Toughened nylon composition and its preparation and use

The pericyclic reaction between 1,1-disubstituted olefin and maleic anhydride product, which can be used to enhance the toughness and impact resistance of the polymer, thereby enhancing the toughness and impact strength, and the toughness and impact resistance of the polymer, especially the toughness and toughness of the polymer, thereby enhancing the toughness and impact resistance of the polymer.

CN117924917BActive Publication Date: 2024-12-03APALENE TECHNOLOGY CO LTD (SHANGHAI)
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202311795789.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-12-25
Publication Date
2024-12-03
Estimated Expiration
2043-12-25

AI Technical Summary

Technical Problem

Epoxy resin and nylon polymers exhibit high brittleness and poor impact resistance, limiting their application in high-impact and high-toughness environments, while alpha olefin coordination oligomers with vinylidene groups are underutilized as they are often discarded as waste due to low molecular weight and low viscosity.

Method used

A pericyclic reaction between 1,1-disubstituted olefins and maleic anhydride produces an anhydride product that acts as a reactive toughening agent, grafting onto epoxy resin and polyamide molecules, introducing flexible side chains to enhance toughness and impact strength.

Benefits of technology

The anhydride product of the reactive toughening agent, which is a reactive toughening agent, which can be used as a reactive toughening agent, which can be used to enhance the toughness and impact strength, and the toughness and impact strength of the polymer, thereby enhancing the toughness and impact resistance of the polymer, especially at low temperatures.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure FT_1
    Figure FT_1
  • Figure FT_2
    Figure FT_2
  • Figure FT_3
    Figure FT_3
Patent Text Reader

Abstract

The present invention provides a toughened nylon composition and its preparation and use. The toughened nylon composition comprises a nylon resin, a main toughening agent, a reactive toughening agent and a processing aid; wherein the reactive toughening agent is a 1,1-disubstituted olefin anhydride product. The toughened nylon composition prepared by the method provided by the present invention can be widely used in the fields of automobiles, electronic appliances, transportation, machinery and instruments.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of polymer materials, and in particular relates to a toughened nylon composition and a preparation method and application thereof. Background Art

[0002] Epoxy resin is the main polymer in thermosetting resin. Before curing, epoxy resin contains highly chemically active functional groups such as epoxy groups and hydroxyl groups. A suitable curing agent is selected to cross-link it to form a three-dimensional network structure. After curing, epoxy resin has the characteristics of small deformation shrinkage, high tensile strength and modulus, and good chemical stability. Therefore, it is widely used in the field of electronic appliances, such as electronic appliance adhesives, PCB circuit board coating glue, laminates, potting glue, etc., and is particularly suitable for structural bonding between electronic devices or components. However, the cross-linking density of epoxy resin after curing is high, the internal stress is large, and most of the molecular chain segments are non-rotatable rigid segments, which leads to high brittleness of epoxy resin cured products, poor impact resistance, and easy cracking and brittle fracture, which limits the application of epoxy resin in high impact resistance and high toughness occasions. Therefore, improving the toughness of epoxy resin cured products has become a research hotspot.

[0003] Polyamide (nylon) is a widely used thermoplastic polymer with good mechanical properties, heat resistance, wear resistance, chemical solvent resistance, self-lubrication and certain flame retardancy. It has excellent processing performance and can be integrated into complex structural parts. It is widely used in the fields of automobiles, electronic appliances, transportation, machinery and instrumentation. However, nylon also has obvious defects, which are poor impact resistance and obvious brittleness at low temperatures. In particular, the notched impact strength at ultra-low temperatures below -40°C can generally only reach 10%-20% of the room temperature impact strength. The defect of insufficient toughness has hindered the development and application of nylon.

[0004] Therefore, for engineering plastics such as nylon and adhesives such as epoxy resin, they need to try to reduce brittleness, increase toughness, and improve impact resistance during use, especially impact resistance at low temperatures.

[0005] Metallocene-catalyzed alpha olefins can be used to prepare a series of polyalphaolefins (PAO) with different polymerization degrees through coordination polymerization. PAO is usually used to manufacture lubricating base oils, base oils and other products. Its coordination polymerization process follows the Cossee-Arlman chain growth mechanism. When the polymerization target is low-viscosity products, it is inevitable to generate a series of alpha olefin coordination oligomers from dimers, trimers, tetramers to polymers with higher polymerization degrees. Among these oligomers, alpha olefin dimers with a polymerization degree of 2 are light component products. Due to their low molecular weight and low viscosity, they are difficult to be directly used in lubricating base oils. They are often considered to be waste formed in the production process of PAO and have low market utilization value. However, this part of the product has a high content of vinylidene (also known as: 1,1-disubstituted vinyl). If it is directly burned as fuel oil, its value is not fully utilized, and it is also a waste of raw material alpha olefins.

[0006] There are many existing technologies for reacting highly active vinylidene groups in α-olefin coordination oligomers and introducing functional groups. Patent EP1792900A1 proposes using H2O2 / HCOOH to react with α-olefin dimers with vinylidene groups to obtain 1,2-diols with good yields. The diols are converted into corresponding aldehydes through acid-catalyzed rearrangement, and then reacted with 1,2-diols to obtain dioxane derivatives. Ether oxygen is introduced into α-olefin dimers as polar units, thereby improving the solubility of PAO in lubricant additives. Patent EP1908746A1 proposes using polyacids of metal oxygen-containing acids as catalysts to perform acid rearrangement reactions on the basis of α-olefin dimer epoxides to obtain aldehydes of 2-position branched long-chain alkyl groups. Patent US20150275127A1 mentions the use of tetramethyl disiloxane and α-olefin dimer to carry out hydrosilylation reaction under the action of platinum catalyst, thereby obtaining low-viscosity, low-volatility alkylated siloxane compounds. Such compounds have relatively high polarity and can be added to lubricating oils to improve the solubility and dispersibility of polar additives in lubricating oils. It can be seen that the existing technology for the application of functionalized α-olefin coordination oligomers is mostly concentrated in the field of lubricants, and its application in other fields is very rare. Summary of the invention

[0007] The inventors have found that the product obtained by the grafting reaction of 1,1-disubstituted vinyl groups of α-olefin coordination oligomers including α-olefin dimers with maleic anhydride can be used as a reactive toughening agent. The anhydride group can react with the epoxy group to participate in the curing of epoxy resin, and can also react with the amino group at the end of the polyamide molecule to be grafted on the polyamide molecule. At the same time, the α-olefin coordination oligomer has a degree of polymerization of 2-4, and there is a branched structure in the molecule, which can provide a flexible side chain, which is grafted on the polymer through the reactive anhydride, thereby improving the branching degree and the molecular chain mobility of the polymer, thereby improving the toughness and impact strength of the polymer, especially the impact strength at low temperatures.

[0008] To achieve the above technical objectives, the present invention provides a 1,1-disubstituted olefin anhydride product, its preparation and use; a curable epoxy resin composition using the 1,1-disubstituted olefin anhydride product as a reactive toughening agent, and a curing method and product thereof; and a toughened nylon composition using the 1,1-disubstituted olefin anhydride product as a reactive toughening agent, and its preparation and use.

[0009] The present invention includes the following technical solutions:

[0010] In the first aspect, a 1,1-disubstituted olefin anhydride product is provided, the general structural formula of which is shown in Formula I:

[0011]

[0012] Wherein, R0 of the compound of formula I is a straight chain or branched hydrocarbon group with 10 to 50 carbon atoms, preferably, R0 is a straight chain or branched hydrocarbon group with 11 to 23 carbon atoms.

[0013] Preferably, the 1,1-disubstituted olefin molecule contains at least one vinylidene (also known as vinylidene or 1,1-disubstituted vinyl, English: Vinylidene) double bond.

[0014] Preferably, the 1,1-disubstituted olefin is selected from alpha olefin coordination oligomers, which are obtained by polymerization of a metallocene catalyst system and one or more linear alpha olefins, wherein the number of carbon atoms of the linear alpha olefin is 5-20, wherein the source of the linear alpha olefin includes alpha olefins obtained by homopolymerization of low-carbon olefins, Fischer-Tropsch alpha olefins and ethylene oligomerization alpha olefins. The metallocene catalyst system comprises at least one metallocene catalyst, which is an inorganic-organic complex containing at least one cyclopentadienyl or cyclopentadienyl derivative as a ligand and at least one Group IVB transition element as a central atom.

[0015] Preferably, the α-olefin coordination oligomer structure is selected from:

[0016] Any one or more combinations of , where the value range of n is 3-17.

[0017] In a second aspect, the preparation method of the above-mentioned 1,1-disubstituted olefin anhydride product comprises: obtaining the product by a pericyclic reaction of 1,1-disubstituted olefin and maleic anhydride.

[0018] Preferably, the pericyclic reaction is a thermally induced pericyclic reaction, wherein the pericyclic reaction is a pericyclic reaction between the π bond of the carbon-carbon double bond of maleic anhydride and the σ bond of the α-position carbon-hydrogen bond of the vinylidene group of 1,1-disubstituted olefin, whereby the original double bond is displaced and a new carbon-hydrogen bond and carbon-carbon double bond are generated.

[0019] The specific steps of the preparation method include: mixing 1,1-disubstituted olefin and maleic anhydride, maintaining the mixture at a certain reaction temperature for a certain period of time, and then separating and purifying the mixture.

[0020] Preferably, a polymerization inhibitor is added during the reaction to prevent the reactants with double bonds from forming free radicals and undergoing free radical polymerization. The polymerization inhibitor is preferably hydroquinone and / or p-hydroxyanisole.

[0021] Preferably, the reaction temperature is at least 120°C, and more preferably, the reaction temperature is 160-220°C.

[0022] Preferably, the time is 8 to 48 hours, more preferably, the time is 16 to 48 hours.

[0023] The specific steps of separation and purification include: cooling and diluting with an inert solvent, adding a filter aid and filtering, evaporating the filtrate to remove the inert solvent, and distilling the residue under reduced pressure to obtain the product.

[0024] Preferably, the inert solvent is petroleum ether, and the filter aid is white clay.

[0025] The synthetic route of the anhydride product of 1,1-disubstituted olefins is as follows:

[0026]

[0027] Wherein, R1 and R2 are straight-chain or branched alkyl groups with 4 to 24 carbon atoms, R0 is a straight-chain or branched hydrocarbon group with 10 to 50 carbon atoms, and preferably, R0 is a straight-chain or branched hydrocarbon group with 11 to 23 carbon atoms.

[0028] In a third aspect, the anhydride product of the 1,1-disubstituted olefin described above is used as a reactive toughening agent in polymer toughening.

[0029] In a fourth aspect, a curable epoxy resin composition comprises:

[0030] Component A, epoxy resin prepolymer; component B, curing agent; component C, reactive toughening agent.

[0031] Wherein, the reactive toughening agent is selected from the above-mentioned 1,1-disubstituted olefin anhydride product, whose structure is as described above, and the amount of the reactive toughening agent is 1 to 15wt% of the epoxy resin prepolymer. Preferably, the amount of the reactive toughening agent is 1 to 10wt% of the epoxy resin prepolymer, and more preferably, the amount of the reactive toughening agent is 3 to 8wt% of the epoxy resin prepolymer.

[0032] Wherein, the curing agent is selected from any one of an amine curing agent and an acid anhydride curing agent, and the amount of the curing agent is Wherein, RGEW is the reactive group equivalent weight in the curing agent that can react with the epoxy group, EEW is the epoxy equivalent weight of the epoxy resin prepolymer, and c is the correction coefficient, and the value range of c is 0.6 to 1.1.

[0033] For example, the amount of amine curing agent used is epoxy resin prepolymer The amount of anhydride curing agent is Wherein, AHEW is the active hydrogen equivalent of the amine curing agent, EEW is the epoxy equivalent of the epoxy resin prepolymer, and AAEW is the anhydride equivalent of the anhydride curing agent.

[0034] Furthermore, M CA is the relative molecular mass of the curing agent, It is the average number of reactive groups per molecule of curing agent that can react with epoxy groups.

[0035] Furthermore, the epoxy resin composition also includes: a curing accelerator, the amount of the curing accelerator is 0.1 to 1 wt% of the total amount of the epoxy resin composition; wherein the curing accelerator is selected from: one or more combinations of phenolic accelerators, imidazole accelerators, amine accelerators, and Lewis acid accelerators.

[0036] Furthermore, phenolic accelerators include: phenol, resorcinol, nonylphenol, bisphenol A and 2,4,6-tris(dimethylaminomethyl)phenol, etc., amine accelerators include: o-hydroxybenzyldimethylamine, triethylamine, triethanolamine, benzyldimethylamine and alkyltrimethylammonium bromide salts, etc., imidazole accelerators include: 2-methylimidazole and 2-phenylimidazole, etc., Lewis acid accelerators include: BF3, SnCl4, AlCl3, FeCl3, TiCl4 and ZnCl2, etc.

[0037] Among them, the epoxy resin prepolymer is selected from: one or more combinations of bisphenol A epoxy resin, bisphenol F epoxy resin, polyphenol glycidyl ether epoxy resin, aliphatic glycidyl ether epoxy resin, glycidyl ester epoxy resin, glycidyl amine epoxy resin, alicyclic epoxy resin, cyanuric acid triglycidyl epoxy resin, and hydantoin epoxy resin. Furthermore, each molecule of the epoxy resin prepolymer contains at least 2 epoxy groups.

[0038] Preferably, the epoxy resin prepolymer is a bisphenol A epoxy resin, wherein m=0-25, and the epoxy resin prepolymer is composed of compounds with different polymerization degrees. When m=0, the epoxy resin prepolymer does not have a repeating structure, and its structural formula is shown in Formula II:

[0039]

[0040] In a fifth aspect, a method for curing the curable epoxy resin composition described above comprises:

[0041] S1, mixing and stirring the epoxy resin prepolymer, curing agent and reactive toughening agent in the formula, and placing the mixture at a temperature of T1 to degas the mixture;

[0042] S2, heating the deaerated mixture to T2 temperature and maintaining it for 1-3 hours;

[0043] S3, heating the deaerated mixture to T3 temperature and maintaining it for 1-3 hours;

[0044] Preferably, 40°C≤T1≤140°C, 60°C≤T2≤170°C, 80°C≤T3≤220°C, wherein T1<T2<T3;

[0045] Preferably, the degassing treatment is a vacuum degassing treatment, which is carried out in a vacuum drying oven.

[0046] Preferably, in step S1, the curing accelerator in the formula is mixed and stirred evenly with the epoxy resin prepolymer, the curing agent and the reactive toughening agent.

[0047] Preferably, in step S2, before heating, the mixture is poured into a preheated mold for molding.

[0048] A sixth aspect is a cured colloid, characterized in that it is obtained by curing the curable epoxy resin composition described above.

[0049] Seventhly, the above-mentioned curing colloid is used in electronic and electrical adhesives, PCB circuit board coating glue, potting glue, and coatings.

[0050] In an eighth aspect, a toughened nylon composition comprises the following components in parts by weight: 70-90 parts of nylon resin, 5-15 parts of a primary toughening agent, 1-10 parts of a reactive toughening agent, and 1-10 parts of a processing aid;

[0051] Among them, the main toughening agent is selected from maleic anhydride grafted polyolefin resin or elastomer, and further, the main toughening agent is selected from maleic anhydride grafted polyethylene (PE-g-MAH), maleic anhydride grafted polypropylene (PP-g-MAH), maleic anhydride grafted polyolefin elastomer (POE-g-MAH), maleic anhydride grafted ethylene propylene diene rubber (EPDM-g-MAH) and maleic anhydride grafted ethylene vinyl acetate (EVA-g-MAH).

[0052] The reactive toughening agent is selected from the above-mentioned 1,1-disubstituted olefin anhydride products, and the structure thereof is as described above.

[0053] In a ninth aspect, the method for preparing the toughened nylon composition described above comprises: premixing the nylon resin, the main toughening agent, the reactive toughening agent and the processing aid, melt-mixing by a twin-screw, cooling and pelletizing to obtain the composition.

[0054] A tenth aspect is the application of the toughened nylon composition described above in the fields of automobiles, electronic appliances, transportation, machinery and instrumentation.

[0055] The beneficial effect of the present invention is that: by carrying out a pericyclic reaction between 1,1-disubstituted olefin and maleic anhydride, an anhydride product of 1,1-disubstituted olefin is obtained, namely maleic anhydride grafted 1,1-disubstituted olefin, wherein the 1,1-disubstituted olefin includes a light component byproduct formed in the coordination polymerization process of alpha olefin: alpha olefin coordination oligomer, thereby expanding the application field of alpha olefin coordination oligomer and improving its utilization value.

[0056] Maleic anhydride grafted 1,1-disubstituted olefins contain highly reactive anhydride groups, which can be used as reactive toughening agents. The anhydride groups can react with epoxy groups to participate in epoxy resin curing, and can also react with amino groups at the ends of polyamide molecules to be grafted onto polyamide molecules. After the reaction, a series of flexible side chains of different lengths are introduced into the polymer, and the crosslinking density or crystallinity of the system is reduced through the physical entanglement between the long side chains. In addition, the long side chain segments have higher mobility, which reduces the stress concentration effect. When subjected to external forces, they can absorb energy and have a toughening effect on the polymer. BRIEF DESCRIPTION OF THE DRAWINGS

[0057] Figure 1 C6 dimer 1 H-NMR spectrum.

[0058] Figure 2 C6 trimer 1 H-NMR spectrum.

[0059] Figure 3 C6 tetramer 1 H-NMR spectrum.

[0060] Figure 4 C8 dimer 1 H-NMR spectrum.

[0061] Figure 5 C8 trimer 1 H-NMR spectrum.

[0062] Figure 6 C10 dimer 1 H-NMR spectrum.

[0063] Figure 7 C12 dimer 1H-NMR spectrum.

[0064] Figure 8 This is the GC spectrum of the orange-yellow fraction obtained in Example 1.

[0065] Figure 9-14 The MS spectra corresponding to each GC peak of the orange-yellow fraction obtained in Example 1 (peak groups 1-6).

[0066] Fig.15 Example 2 Initial reaction mixture 1 H-NMR spectrum.

[0067] Fig.16 , 17 The orange-yellow fraction obtained in Example 2 1 H-NMR and 13 C-NMR spectrum.

[0068] Fig.18 , 19 The brown resinous residue obtained in Example 2 1 H-NMR and 13 C-NMR spectrum.

[0069] Fig. 20 This is the GC spectrum of the orange-yellow fraction obtained in Example 5.

[0070] Figure 21-24 The MS spectra corresponding to each GC peak of the orange-yellow fraction obtained in Example 5 (peak groups 1-4).

[0071] Fig.25 These are scanning electron microscope images of the fracture surfaces of epoxy resin cured colloid tensile test samples, where (a) is Comparative Example 1, (b) is Example 9-2, (c) is Example 9-3, and (d) is Example 9-5. DETAILED DESCRIPTION

[0072] It should be noted that the following detailed descriptions are exemplary and are intended to provide further explanation of the present invention. Unless otherwise specified, all technical and scientific terms used in the present invention have the same meanings as those commonly understood by those skilled in the art to which the present invention belongs.

[0073] It should be noted that the terms used herein are only for describing specific embodiments and are not intended to limit exemplary embodiments according to the present invention. As used herein, unless the context clearly indicates otherwise, the singular form is also intended to include the plural form. In addition, it should be understood that when the terms "comprising" and / or "including" are used in this specification, it indicates the presence of features, steps, operations, devices, components and / or combinations thereof.

[0074] If the specific experimental conditions are not specified in the examples, they are usually based on the conventional conditions in the field or the conditions recommended by the reagent company; the materials, reagents, etc. used in the examples can be purchased through commercial channels unless otherwise specified.

[0075] Preparation of α-olefin coordination oligomers: Preparation was carried out according to the method of patent application No. 202310825467.9, and the metallocene main catalyst used was [t-BuN(Me)2C(η 5 -C5H4)]-ZrCl2, cocatalyst methylaluminoxane MAO, thereby preparing 1-C6 / 1-C8 / 1-C10 / 1-C12 linear alpha olefin oligomers C6 dimer, C6 trimer, C6 tetramer, C8 dimer, C8 trimer, C10 dimer, C12 dimer, and separating them by collecting specific fractions through vacuum distillation. The specific separation conditions are shown in Table 1. 1 H-NMR structural characterization, the results are listed in Figure 1-7 .

[0076] go through 1 From the chemical shifts at 4.60 to 4.90 in the H-NMR spectrum, it can be seen that the unsaturated double bonds in the α-olefin coordination oligomers are mainly vinylidene (1,1-disubstituted vinyl, vinylidene) structures, and the shift peaks between 5.0 and 5.7 are very inconspicuous, indicating that the content of vinyl (vinyl) and 1,1,2-trisubstituted vinyl in the α-olefin coordination oligomers is extremely small.

[0077] Table 1

[0078] Oligomer Molecular formula Separation conditions Corresponding structure and spectral characterization C6 dimer <![CDATA[C 12 H 24 ]]> 7mmHg collect 70~90℃ fraction Figure 1 C6 trimer <![CDATA[C 18 H 36 ]]> 0.5mmHg collect 95~120℃ fraction Figure 2 C6 tetramer <![CDATA[C 24 H 48 ]]> 0.2mmHg collect 120~150℃ fraction Figure 3 C8 dimer <![CDATA[C 16 H 32 ]]> 0.8mmHg collect 100~125℃ fraction Figure 4 C8 trimer <![CDATA[C 24 H 48 ]]> 0.5mmHg collect 140~170℃ fraction Figure 5 C10 dimer <![CDATA[C 20 H 40 ]]> 0.5mmHg collect 110~135℃ fraction Figure 6 C12 dimer <![CDATA[C 24 H 48 ]]> 0.2mmHg collect 110~130℃ fraction Figure 7

[0079] Example 1

[0080] 25.25 g (150 mmol) of C6 dimer, 18.39 g (187.5 mmol) of maleic anhydride and 0.25 g of inhibitor p-hydroxyanisole were added to a 250 mL round-bottom flask. After installing a condensing reflux tube, the air in the system was replaced with nitrogen three times. The temperature of the magnetic stirrer was then set to 180 ° C. The reaction was completed after heated and stirred for 21 hours. After the reactant was cooled to room temperature, 100 mL of petroleum ether and 10 g of carclazyte were added. After stirring for 5 minutes, the filtrate was concentrated by rotary evaporator to remove excess maleic anhydride. The residue was distilled under reduced pressure (9 mmHg / 290 ° C) to obtain 35.61 g of an orange-yellow fraction (yield 89.1%) and a small amount of viscous brown resinous residue.

[0081] The orange-yellow fraction was tested by GC-MS and found to have 6 groups of peaks in GC. The retention time, peak area ratio and corresponding MS molecular ion peak of each group of peaks are shown in Table 2. It can be confirmed that the molecular formula of the reactive toughening agent is C 16 H 26 O3, consists of 6 isomers.

[0082] Table 2

[0083] Peak Retention time / min Peak area ratio / % MS molecular ion peak 1 8.20 3.02 266 2 8.33 8.07 266 3 8.52 36.65 266 4 8.61 30.14 266 5 8.99 4.83 266 6 9.09 17.29 266

[0084] Example 2

[0085] 25.25 g (150 mmol) of C6 dimer and 18.39 g (187.5 mmol) of maleic anhydride were added to a 250 mL round-bottom flask. After installing a condensing reflux tube, the air in the system was replaced with nitrogen three times. Then the temperature of the magnetic stirrer was set to 180°C. After heating and stirring for 21 hours, the reaction was terminated. After the reactants were cooled to room temperature, 100 mL of petroleum ether and 10 g of white clay were added. After stirring for 5 minutes, the filtrate was filtered and concentrated by a rotary evaporator. The residue was distilled under reduced pressure (9 mmHg / 290°C) to obtain 16.79 g of an orange-yellow fraction (yield 42.0%) and 22.74 g of a viscous brown resinous residue. The unreacted C6 dimer and maleic anhydride mixture, the orange-yellow fraction and the brown resinous residue were sampled and analyzed. 1 H-NMR (solvent CDCl3) structural characterization, the orange-yellow fraction and the brown resinous residue were sampled and 13 C-NMR (solvent CDCl3) structural characterization. The results are listed in Figure 15-19 .

[0086] Example 3

[0087] 37.88g (150mmol) C6 trimer, 18.39g (187.5mmol) maleic anhydride and 0.25g inhibitor p-hydroxyanisole are added to a 250mL round-bottomed flask, after installing the condensing reflux pipe, the air in the system is replaced with nitrogen three times, then the magnetic stirring device temperature is set to 190°C, and the reaction is terminated after heated stirring for 21 hours. After the reactant is cooled to room temperature, 100mL petroleum ether and 10g carclazyte are added, and suction filtration is performed after stirring for 5 minutes. The filtrate is concentrated by a rotary evaporator, and the residue is distilled under reduced pressure (9mmHg / 290°C) to obtain an orange-yellow fraction 43.54g (yield 82.8%) and a small amount of brown resinous residue. Wherein the orange-yellow fraction is found to have 4 groups of peaks in GC through GC-MS testing, and the retention time of each group of peaks, the peak area ratio and the molecular ion peak of the corresponding MS are as shown in Table 3, thus it can be confirmed that the molecular formula of the reactive toughening agent is C 22 H 38O3, consists of 4 isomers.

[0088] Table 3

[0089] Peak Retention time / min Peak area ratio / % MS molecular ion peak 1 14.67 8.18 350 2 14.95 9.70 350 3 15.12 46.98 350 4 15.46 35.14 350

[0090] Example 4

[0091] 50.49g (150mmol) C6 tetramer, 18.39g (187.5mmol) maleic anhydride and 0.25g inhibitor p-hydroxyanisole are added to a 250mL round-bottomed flask, after installing the condensing reflux pipe, the air in the system is replaced with nitrogen three times, then the magnetic stirring device temperature is set to 190°C, and the reaction is terminated after heated stirring for 21 hours. After the reactant is cooled to room temperature, 100mL petroleum ether and 10g carclazyte are added, and suction filtration is performed after stirring for 5 minutes. The filtrate is concentrated by a rotary evaporator, and the residue is distilled under reduced pressure (9mmHg / 290°C) to obtain orange-yellow fraction 49.28g (yield 75.6%) and a small amount of brown resinous residue. Wherein the orange-yellow fraction is tested by GC-MS and 6 groups of peaks are found in GC, and the retention time of each group of peaks, the peak area ratio and the molecular ion peak of the corresponding MS are as shown in Table 4, and thus it can be confirmed that the molecular formula of the reactive toughening agent is C 28 H 50 O3, consists of 6 isomers.

[0092] Table 4

[0093] Peak Retention time / min Peak area ratio / % MS molecular ion peak 1 20.84 2.04 434 2 21.17 5.83 434 3 21.38 45.33 434 4 21.76 37.38 434 5 21.90 7.50 434 6 22.05 1.92 434

[0094] Example 5

[0095] 33.66g (150mmol) C8 dimer, 18.39g (187.5mmol) maleic anhydride and 0.25g inhibitor p-hydroxyanisole are added to a 250mL round-bottomed flask, after installing the condensing reflux pipe, the air in the system is replaced with nitrogen three times, then the magnetic stirring device temperature is set to 180°C, and the reaction is terminated after heated stirring for 21 hours. After the reactant is cooled to room temperature, 100mL petroleum ether and 10g carclazyte are added, and suction filtration is performed after stirring for 5 minutes. The filtrate is concentrated by a rotary evaporator, and the residue is distilled under reduced pressure (9mmHg / 290°C) to obtain orange-yellow fraction 41.35g (yield 85.5%) and a small amount of brown resinous residue. Wherein the orange-yellow fraction is tested by GC-MS and 4 groups of peaks are found in GC. The retention time of each group of peaks, the peak area ratio and the molecular ion peak of the corresponding MS are as shown in Table 5, and thus it can be confirmed that the molecular formula of the reactive toughening agent is C 20 H 34 O3, consists of 4 isomers.

[0096] Table 5

[0097] Peak Retention time / min Peak area ratio / % MS molecular ion peak 1 11.84 5.85 322 2 11.96 4.47 322 3 12.25 50.74 322 4 12.70 38.94 322

[0098] Example 6

[0099] 50.49g (150mmol) C8 trimer, 18.39g (187.5mmol) maleic anhydride and 0.25g inhibitor p-hydroxyanisole are added to a 250mL round-bottomed flask, after installing the condensing reflux pipe, the air in the system is replaced with nitrogen three times, then the magnetic stirring device temperature is set to 180°C, heated and stirred for 21 hours and the reaction is terminated, after the reactant is cooled to room temperature, 100mL petroleum ether and 10g carclazyte are added, suction filtration is performed after stirring for 5 minutes, and the filtrate is concentrated by a rotary evaporator, and the residue is distilled under reduced pressure (9mmHg / 290°C) to obtain orange-yellow fraction 46.78g (yield 71.7%) and a small amount of brown resinous residue. Wherein the orange-yellow fraction is found to have 4 groups of peaks in GC through GC-MS test, and the retention time of each group of peaks, peak area ratio and the molecular ion peak of corresponding MS are as shown in Table 6, thus it can be confirmed that the molecular formula of the reactive toughening agent is C 28 H 50 O3, consists of 4 isomers.

[0100] Table 6

[0101] Peak Retention time / min Peak area ratio / % MS molecular ion peak 1 21.25 3.99 434 2 21.56 6.57 434 3 21.89 47.84 434 4 22.18 41.60 434

[0102] Example 7

[0103] 42.08g (150mmol) C10 dimer, 18.39g (187.5mmol) maleic anhydride and 0.25g inhibitor p-hydroxyanisole are added to a 250mL round-bottomed flask, after installing the condensing reflux pipe, the air in the system is replaced with nitrogen three times, then the magnetic stirring device temperature is set to 180°C, heated and stirred for 21 hours and the reaction is terminated, after the reactant is cooled to room temperature, 100mL petroleum ether and 10g carclazyte are added, suction filtration is performed after stirring for 5 minutes, and the filtrate is concentrated by a rotary evaporator, and the residue is distilled under reduced pressure (9mmHg / 290°C), and an orange-yellow fraction 45.27g (yield 79.7%) and a small amount of brown resinous residue are obtained. Wherein the orange-yellow fraction is tested by GC-MS and 4 groups of peaks are found to occur in GC, and the retention time of each group of peaks, the peak area ratio and the molecular ion peak of the corresponding MS are as shown in Table 7, thus it can be confirmed that the molecular formula of the reactive toughening agent is C 24 H 42 O3, consists of 4 isomers.

[0104] Table 7

[0105] Peak Retention time / min Peak area ratio / % MS molecular ion peak 1 17.54 6.26 378 2 17.86 7.78 378 3 18.09 40.36 378 4 18.42 45.60 378

[0106] Example 8

[0107] 50.49g (150mmol) C12 dimer, 18.39g (187.5mmol) maleic anhydride and 0.25g inhibitor p-hydroxyanisole are added to a 250mL round-bottomed flask, after installing the condensing reflux pipe, the air in the system is replaced with nitrogen three times, then the magnetic stirring device temperature is set to 180°C, heated and stirred for 21 hours and the reaction is terminated, after the reactant is cooled to room temperature, 100mL petroleum ether and 10g carclazyte are added, suction filtration is performed after stirring for 5 minutes, and the filtrate is concentrated by a rotary evaporator, and the residue is distilled under reduced pressure (9mmHg / 290°C), and orange-yellow fraction 52.93g (yield 81.2%) and a small amount of brown resinous residue are obtained. Wherein the orange-yellow fraction is tested by GC-MS and 4 groups of peaks are found in GC, and the retention time of each group of peaks, the peak area ratio and the molecular ion peak of the corresponding MS are as shown in Table 8, thus it can be confirmed that the molecular formula of the reactive toughening agent is C 28 H 50 O3, consists of 4 isomers.

[0108] Table 8

[0109] Peak Retention time / min Peak area ratio / % MS molecular ion peak 1 20.71 4.03 434 2 21.02 5.81 434 3 21.35 39.44 434 4 21.77 50.72 434

[0110] The kinematic viscosity (Kv) of the orange-yellow fractions of Examples 1-8 at 40°C and 100°C, and the kinematic viscosity of the viscous brown resinous residue obtained in Example 2 were measured using a SVM 2001 kinematic viscosity meter. The results are shown in Table 9.

[0111] Table 9

[0112] product Yield <![CDATA[Kv@40℃(mm 2 / s)]]> <![CDATA[Kv@100℃(mm 2 / s)]]> Example 1 89.1% 4.13 32.81 Example 2 42.0% 4.25 33.16 Example 2 Viscous residue - 34.03 1044 Example 3 82.8% 5.87 44.25 Example 4 75.6% 7.69 68.33 Example 5 85.5% 5.36 38.16 Example 6 71.7% 7.51 66.46 Example 7 79.7% 6.40 50.52 Example 8 81.2% 7.44 64.80

[0113] As can be seen from the above table, the viscous resinous residue at the bottom of the flask after the reaction is completed is significantly different from the kinematic viscosity of the orange-yellow fraction obtained by vacuum distillation. The orange-yellow fraction is the product of the cycloaddition reaction of maleic anhydride and α-olefin coordination oligomers, while the viscous resinous residue is a polymer obtained by free radical polymerization of maleic anhydride and α-olefin coordination oligomers, which has a higher kinematic viscosity than the cycloaddition product. By comparing Example 1 with Example 2, it can be seen that by adding an inhibitor to the reactants, free radical polymerization can be avoided to form a viscous resinous residue, and a higher yield of cycloaddition reaction products can be obtained.

[0114] At the same time, through Figure 15-19From the structural characterization, it can be seen that the orange-yellow fraction obtained by vacuum distillation in Example 2 is compared with the reaction mixture that has not started the reaction. It can be seen that the initial reaction mixture has a vinylidene peak of 4.60 to 4.90 and a double bond peak near the carbonyl group of about 7.0. After the reaction, the orange-yellow fraction has an intramolecular double bond peak of 5.0 to 5.5, including two double bonds of 1,2-disubstituted vinyl and 1,1,2-trisubstituted vinyl. It can be inferred that the process of the cycloaddition reaction is the reaction of the vinylidene of the α-olefin coordination oligomer with the double bond near the carbonyl group of maleic anhydride. From the structural characterization of the brown viscous resin residue at the bottom of the flask, the peak shapes of the hydrogen spectrum and the carbon spectrum have been significantly broadened, and the double bond peak between the chemical shifts of 100 and 150 of the carbon spectrum has disappeared, indicating that the brown viscous resin residue at the bottom of the flask is formed by the polymerization reaction between maleic anhydride and the carbon-carbon double bonds of the α-olefin coordination oligomer, rather than a cycloaddition reaction.

[0115] The invention discloses a curable epoxy resin composition using E-44 bisphenol A epoxy resin as a main resin and methylhexahydrophthalic anhydride (MeHHPA) as a curing agent, which can be used for impregnation of coils of electrical equipment, casting of electrical components and sealing of semiconductors. Maleic anhydride-grafted 1,1-disubstituted olefin is added to the curing agent MeHHPA as a reactive toughening agent, and 2,4,6-tris(dimethylaminomethyl)phenol (DMP-30) is used as a curing accelerator.

[0116] Example 9-1: Formula of curable epoxy resin composition: 100 parts by mass of E-44 epoxy resin (epoxy value 0.44, epoxy equivalent 227), 59.2 parts by mass of MeHHPA (anhydride equivalent 168), 5.9 parts by mass of maleic anhydride grafted 1,1-disubstituted olefin of Example 1, and 0.3 parts by mass of DMP-30.

[0117] Example 9-2: Formula of curable epoxy resin composition: 7.7 parts by mass of maleic anhydride grafted 1,1-disubstituted olefin of Example 3, and the rest is the same as Example 9-1.

[0118] Example 9-3: Formula of curable epoxy resin composition: 9.6 parts by mass of maleic anhydride grafted 1,1-disubstituted olefin of Example 4, and the rest is the same as Example 9-1.

[0119] Example 9-4: Formula of curable epoxy resin composition: 7.1 parts by mass of maleic anhydride grafted 1,1-disubstituted olefin of Example 5, and the rest is the same as Example 9-1.

[0120] Example 9-5: Formula of curable epoxy resin composition: 9.6 parts by mass of maleic anhydride grafted 1,1-disubstituted olefin of Example 6, and the rest is the same as Example 9-1.

[0121] Example 9-6: Formula of curable epoxy resin composition: 8.3 parts by mass of maleic anhydride grafted 1,1-disubstituted olefin of Example 7, and the rest is the same as Example 9-1.

[0122] Example 9-7: Formula of curable epoxy resin composition: 9.6 parts by mass of maleic anhydride grafted 1,1-disubstituted olefin of Example 8, and the rest is the same as Example 9-1.

[0123] Comparative Example 1: Formula of curable epoxy resin composition: 100 parts by mass of E-44 epoxy resin (epoxy value 0.44, epoxy equivalent 227), 62.9 parts by mass of MeHHPA (anhydride equivalent 168), and 0.3 parts by mass of DMP-30.

[0124] The curing procedure of Example 9 and Comparative Example 1 is as follows: the components of the curable epoxy resin composition are mixed and stirred evenly, placed in a vacuum drying oven at 80°C for degassing for 15 minutes, then poured into a preheated stainless steel mold, and cured at 150°C for 2 hours, and then continued to heat to 190°C for curing for 2 hours to obtain a cured epoxy resin colloid.

[0125] The curable epoxy resin composition with E-51 bisphenol A epoxy resin as the main resin and 4,4'-diaminodiphenyl sulfone (DDS) as the curing agent can be used for castings, laminates and adhesives. The cured epoxy resin has excellent thermal stability and outstanding chemical stability, but poor flexibility. Maleic anhydride grafted 1,1-disubstituted olefin is added to the curing agent DDS as a reactive toughening agent.

[0126] Example 10-1 The formula of the curable epoxy resin composition: 100 parts by mass of E-51 epoxy resin (epoxy value 0.51, epoxy equivalent 196), 30 parts by mass of DDS (active hydrogen equivalent 62), and 5.9 parts by mass of the maleic anhydride grafted 1,1-disubstituted olefin of Example 1.

[0127] Example 10-2: Formula of curable epoxy resin composition: 7.7 parts by mass of maleic anhydride grafted 1,1-disubstituted olefin of Example 2, and the rest is the same as Example 10-1.

[0128] Example 10-3: Formula of curable epoxy resin composition: 9.6 parts by mass of maleic anhydride grafted 1,1-disubstituted olefin of Example 3, and the rest is the same as Example 10-1.

[0129] Example 10-4: Formula of curable epoxy resin composition: 7.1 parts by mass of maleic anhydride grafted 1,1-disubstituted olefin of Example 4, and the rest is the same as Example 10-1.

[0130] Example 10-5: Formula of curable epoxy resin composition: 9.6 parts by mass of maleic anhydride grafted 1,1-disubstituted olefin of Example 5, and the rest is the same as Example 10-1.

[0131] Example 10-6 The formula of the curable epoxy resin composition: 8.3 parts by mass of the maleic anhydride grafted 1,1-disubstituted olefin of Example 6, and the rest are the same as Example 10-1.

[0132] Example 10-7 The formula of the curable epoxy resin composition: 9.6 parts by mass of the maleic anhydride grafted 1,1-disubstituted olefin of Example 7, and the rest are the same as Example 10-1.

[0133] Comparative Example 2: Formula of curable epoxy resin composition: 100 parts by mass of E-51 epoxy resin (epoxy value 0.51, epoxy equivalent 196), and 31.6 parts by mass of DDS (active hydrogen equivalent 168).

[0134] The curing procedure of Example 10 and Comparative Example 1 is as follows: the components of the curable epoxy resin composition are mixed and stirred evenly, placed in a vacuum drying oven at 120°C for degassing for 15 minutes, then poured into a preheated stainless steel mold, and cured at 150°C for 2 hours, and then continued to heat to 200°C for curing for 2 hours to obtain a cured epoxy resin colloid.

[0135] Performance test of epoxy resin curing colloid:

[0136] Tensile strength and elongation at break: tested according to the method of GB / T1040.3-2006. The specimen is dumbbell-shaped, with a length of 200 mm, a width of 20 mm, a middle of 10 mm, a thickness of 1 mm, and a tensile rate of 2 mm / min.

[0137] Impact strength: The test was carried out using a pendulum impact tester in accordance with the method of GB / T2567-2008. The sample size was 80 mm × 10 mm × 4 mm, the pendulum was 5.5 J, and the sample was a notched type II sample.

[0138] Bending deflection: The test was carried out according to the method of GB / T2567-2008, the sample size was 80mm×15mm×4mm, the span was 64mm, and the pressure head descending speed was 2mm / min.

[0139] The performance test results of Examples 9, 10 and Comparative Examples 1, 2 are shown in Table 10.

[0140] Table 10

[0141]

[0142]

[0143] Tensile strength reflects the material's resistance to fracture. Elongation at break refers to the percentage of the increase in length when the material is broken during a tensile test to the initial marked length. Elongation at break reflects the mobility of molecular segments in epoxy resin cured colloids. Impact strength is the ratio of the energy absorbed by the specimen during impact damage to the original cross-sectional area. It is an important indicator for judging the toughness of a material. Bending deflection, also known as bending displacement, refers to the displacement from the center point when the specimen bends and breaks during a bending test. It is used to characterize the flexibility of a material.

[0144] The higher the epoxy value of the epoxy resin, the more complete the cross-linking curing reaction will be, and the corresponding tensile strength and impact strength of the cured colloid will be higher, but the corresponding molecular segment mobility will decrease, and the elongation at break and bending deflection will be reduced. From the performance of the epoxy resin cured colloids in the above table, the cross-linking density of the comparative example 1 with the main resin being E-44 and the comparative example 2 with the main resin being E-51 is low, the tensile strength and impact strength of the comparative example 1 are low, and the elongation at break and bending deflection are relatively higher. The Example 9 series of cured colloids obtained by adding a reactive toughening agent to the comparative example 1 and then curing, introduce a series of flexible side chains of different lengths through the toughening agent, and reduce the cross-linking density of the system through the physical entanglement between the long side chains, thereby giving the epoxy resin system toughness. In particular, the maleic anhydride grafted C6 trimer, C6 tetramer, and C8 trimer with a larger number of branches have a higher skeleton space for the branches, thereby expanding the free volume of the entire epoxy resin system, and the chain segment has a higher mobility, which reduces the stress concentration effect. When subjected to external forces, it can absorb energy, and part of the energy dissipates in the form of heat due to mechanical loss, thereby preventing the development of cracks and achieving a toughening effect, which is particularly reflected in the ability to significantly improve the impact strength of the epoxy resin cured colloids of Examples 9 and 10.

[0145] In addition, the introduction of flexible long chain branches reduces the crosslinking density of the cured colloid, enhances the chain segment mobility, and correspondingly increases the elongation at break and bending deflection, while reducing the mechanical strength, which is reflected in the fact that the tensile strength of the cured colloid after adding the reactive toughening agent decreases to varying degrees. The same rule can be found from the performance comparison of the cured colloids of Example 10 series and Comparative Example 2.

[0146] The cross section after the impact test was subjected to scanning electron microscopy to analyze its morphological characteristics, such as Fig.25As shown, the impact section of comparative example 1 without adding reactive toughening agent is relatively smooth and flat with almost no obvious cracks and depressions on the surface, which indicates that the material breaks rapidly, which is consistent with the brittle fracture characteristics. From the electron microscope images of examples 9-2, 9-3 and 9-5 after adding reactive toughening agent, it can be clearly seen that a large number of rough filamentous ridges and arched cracks are generated on the fracture surface of the epoxy cured colloid, especially the fracture surfaces of examples 9-2 and 9-3 also have obvious depression structures, accompanied by stress whitening, which indicates that the impact stress is transferred from the epoxy resin body to the flexible molecular chain segment. Under the action of external force, the flexible chain segment produces yield strain to prevent the microcracks from further expanding, thereby increasing the degree of stress dispersion, so that the epoxy resin cured colloid can absorb more energy, and its toughness and impact strength are improved.

[0147] Nylon 6 toughened and modified formula, with nylon 6 as the main resin, DuPont FUSABOND TM N493 maleic anhydride grafted low Tg ethylene copolymer was used as the main toughening agent, and the maleic anhydride grafted 1,1-disubstituted olefin prepared in Example 1-8 was used as a reactive toughening agent. In addition, other processing aids were used: antioxidant 1010, lubricant pentaerythritol stearate (PETS), and light stabilizer carbon black.

[0148] Example 11-1 Nylon 6 toughening modified material formula: 85 parts by mass of nylon 6, 10.5 parts by mass of N493, 4.5 parts by mass of maleic anhydride grafted 1,1-disubstituted olefin of Example 1, 1.6 parts by mass of antioxidant 1010, 2.4 parts by mass of lubricant PETS, and 1.6 parts by mass of carbon black.

[0149] Example 11-2: Formulation of nylon 6 toughened modified material: 4.5 parts by mass of maleic anhydride grafted 1,1-disubstituted olefin of Example 3, and the rest is the same as Example 11-1.

[0150] Example 11-3: Formulation of nylon 6 toughened modified material: 4.5 parts by mass of maleic anhydride grafted 1,1-disubstituted olefin of Example 4, and the rest is the same as Example 11-1.

[0151] Example 11-4: Formulation of nylon 6 toughened modified material: 4.5 parts by mass of maleic anhydride grafted 1,1-disubstituted olefin of Example 5, and the rest is the same as Example 11-1.

[0152] Example 11-5: Formulation of nylon 6 toughened modified material: 4.5 parts by mass of maleic anhydride grafted 1,1-disubstituted olefin of Example 6, and the rest is the same as Example 11-1.

[0153] Example 11-6: Formulation of nylon 6 toughened modified material: 4.5 parts by mass of maleic anhydride grafted 1,1-disubstituted olefin of Example 7, and the rest is the same as Example 11-1.

[0154] Example 11-7: Formulation of nylon 6 toughened modified material: 4.5 parts by mass of maleic anhydride grafted 1,1-disubstituted olefin of Example 8, and the rest is the same as Example 11-1.

[0155] Example 11-8 Nylon 6 toughening and modification material formula: 88 parts by mass of nylon 6, 9 parts by mass of N493, 3 parts by mass of maleic anhydride grafted 1,1-disubstituted olefin of Example 3, 1.6 parts by mass of antioxidant 1010, 2.4 parts by mass of lubricant PETS, and 1.6 parts by mass of carbon black.

[0156] Example 11-9: Formulation of nylon 6 toughened modified material: 3 parts by mass of maleic anhydride grafted 1,1-disubstituted olefin of Example 4, and the rest is the same as Example 11-8.

[0157] Example 11-10: Formulation of nylon 6 toughening and modification material: 3 parts by mass of maleic anhydride grafted 1,1-disubstituted olefin of Example 6, and the rest is the same as Example 11-8.

[0158] Comparative Example 3: Untoughened nylon 6 formulation: 100 parts by mass of nylon 6, 1.6 parts by mass of antioxidant 1010, 2.4 parts by mass of lubricant PETS, and 1.6 parts by mass of carbon black.

[0159] Comparative Example 4: Formula of nylon 6 toughened modified material: 85 parts by mass of nylon 6, 15 parts by mass of N493, 1.6 parts by mass of antioxidant 1010, 2.4 parts by mass of lubricant PETS, and 1.6 parts by mass of carbon black.

[0160] Comparative Example 5: Formula of nylon 6 toughened modified material: 88 parts by mass of nylon 6, 12 parts by mass of N493, 1.6 parts by mass of antioxidant 1010, 2.4 parts by mass of lubricant PETS, and 1.6 parts by mass of carbon black.

[0161] Preparation method of nylon 6 toughened modified material: dry the nylon 6 raw materials of the above embodiment and comparative example at 120°C for 4 hours, add the main toughening agent, reactive toughening agent and other processing aids according to the formula ratio, mix them evenly in a mixer, melt extrude them in a twin-screw extruder, and dry them at 160°C for 4 hours after water cooling and pelletizing to obtain nylon 6 toughened modified material. The temperature parameters of the twin-screw extruder are shown in Table 11, the main screw speed of the twin-screw extruder is 360r / min, the feeding screw speed is 50r / min, and the pelletizer speed is 300r / min.

[0162] Table 11

[0163] Zone 1 Zone 2 Zone 3 District 4 District 5 District 6 District 7 Machine head Temperature / ℃ 225 230 235 240 240 235 235 240

[0164] After drying, the toughened and modified nylon 6 material is poured into the injection molding machine to form injection molding standard parts for mechanical property testing, and the mechanical property testing includes the following specific indicators.

[0165] Melt index: The melt mass flow rate (MFR) was determined according to method A of GB / T3682.1-2018. The dried nylon 6 toughened modified material was tested at a pressure of 21.18N (load of 2.16kg) and 230°C.

[0166] Tensile strength and elongation at break: The test was carried out in accordance with the method of GB / T 1040.1-2018. The specimen was a standard part obtained by injection molding. The tensile rate was 20 mm / min. The tensile strength and elongation at break were recorded after the tensile fracture.

[0167] Izod notched impact strength: The test is conducted in accordance with ASTM D256 plastic cantilever beam notched impact test (method A). The pendulum is 5.5J and the specimen is a standard part obtained by injection molding. The standard part is placed in a temperature control box at a set temperature for 2 hours before the notched impact strength test is conducted. The set temperatures of the temperature control box are 23°C, -40°C and -50°C, thereby testing the changes in the notched impact strength of the standard parts at different temperatures.

[0168] The performance test results of Example 11 and Comparative Examples 3, 4, and 5 are shown in Table 12.

[0169] Table 12

[0170]

[0171] It can be seen from the performance test results of Example 11 and Comparative Examples 3, 4, and 5 that nylon 6 without the addition of the main toughening agent has high processability, fluidity (MFR), and physical and mechanical properties (tensile strength), but the elongation at break and the notched impact strength are significantly lower, especially the defect of being brittle under low temperature conditions, and cannot be used under ultra-low temperature environments of -40°C or lower. The toughness of nylon 6 can be improved by adding the main toughening agent N493. With the increase in the mass fraction of N493, the elongation at break and the notched impact strength of nylon 6 are improved, but the corresponding MFR and tensile strength are reduced. The reason is that the main toughening agent N493 itself has a low Tg and insufficient rigidity, and the anhydride group therein reacts with the amino group at the end of the nylon 6 molecule to produce a macromolecular chain with poor fluidity. The macromolecular chain itself is difficult to move and will also hinder the movement of other segments, thus resulting in a significant decrease in the fluidity of the nylon 6 of Comparative Examples 4 and 5 after toughening.

[0172] Examples 11-1 to 11-7 use 4.5 parts by mass of maleic anhydride grafted 1,1-disubstituted olefin as a reactive toughening agent to replace the main toughening agent of the macromolecule, and Examples 11-8 to 11-10 use 3 parts by mass of maleic anhydride grafted 1,1-disubstituted olefin as a reactive toughening agent to replace the main toughening agent of the macromolecule, thereby improving the fluidity, elongation at break and notched impact strength of nylon 6 after toughening. Compared with the main toughening agent N493 of the macromolecule, the reactive toughening agent has a branched structure, a long carbon chain and anhydride groups, and a lower molecular weight, which has little effect on the fluidity of the nylon molecules after the grafting reaction. Grafting to the nylon 6 molecule through the reaction of the anhydride group can increase the branching degree of nylon 6, increase the mobility of the molecular chain and reduce the regularity of the nylon molecular chain, which is specifically manifested as the fluidity, elongation at break and notched impact strength of nylon 6 in Examples 11-1 to 11-10 compared with Examples 4 and 5 are higher, but the physical and mechanical properties (tensile strength) are reduced. In addition, Examples 11-2, 11-3, 11-5, 11-8, 11-9, and 11-10 use C6 trimer, C6 tetramer, and C8 trimer grafted with maleic anhydride with a higher degree of branching, which destroy the regularity of the nylon 6 segment through the high branching structure and long carbon chain in the molecule, increase the mobility of the nylon 6 segment, and reduce its crystallinity. Therefore, at the same amount of reactive toughening agent, the elongation at break and notched impact strength of these examples, especially the notched impact strength at extremely low temperatures, are significantly higher, and at the same time, they also have a relatively higher MFR, are easier to flow at high temperatures, and are conducive to the processing and molding of toughened and modified nylon 6.

[0173] Finally, it should be noted that the above is only a preferred embodiment of the present application and is not intended to limit the scope of protection of the present application. Although the present application has been described in detail with reference to the aforementioned embodiments, for those skilled in the art, any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present application should be included in the scope of protection of the present application.

Claims

1. A toughened nylon composition comprising the following components in parts by weight: 70-90 parts of nylon resin, 5-15 parts of a primary toughening agent, 1-10 parts of a reactive toughening agent, and 1-10 parts of a processing aid; in, The reactive toughening agent is a 1,1-disubstituted olefin anhydride product, and its structure is shown in Formula I: Wherein, R0 is a straight chain or branched hydrocarbon group of 11 to 23 carbon atoms; the 1,1-disubstituted olefin molecule contains at least one vinylidene double bond; the 1,1-disubstituted olefin is an alpha olefin coordination oligomer; The main toughening agent is maleic anhydride grafted polyethylene (PE-g-MAH).

2. The method for preparing the toughened nylon composition according to claim 1, comprising: The nylon resin, the main toughening agent, the reactive toughening agent and the processing aid are pre-mixed, melt-mixed by a twin-screw, and cooled and pelletized.

3. Application of the toughened nylon composition according to claim 1, wherein the toughened nylon composition is used in the fields of electronics, transportation, machinery and instrumentation. The use according to claim 3 , wherein the transportation is a car.