decrease in the thermal shrinkage rate of the viscous composite phase change sheet.

[0202] From the comparison between Example 1 and Comparative Examples 2 and 3, it can be seen that if no high melting point regulator is added or the content of the high melting point regulator is too low, more powdery substances will appear on the surface of the sheet after the high and low temperature cycle, and serious leakage will occur; in addition, if no high melting point regulator is added or the content of the high melting point regulator is too low, the polymer skeleton structure is difficult to maintain, and the sheet may be severely deformed.

[0203] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.

Claims

1. A viscous composite phase change sheet, characterized in that: The viscous composite phase change sheet material is obtained by pressing the viscous composite phase change material into sheets; Wherein, the thermal expansion rate of the viscous composite phase change sheet is 1.0-1.7%, and the thermal shrinkage rate of the viscous composite phase change sheet is 0.9-1.6%; The raw materials for preparing the viscous composite phase change material include the following components by weight: 20-40 parts of polystyrene, 30-60 parts of fatty acid methyl ester, 5-15 parts of hydrogenated styrene olefin thermoplastic elastomer, 5-30 parts of high melting point regulator and 0.1-2 parts of nucleating agent; The structural formula of the fatty acid methyl ester is shown in the following formula I: Wherein, R1 is a C14-C18 straight or branched chain alkyl; The high melting point regulator is selected from long-chain fatty acids and / or long-chain fatty alcohols; the structural formula of the long-chain fatty acid is shown in Formula II below: Wherein, R2 is a C16-C20 straight chain or branched chain alkyl; The structural formula of the long-chain fatty alcohol is shown in Formula III below: R3-CH2-OH Formula IIII Wherein, R3 is a C16-C20 straight chain or branched chain alkyl; The nucleating agent is selected from stearate, carbonate or ultra-high molecular weight polyethylene.

2. The adhesive composite phase change sheet according to claim 1, characterized in that: The weight average molecular weight of the polystyrene is 6×10 4 ~10×10 4 g / mol.

3. The adhesive composite phase change sheet according to claim 1, characterized in that: The melt index of the polystyrene is 3 to 8 g / 10 min.

4. The adhesive composite phase change sheet according to claim 1, characterized in that: The fatty acid methyl ester is selected from any one of methyl stearate, methyl palmitate or methyl myristic acid, or a combination of at least two thereof.

5. The adhesive composite phase change sheet according to claim 1, characterized in that: The hydrogenated styrene-olefin thermoplastic elastomer is selected from any one or a combination of at least two of hydrogenated styrene-butadiene-styrene triblock polymers, hydrogenated styrene-isoprene-styrene triblock polymers, styrene-isoprene-styrene triblock copolymers, hydrogenated styrene-isoprene diblock polymers, star-shaped styrene-ethylene-butylene-styrene block copolymers or hydrogenated styrene-isoprene triblock polymers.

6. The adhesive composite phase change sheet according to claim 1, characterized in that: The long-chain fatty acid is stearic acid.

7. The adhesive composite phase change sheet according to claim 1, characterized in that: The long-chain fatty alcohol is stearyl alcohol.

8. The adhesive composite phase change sheet according to claim 1, characterized in that: The stearate is selected from zinc stearate and / or calcium stearate.

9. The adhesive composite phase change sheet according to claim 1, characterized in that: The carbonate is selected from zinc carbonate and / or calcium carbonate.

10. The adhesive composite phase change sheet according to claim 1, characterized in that: The weight average molecular weight of the ultra-high molecular weight polyethylene is 1×10 7 ~10×10 7 g / mol.

11. The adhesive composite phase change sheet according to claim 1, characterized in that: The molecular weight distribution width index of the ultra-high molecular weight polyethylene is 10-15.

12. The adhesive composite phase change sheet according to claim 1, characterized in that: The thickness of the adhesive composite phase change sheet is 1 to 3 mm.

13. A method for preparing a viscous composite phase change sheet according to any one of claims 1 to 12, characterized in that: The preparation method comprises the following steps: The polystyrene, fatty acid methyl ester, hydrogenated styrene olefin thermoplastic elastomer, high melting point regulator and nucleating agent are mixed and kneaded to obtain the viscous composite phase change material; The viscous composite phase change material is pressed into sheets to obtain the viscous composite phase change sheet.

14. The method for preparing the viscous composite phase change material according to claim 13, characterized in that: The temperature of the banburying is 180-200° C.; the time of the banburying is 0.5-2 hours.

15. The method for preparing the viscous composite phase change material according to claim 13, characterized in that: The tableting is carried out in a vulcanizing press.

16. The method for preparing the viscous composite phase change material according to claim 13, characterized in that: The tabletting pressure is 1-3 MPa.

17. Use of the adhesive composite phase change sheet according to any one of claims 1 to 12 in preparing a temperature regulating material.