A preparation process of a foldable mobile phone protective film and its product
By mixing and stretching polyethylene, polyvinyl alcohol and other materials in step, and combining acrylic pressure-sensitive adhesive, a folding mobile phone protective film with strong self-healing ability and good scratch resistance is prepared, which solves the existing problem In the technology, the protection film has limited self-healing performance and insufficient scratch resistance, which has achieved effective protection of folding mobile phone screens.
Patent Information
- Application Number
- CN202311762193.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-12-20
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2043-12-20
AI Technical Summary
The existing folding mobile phone protective film does not perform well in terms of scratch resistance, is prone to scratches or scratches by sharp objects, and has limited self-healing performance, making it difficult to automatically repair large injuries or scratches.
Use polyethylene, polyvinyl alcohol, resin powder, polyurethane, calcium stearate, paraffin, vapor phase silica and acrylic-acrylate copolymer for kneading and step-by-step stretching, combining acrylic pressure-sensitive adhesive as the adhesive The folding mobile phone protective film has strong self-healing ability and good bending resistance.
It improves the self-healing ability, scratch resistance and light transmission of the folding mobile phone protective film, and can quickly recover marks caused by external squeeze or folding, reduce the impact of external damage on the screen and extend the service life.
Smart Images

Figure BDA0004618896180000061 
Figure BDA0004618896180000071 
Figure BDA0004618896180000081
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of foldable mobile phone protective films, and in particular to a preparation process of a foldable mobile phone protective film and a product thereof. Background Art
[0002] Foldable phones can be folded and unfolded into a larger screen when needed. They are more suitable for application scenarios that require a large screen, such as gaming and watching videos. In other words, by folding a phone, a larger screen can be carried in a smaller space.
[0003] The screen of a foldable phone can be folded 180°. Compared with the screen of a general phone, the screen of a foldable phone is more fragile and easier to break. Therefore, a protective film is needed to better protect the screen of a foldable phone. In order to ensure the user experience, the bending resistance and self-recovery of the protective film on the surface of the phone are required. It needs to maintain a certain strength after multiple bends without obvious creases. Therefore, a protective film with better protection performance is needed.
[0004] However, the current folding screen protective film is not ideal in terms of scratch resistance and is easily scratched or scratched by sharp objects or hard objects. Secondly, marks are produced after folding. Since the anti-scratch layer is affected by stretching and stress when folding, it is easy to form marks or traces in the folding area of the screen, affecting the visual effect. In addition, the self-healing performance is limited and the self-healing ability is weak. It is difficult to automatically repair larger damage or scratches. Summary of the invention
[0005] In order to solve the problem that the foldable mobile phone protective film is difficult to automatically repair large damage or scratches and has poor self-healing ability, the present application provides a preparation process of a foldable mobile phone protective film and a product thereof.
[0006] In the first aspect, the present application provides a preparation process of a foldable mobile phone protective film, which adopts the following technical solution:
[0007] A preparation process of a foldable mobile phone protective film, wherein the foldable mobile phone protective film is prepared by the following method:
[0008] S1, mixing polyethylene at 110-130° C. for plasticization, and then adding polyvinyl alcohol for further mixing to obtain a mixture A;
[0009] S2, the mixture A, resin powder, polyurethane, calcium stearate, paraffin, fumed silica, compatibilizer and acrylic acid-acrylate copolymer are mixed and kneaded at a mixing temperature of 100-130 for 2-3 hours to obtain a sheet;
[0010] S3, stretching the sheet in steps, the step-by-step stretching comprising the following steps: the first step, stretching the sheet in one direction by a stretching machine, the first step stretching temperature is 90-110°C, and the first step stretching ratio is 2.5-5.0 times; the second step, stretching the sheet in a direction orthogonal to the stretching direction of the first stage, the second step stretching temperature is 120-130°C, and the second step stretching ratio is 3.0-8.0 times; the third step, heat treatment is performed at a temperature of 160-180°C under tight tension to obtain a primary film;
[0011] S4. Apply acrylic pressure-sensitive adhesive to one side of the primary film, attach a release film, and cut to obtain a laminated mobile phone protective film.
[0012] By adopting the above technical solution, the prepared foldable mobile phone protective film has strong self-healing ability, and can quickly recover from the marks caused by external extrusion or self-folding, solving the problem of limited self-healing performance of traditional foldable screen protective films. At the same time, the surface of the foldable mobile phone protective film has excellent scratch resistance and strong bending resistance. It can bend with the unfolding and folding of the screen, and can withstand the movement of the folding screen without cracking or breaking. When scratched or damaged by the outside world, it can automatically restore to a smooth state, reducing the impact of external damage on the screen.
[0013] In the present application, polyethylene is first mixed and plasticized to improve the flexibility and impact resistance of the folding mobile phone protective film, and then polyvinyl alcohol is mixed with the mixed and plasticized polyethylene to prepare a mixture A, thereby further improving the bonding properties of polyethylene, polyvinyl alcohol and resin powder, polyurethane, and acrylic acid-acrylate copolymer, thereby improving the softness and self-healing ability of the folding mobile phone protective film.
[0014] In step S2 of the present application, resin powder, polyurethane, calcium stearate, paraffin, fumed silica, compatibilizer and acrylic acid-acrylate copolymer are mixed with mixture A to further improve the flexibility and bending resistance, wear resistance, light transmittance and self-healing ability of the folding mobile phone protective film, and the folding mobile phone protective film has multiple functions. Among them, polyurethane has high transparency, which can ensure the clarity and normal light transmission of the screen, and at the same time allow consumers to use the screen with a better feel. However, polyurethane has problems such as easy scratching, non-wear resistance, and weak self-repairing ability, and these problems affect the protective performance and service life of the folding mobile phone protective film. In the present application, resin powder, acrylic acid-acrylate copolymer and polyurethane are used to improve the self-repair, wear resistance and bending resistance of the folding mobile phone protective film, and the light transmittance of the folding mobile phone protective film is less affected.
[0015] Preferably, the resin powders in the present application are all highly transparent resin powders.
[0016] Acrylic acid copolymerization can adjust the bonding performance between the mixture A, polyurethane and resin powder, thereby improving the scratch resistance, wear resistance, bending resistance and self-healing performance of the folding mobile phone protective film.
[0017] In the present application, the sheet is stretched according to a specific temperature, steps and stretching ratio to improve the scratch resistance, abrasion resistance, light transmittance, self-healing performance and bending resistance of the foldable mobile phone protective film.
[0018] In order to take into account multiple performances, traditional folding mobile phone protective films usually include 5-6 layers, including a laminated surface protective film layer, a highly wear-resistant and anti-fingerprint hardening layer, a polyester base film, a high-viscosity pressure-sensitive adhesive layer and a release film layer. There are many layers and the processing process is complicated.
[0019] The preparation process in this application makes it possible to reduce the number of layers of the foldable mobile phone protective film. The preparation method in this application is simple to operate and only requires an adhesive layer and a protective layer to achieve multiple functions.
[0020] By using acrylic pressure-sensitive adhesive as the adhesive layer, it can fit tightly with the screen of the folding screen mobile phone, and there will be no creases or bulges in the folded or bent parts.
[0021] Preferably, the weight parts of raw materials used to prepare the sheet are as follows:
[0022] Polyethylene 7-13 parts
[0023] Polyvinyl alcohol 5-9 parts
[0024] Resin powder 10-15 parts
[0025] Polyurethane 8-12 parts
[0026] Calcium stearate 5-8 parts
[0027] 2-3 parts of compatibilizer
[0028] 6-12 parts of fumed silica
[0029] 4-8 parts of acrylic acid-acrylate copolymer.
[0030] By adopting the above technical solution, the amount of raw materials used in preparing the sheet is optimized, so that the self-repairing performance, scratch resistance, light transmittance and bending resistance of the mobile phone folding protective film are further improved.
[0031] Preferably, in step S2, an open mill is used for mixing, and the speed ratio of the two rollers in the open mill is adjusted to 1-3, and the roller distance is 1-2 mm.
[0032] By adopting the above technical solution, the two rollers rotate relative to each other, the speed ratio and roller distance of the two rollers are optimized, the friction and adhesion between the material and the roller surface, and the bonding between the materials are pulled into the gap between the two rollers, subjected to strong shearing and extrusion, and repeated shearing and extrusion heating and roller heating, so that the mixture A, resin powder, polyurethane, calcium stearate, paraffin, fumed silica, compatibilizer and acrylic acid-acrylate copolymer can be fully mixed and compatible. Through physical and mechanical effects, the scratch resistance, light transmittance, self-healing performance and bending resistance of the folding mobile phone protective film are improved.
[0033] Preferably, the resin powder is a modified resin powder, which is prepared by the following preparation method:
[0034] A: Add surfactant to soybean oil, stir evenly, then add epoxy resin, continue stirring evenly to obtain mixture A;
[0035] B: Stir and mix the mixed material and the resin powder to obtain a mixed material B;
[0036] C: Under nitrogen protection, the mixture B is aged at a temperature of 40-50° C. for 5-6 hours to obtain a mature material;
[0037] D: Then put the matured material into a twin-screw or single-screw extruder for mixing and extrusion to obtain modified resin powder.
[0038] Preferably, the weight parts of the raw materials used to prepare the modified resin powder are as follows:
[0039] Resin powder 15-20 parts
[0040] 5-10 parts soybean oil
[0041] 2-4 parts surfactant
[0042] Epoxy resin 5-15 parts.
[0043] By adopting the above technical scheme, the compatibility of the resin with polyethylene, polyvinyl alcohol, polyurethane and acrylic acid-acrylate copolymer is improved, so that the scratch resistance, light transmittance, self-repairing performance and bending resistance of the folding mobile phone protective film are better. The chemical and physical properties of the resin powder and polyethylene, polyvinyl alcohol, polyurethane and acrylic acid-acrylate copolymer are too different, resulting in poor compatibility and increased processing difficulty. In this application, soybean oil, surfactant and epoxy resin are obtained to obtain a mixture A, and then the mixture A and resin powder are stirred and mixed, and ripened, so that the compatibility of the resin with other copolymers is greatly improved, thereby improving the scratch resistance, self-repairing performance and bending resistance of the folding mobile phone protective film.
[0044] Preferably, the epoxy resin is a phenolic epoxy resin, the epoxide value of the phenolic epoxy resin is 15-20eq / 100g, and the molecular weight is 2000-5000.
[0045] By adopting the above technical scheme, the compatibility of the modified resin powder with polyethylene, polyvinyl alcohol, polyurethane and acrylic acid-acrylate copolymer is improved, thereby improving the scratch resistance, self-healing performance and bending resistance of the folding mobile phone protective film.
[0046] Preferably, the feeding rate of the twin-screw extruder in step D is 100-120 kg / hour; the temperatures of the screws of each section of the twin-screw extruder from the feed port to the die are 150-170°C, 160-170°C, 180-190°C, 190-170°C, 180-160°C and 160-150°C, respectively, and the screw speed is 200-300 rpm.
[0047] By adopting the above technical scheme, the resin powder, soybean oil and epoxy resin can be fully and evenly mixed, and the formed modified resin powder has good compatibility with polyethylene, polyvinyl alcohol, polyurethane and acrylic acid-acrylate copolymer.
[0048] In order to ensure that the light transmittance of the foldable mobile phone protective film reaches more than 87%, and at the same time, the foldable mobile phone protective film can also have scratch resistance, self-repair performance and bending resistance. The preferred resin powder of the present application includes at least one of TPU resin powder, styrene butadiene resin powder or polyvinyl chloride resin powder. The above resin powders are all highly transparent substances.
[0049] Preferably, the weight average molecular weight of the polyurethane is 50,000-200,000, the glass transition temperature Tg is 30-70°C, and the heat deformation temperature Tdeformation is 50-90°C.
[0050] By adopting the above technical scheme, polyurethane can have good bonding properties with polyethylene, polyvinyl alcohol, resin powder and acrylic acid-acrylate copolymer, further improving the scratch resistance, self-healing performance, bending resistance and light transmittance of the folding mobile phone protective film.
[0051] In the second aspect, the present application provides a foldable mobile phone protective film, which adopts the following technical solution:
[0052] A foldable mobile phone protective film comprises an acrylic pressure-sensitive adhesive layer and a protective film layer, wherein the acrylic pressure-sensitive adhesive layer has a thickness of 0.075-0.125 mm, and the protective film layer has a thickness of 0.05-0.1 mm.
[0053] By adopting the above technical solution, the foldable mobile phone protective film can stably adhere to the surface of the foldable mobile phone screen. The foldable mobile phone protective film has good self-repairing ability, scratch resistance, wear resistance and bending resistance, and can play a good protective role on the screen of the foldable mobile phone.
[0054] In summary, this application has the following beneficial effects:
[0055] 1. The present application first mixes and plasticizes polyethylene to change the mechanical properties of polyethylene, then mixes polyvinyl alcohol with the mixed and plasticized polyethylene to obtain a mixture A with good mechanical properties and compatibility; then mixes and mixes the mixture A with resin powder, polyurethane, calcium stearate, paraffin, fumed silica, a compatibilizer, and acrylic acid-acrylate copolymer to obtain a sheet with good mechanical properties; then the sheet is stretched step by step to obtain a primary film, and finally, an acrylic pressure-sensitive adhesive is coated on the surface of the primary film, a release film is attached, and shearing is performed to form a laminated mobile phone protective film with strong self-healing ability, good bending resistance, good scratch resistance, and good light transmittance.
[0056] 2. The present application prepares modified resin powder by mixing resin powder, soybean oil, surfactant and epoxy resin, so as to make the resin powder compatible with polyethylene, polyvinyl alcohol, polyurethane and acrylic acid-acrylate copolymer, thereby further improving the scratch resistance, abrasion resistance, self-healing performance and bending resistance of the folding mobile phone protective film. DETAILED DESCRIPTION
[0057] Example
[0058] Example 1
[0059] A foldable mobile phone protective film is prepared by the following preparation method:
[0060] S1, mixing 0.70 kg of polyethylene at 110° C., mixing and plasticizing, and then adding 0.50 kg of polyvinyl alcohol and continuing to mix to obtain a mixture A;
[0061] S2, mix mixture A, 1.00Kg of resin powder, 1.50Kg of polyurethane, 0.50Kg of calcium stearate, 0.50Kg of paraffin wax, 0.60Kg of fumed silica, 0.20Kg of compatibilizer (styrene-butadiene-styrene block copolymer) and 0.40Kg of acrylic acid-acrylate copolymer and mix them in an open mill, the roller speed ratio of the open mill is 1, the roller spacing is 1mm, the mixing temperature is 100°C, and the mixing time is 2h to obtain a sheet;
[0062] S3, stretching the sheet in steps, the step-by-step stretching comprising the following steps: first, stretching the sheet in one direction using a stretching machine, the first step stretching temperature is 90°C, and the first step stretching ratio is 2.5 times; second, stretching the sheet in a direction orthogonal to the stretching direction of the first stage, the second step stretching temperature is 130°C, and the second step stretching ratio is 3.0 times; third, heat treatment is performed at a temperature of 160°C under tight tension to obtain a protective film layer;
[0063] S4. Apply acrylic pressure-sensitive adhesive to one side of the protective film layer, attach a release film, and cut to obtain a laminated mobile phone protective film.
[0064] The molecular weight of polyethylene is 10,000.
[0065] The molecular weight of polyvinyl alcohol is 120,000.
[0066] The resin powder is polyurethane resin powder, with a melt flow rate (204°C) of 52g / 10min and a tensile strength of 250kg / cm 2 , bending strength is 850kg / cm 2 , the elongation at break is 405%.
[0067] The weight average molecular weight of the polyurethane is 50,000, the glass transition temperature Tg is 30°C, and the heat deformation temperature Tdeformation is 50°C.
[0068] Acrylic acid-acrylate copolymer The average molecular weight of the acrylic acid-acrylate copolymer is 5000, and the molar ratio of the acrylic acid structural unit to the acrylate structural unit is 2:3.
[0069] The difference between Example 2-3 and Example 1 is that the amount, type and experimental parameters of some raw materials used in preparing the foldable mobile phone protective film are different from those in Example 1. The specific differences are shown in Table 1:
[0070] Table 1 Amounts, types and experimental parameters of raw materials used in preparing foldable mobile phone protective films in Examples 1-3
[0071]
[0072]
[0073] The molecular weight of the styrene butadiene resin powder is 121,000, the butadiene content is 15.8w%, the melt index is 0.19g / 10min, the bending strength is 34MPa, and the elongation at break is 110%.
[0074] The molecular weight of polyvinyl chloride resin powder is 50,000, the softening point is 85°C, the tensile strength is 60MP, and the impact strength is 5kJ / m 2 .
[0075] Styrene-butadiene-styrene block copolymer, SBS YH-791E, was purchased from Sinopec Baling Petrochemical Company.
[0076] Polystyrene grafted maleic anhydride copolymer SZ 23110 was purchased from Polysco pepolymers BV.
[0077] Maleic anhydride grafted polyethylene copolymer, MC218, was purchased from Ningbo Nengzhiguang New Materials Technology Co., Ltd.
[0078] LIMITED.
[0079] Example 4
[0080] A foldable mobile phone protective film, the difference between this embodiment and embodiment 1 is that the resin powder is a modified resin powder, which is prepared by the following method:
[0081] A: Add 0.20 kg of surfactant (octylphenol polyoxyethylene ether) to 0.50 kg of soybean oil, stir evenly, then add 0.50 kg of epoxy resin, continue stirring evenly, and obtain mixture A;
[0082] B: Stir and mix the mixed material and 1.50 kg of resin powder to obtain mixed material B;
[0083] C: Under nitrogen protection, the mixture B was aged at a temperature of 40°C for 5 hours to obtain a mature material;
[0084] D: The matured material is then put into a twin-screw extruder for mixing and extrusion to obtain modified resin powder.
[0085] The feeding rate of the twin-screw extruder is 100kg / hour; the temperatures of each section of the screw of the twin-screw extruder from the feeding port to the die are 150°C, 160°C, 180°C, 190°C, 18°C and 160°C respectively, and the screw speed is 200rpm.
[0086] The resin powder is polyurethane resin powder, with a melt flow rate (204°C) of 52g / 10min and a tensile strength of 250kg / cm 2 , bending strength is 850kg / cm 2 , the elongation at break is 405%.
[0087] The epoxy resin is a phenolic epoxy resin, and the epoxy value of the phenolic epoxy resin is 15-20eq / 100g and the molecular weight is 2000.
[0088] The difference between Example 5-6 and Example 4 is that the amount of some raw materials and parameters for preparing the modified resin powder are different from those in Example 4. The specific differences between Examples 4-6 are shown in Table 2.
[0089] Table 2 Raw material dosage and parameters for preparing modified resin powder
[0090]
[0091] Example 7
[0092] A foldable mobile phone protective film. The difference between this embodiment and embodiment 1 is that the resin powder is, and the remaining raw material types, amounts and test steps are consistent with those in embodiment 1.
[0093] Example 8
[0094] A foldable mobile phone protective film. The difference between this embodiment and embodiment 1 is that in step S2, an open mill is used for mixing, the speed ratio of the two rollers in the open mill is adjusted to 1, and the roller distance is 3 mm. The remaining raw material types, amounts and test steps are consistent with those in embodiment 1.
[0095] Example 9
[0096] A foldable mobile phone protective film. The difference between this embodiment and embodiment 4 is that when preparing the modified resin powder, step C is omitted, and the remaining raw material types, amounts and test steps are consistent with those of embodiment 4.
[0097] Example 10
[0098] A foldable mobile phone protective film. The difference between this embodiment and embodiment 4 is that in the preparation of modified resin powder, epoxy resin is replaced by maguro resin, and the remaining raw material types, amounts and test steps are consistent with those of embodiment 4.
[0099] The softening point of Maguron resin is 90°C and the average molecular weight is 3,000.
[0100] Comparative Example
[0101] Comparative Example 1
[0102] A foldable mobile phone protective film, the difference between this comparative example and Example 1 is that a casting film making method is adopted in step S3, and the process is as follows:
[0103] Mix mixture A, resin powder, polyurethane, calcium stearate, paraffin, fumed silica, a compatibilizer and acrylic acid-acrylate copolymer to obtain a mixture, and then put the mixture into a casting machine. The heating temperature of the extruder and the die head should be controlled between 200°C, the stage temperature of the barrel is 180°C, and the melt temperature is maintained at 230°C.
[0104] Comparative Example 2
[0105] A foldable mobile phone protective film. The difference between this comparative example and Example 1 is that step S1 is omitted, and in step S2, polyethylene, polyvinyl alcohol, resin powder, polyurethane, calcium stearate, paraffin, fumed silica, a compatibilizer and acrylic acid-acrylate copolymer are mixed and kneaded at a mixing temperature of 100° C. for 2 hours to obtain a sheet. The remaining raw material types, amounts and test steps are consistent with those in Example 1.
[0106] Comparative Example 3
[0107] A foldable mobile phone protective film. The difference between this comparative example and Example 1 is that the resin powder is replaced with an equal amount of polyvinyl chloride, and the remaining raw material types, amounts and test steps are consistent with those in Example 1.
[0108] The molecular weight of polyvinyl chloride is 80,000 and the softening point is 85°C.
[0109] Comparative Example 4
[0110] A foldable mobile phone protective film. The difference between this comparative example and Example 1 is that the acrylic acid-acrylate copolymer is replaced by an equal amount of vinyl acetate copolymer, and the remaining raw material types, amounts and test steps are consistent with Example 1.
[0111] The average molecular weight of the vinyl acetate copolymer is 2000, and the content of vinyl acetate is 25%.
[0112] Comparative Example 5
[0113] A foldable mobile phone protective film. The difference between this comparative example and Example 1 is that polyethylene is replaced by an equal amount of polyvinyl chloride, and the remaining raw material types, amounts and test steps are consistent with those in Example 1.
[0114] The molecular weight of polyvinyl chloride is 80,000 and the softening point is 85°C.
[0115] Performance testing
[0116] The folding mobile phone protective films prepared in Examples 1-10 and Comparative Examples 1-5 were subjected to pencil hardness test, light transmittance test, wear resistance, bending resistance and self-healing performance test.
[0117] Detection method / test method
[0118] Pencil hardness test: Use Elcometer 3086 pencil hardness tester to measure the pencil hardness of the product. Measurement method: Use a Mitsubishi pencil with a hardness of H-9H to draw 5 lines under a load of 500g, then observe whether the hard coating has scratches and judge according to the following standards. 0-1 scratches are qualified, 2 or more are unqualified, and the highest hardness of the qualified pencil is recorded as the hardness of the folding mobile phone protective film.
[0119] Light transmittance: measured using a NDH 2000N haze meter produced by Nippon Denshoku Co., Ltd. by the transmitted light method.
[0120] Abrasion resistance: Use Kunshan Jingjia Instrument A20-339 steel wool resistance testing machine under a load of 500gf / cm2, use #0000 steel wool, load 1kg, rub back and forth on the surface of the folding mobile phone protective film 1000 times to confirm whether the coating has scratches. 0 scratches is qualified, and more than or equal to 1 scratch is unqualified.
[0121] Bending resistance: The folding mobile phone protective films of Examples 1-10 and Comparative Examples 1-5 were cut into 150mm×15mm samples, placed on a bending strength tester, and subjected to a load of 200g. The samples were bent back and forth to the left and right sides in a vertical state at a bending angle of 180 degrees until the samples broke. The test was automatically counted, and the number of foldings less than 50,000 was considered unqualified.
[0122] Self-healing performance test: Use a copper rod to draw lines back and forth on the surface of the folding mobile phone film. After observing that the surface of the folding mobile phone film is obviously concave, use a hot hair dryer, set the temperature to 45℃, blow hot air to the film for 10 seconds, then let it stand for 5 minutes and observe the scratches. If there are scratches, it means that the self-healing performance of the folding mobile phone protective film is poor and it is unqualified; if you need to use a 20x magnification method to observe, you can see the scratches, which is good; if you can't see it, it is not excellent. The experimental data is shown in Table 3:
[0123] Table 3 Experimental data of Examples 1-10 and Comparative Examples 1-5
[0124]
[0125]
[0126] It can be seen from Examples 1-10 and Comparative Examples 1-5 in combination with Table 4 that the foldable mobile phone protective film prepared by adopting the self-prepared process has good self-repairing ability, bending resistance, scratch resistance, abrasion resistance, light transmittance and other properties.
[0127] Compared with Comparative Examples 1-2, Example 1 shows that the pencil hardness test, wear resistance, bending resistance and self-repairing ability tests in Comparative Examples 1-2 are all unqualified, indicating that the folding mobile phone protective film prepared by the formula of the present application according to the preparation process of the present application has good self-repairing ability, bending resistance and scratch resistance.
[0128] Compared with Example 1 and Comparative Examples 3-5, although the folding resistance samples in Comparative Examples 3-5 reached and the standard line, the pencil hardness and abrasion resistance samples were not unqualified, and the self-healing performance tests in Comparative Examples 3 and 5 were both unqualified, indicating that by adopting the formula in the present application, the folding mobile phone protective film can have multiple functions such as self-healing ability, bending resistance, scratch resistance and abrasion resistance.
[0129] Comparison between Example 1 and Examples 4-6 shows that the self-repairing ability, bending resistance, and scratch resistance of the foldable mobile phone film can be further improved by adopting the modified resin powder prepared in the present application.
[0130] Comparison between Example 4 and Examples 9-10 shows that by adopting the preparation method in the present application to prepare the modified resin powder, and then using the modified resin powder to prepare the folding mobile phone protective film, the self-repairing ability, bending resistance and scratch resistance of the folding mobile phone film can be further improved.
[0131] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.
Claims
1. A preparation process for a foldable mobile phone protective film, characterized in that: The laminated mobile phone protective film is prepared by the following method: S1, mixing polyethylene at 110-130° C. for plasticization, and then adding polyvinyl alcohol for further mixing to obtain a mixture A; S2, mixing and kneading the mixture A, resin powder, polyurethane, calcium stearate, paraffin, fumed silica, compatibilizer and acrylic acid-acrylate copolymer at a mixing temperature of 100-130° C. for 2-3 hours to obtain a sheet; S3, stretching the sheet in steps, the step-by-step stretching comprising the following steps: first, stretching the sheet in one direction using a stretching machine, the first step stretching temperature is 90-110°C, and the first step stretching ratio is 2.5-5.0 times; second, stretching the sheet in a direction orthogonal to the stretching direction of the first stage, the second step stretching temperature is 120-130°C, and the second step stretching ratio is 3.0-8.0 times; third, performing heat treatment at a temperature of 160-180°C under tight tension to obtain a protective film layer; S4, applying acrylic pressure-sensitive adhesive to one side of the protective film layer, attaching a release film, and cutting to obtain a laminated mobile phone protective film; The weight parts of raw materials used to prepare the sheet are as follows: Polyethylene 7-13 parts Polyvinyl alcohol 5-9 parts Resin powder 10-15 parts Polyurethane 15-20 parts Calcium stearate 5-8 parts 5-8 parts paraffin 2-3 parts of compatibilizer 6-12 parts of fumed silica 4-8 parts of acrylic acid-acrylate copolymer; The resin powder is a modified resin powder, which is prepared by the following preparation method: A: Add surfactant to soybean oil, stir evenly, then add epoxy resin, continue stirring evenly to obtain mixture A; B: Stir and mix the mixed material and the resin powder to obtain a mixed material B; C: Under nitrogen protection, the mixture B is aged at a temperature of 40-50° C. for 5-6 hours to obtain a mature material; D: Put the matured material into a twin-screw extruder for mixing and extrusion to obtain modified resin powder; The weight parts of the raw materials used to prepare the modified resin powder are as follows: Resin powder 15-20 parts 5-10 parts soybean oil 2-4 parts surfactant Epoxy resin 5-15 parts; The epoxy resin is a phenolic epoxy resin, the epoxy value of the phenolic epoxy resin is 15-20eq / 100g, and the molecular weight is 2000-5000; The weight average molecular weight of the polyurethane is 50,000-200,000, the glass transition temperature Tg is within 30-70°C, and the heat deformation temperature Tdeformation is within 50-90°C.
2. The process for preparing a foldable mobile phone protective film according to claim 1, characterized in that: In step S2, an open mill is used for mixing, and the speed ratio of the two rollers in the open mill is adjusted to 1-3, and the roller distance is 1-2 mm.
3. The process for preparing a foldable mobile phone protective film according to claim 1, characterized in that: The feeding rate of the twin-screw extruder in step D is 100-120kg / hour; the temperatures of the screws of each section of the twin-screw extruder from the feed port to the die are 150-170°C, 160-170°C, 180-190°C, 190-170°C, 180-160°C and 160-150°C, respectively, and the screw speed is 200-300rpm.
4. A foldable mobile phone protective film prepared by the foldable mobile phone protective film preparation process according to any one of claims 1 to 3, characterized in that: The foldable mobile phone protective film comprises an acrylic pressure-sensitive adhesive layer and a protective film layer, the acrylic pressure-sensitive adhesive layer has a thickness of 0.075-0.125 mm, and the protective film layer has a thickness of 0.05-0.1 mm.