A novel preparation method of hydroxyapatite and its application in the remediation of heavy metal polluted water

By using aquatic waste to synthesize a new type of chitin-modified hydroxyapatite, the problem of insufficient remediation performance of cadmium and arsenic polluted water in the existing technology has been solved, and high-efficiency and low-cost heavy metal adsorption effects have been achieved, which is suitable for industrial applications.

CN117945374BActive Publication Date: 2024-10-18RES INST OF ZHEJIANG UNIV TAIZHOU +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410115683.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-01-26
Publication Date
2024-10-18
Estimated Expiration
2044-01-26

AI Technical Summary

Technical Problem

It is difficult to simultaneously repair cadmium and arsenic polluted water bodies with existing technology, and the adsorption performance of hydroxyapatite is poor for arsenic. The hydrothermal method has high synthesis efficiency but high energy consumption, which is not conducive to industrialization.

Method used

Using aquatic wastes such as shells and fish bones as calcium sources, and aquatic wastes such as shrimp shells, crab shells, and lobster shells as chitin sources, a new type of chitin-modified hydroxyapatite is synthesized in one step through the mechanical force of a ball mill to improve its Adsorption properties for cadmium and arsenic.

Benefits of technology

The adsorption performance of the new hydroxyapatite for cadmium and arsenic is significantly improved, and the simultaneous remediation of cadmium and arsenic contaminated water bodies is achieved. The process is simple and low-cost, and is suitable for industrial applications and large-scale wastewater treatment.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117945374B_ABST
    Figure CN117945374B_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of a novel hydroxyapatite and an application thereof in the restoration of heavy metal polluted water bodies, comprising the following steps: step S1: washing a calcium source and a chitosan source, drying them for standby use; step S2: mixing the calcium source and the chitosan source, grinding them in a pulverizer, and sieving them to obtain a mixed powder sample; step S3: mixing the mixed powder sample with a phosphorus source and distilled water, placing them in a ball mill for ball milling treatment, and obtaining a novel hydroxyapatite slurry; step S4: washing, drying and grinding the novel hydroxyapatite slurry to obtain a novel hydroxyapatite; the invention crushes the chitosan source by mechanical force of the ball mill, promotes the leaching of chitosan, and more chitosan is modified on the surface of the hydroxyapatite with a larger specific surface area to form the novel hydroxyapatite, which significantly improves the adsorption performance of the novel hydroxyapatite on cadmium and arsenic, and realizes the simultaneous extraction and restoration of cadmium and arsenic in cadmium-arsenic polluted wastewater.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of solid waste resource utilization and water treatment, and relates to a preparation method of a novel hydroxyapatite and application of the same in the restoration of heavy metal polluted water bodies. Background Art

[0002] Heavy metals are key pollutants in water pollution, among which cadmium and arsenic are the main pollutants and are internationally recognized as potentially carcinogenic toxic elements. Cadmium, arsenic and their compounds are widely present in production industries such as metallurgy, chemical industry, and mining. They usually enter water bodies through industrial wastewater, atmospheric deposition, and phosphate fertilizer application, and further accumulate in the human brain, organs, and other organs through the food chain, leading to various diseases and even cancer. Since cadmium and arsenic have opposite chemical properties, it is difficult to achieve simultaneous repair, and the repair materials currently on the market are expensive. Therefore, the development of economical and efficient repair materials for the repair of cadmium and arsenic contaminated water bodies has great practical significance for maintaining a good ecological environment and maintaining human health.

[0003] Hydroxyapatite (HAP) is a weakly alkaline calcium phosphate material with low solubility. It can adsorb heavy metal cations in water through physical adsorption, ion exchange and precipitation. Therefore, using aquatic product waste as raw material to produce hydroxyapatite can not only realize waste resource utilization, but also provide a cheap and environmentally friendly material for heavy metal pollution control.

[0004] At present, hydroxyapatite is mainly synthesized by hydrothermal method, which refers to the synthesis of HAP in aqueous solution or water vapor under high temperature and high pressure in an autoclave. Although this method has high synthesis efficiency and fast reaction speed, it has high energy consumption and high requirements for synthesis conditions, which is not conducive to industrialization and does not conform to the concept of "low-carbon production". At the same time, hydroxyapatite has poor adsorption performance for arsenic, making it difficult to achieve simultaneous remediation of cadmium and arsenic contaminated water bodies. Summary of the invention

[0005] In order to overcome at least one of the deficiencies of the prior art, the present invention provides a method for preparing a novel hydroxyapatite and its application in the restoration of heavy metal polluted water bodies.

[0006] In order to achieve the above object, the present invention adopts the following technical scheme: a method for preparing a novel hydroxyapatite, comprising the following steps:

[0007] Step S1: Rinse the calcium source and chitosan source and dry them for later use;

[0008] Step S2: mixing the calcium source and the chitosan source in a grinder, grinding and sieving to obtain a mixed powder sample;

[0009] Step S3: mixing the mixed powder sample with a phosphorus source and distilled water and subjecting the mixture to ball milling treatment in a ball mill to obtain a novel hydroxyapatite slurry;

[0010] Step S4: washing, drying and grinding the novel hydroxyapatite slurry to obtain novel hydroxyapatite.

[0011] Furthermore, in step S3, the molar ratio of calcium contained in the mixed powder sample to phosphorus contained in the phosphorus source is 1.67.

[0012] Furthermore, the calcium source is configured as aquatic waste containing calcium.

[0013] Furthermore, the chitosan source is aquatic waste containing chitosan.

[0014] Furthermore, the calcium source and the chitosan source are 65-75 parts by weight and 25-35 parts by weight, respectively.

[0015] Further, the phosphorus source is set to (NH 4 ) 2 HPO 4 NH 4 H 2 PO 4 .

[0016] Furthermore, the calcium-containing aquatic waste is configured as shells and fish bones.

[0017] Furthermore, the aquatic waste containing chitosan is shrimp shells, crab shells and lobster shells.

[0018] Furthermore, in step S2, the mixed powder sample is passed through a 0.75 mm sieve.

[0019] The application of the new hydroxyapatite prepared according to the preparation method in the restoration of heavy metal polluted water bodies.

[0020] In summary, the present invention is beneficial in that:

[0021] 1) The present invention uses calcium-containing aquatic waste such as shells and fish bones as calcium sources, uses chitin-containing aquatic waste such as shrimp shells, crab shells and lobster shells as chitin sources, uses diammonium hydrogen phosphate and diammonium dihydrogen phosphate as phosphorus sources, and uses the mechanical force of ball milling to synthesize a new type of chitin-modified hydroxyapatite in one step, which significantly improves the adsorption performance of cadmium and arsenic in wastewater. The present invention not only realizes the resource utilization of aquatic product waste, but also the new type of hydroxyapatite prepared from shells, fish bones, shrimp shells, crab shells and lobster shell waste has the advantages of low cost, simple preparation process and excellent adsorption performance, which is of great significance in industrial application and large-scale wastewater treatment.

[0022] 2) The present invention uses the mechanical force of a ball mill to break up the calcium source, so that the calcium source, calcium carbonate, diammonium hydrogen phosphate and diammonium dihydrogen phosphate are synthesized into hydroxyapatite with a smaller particle size, which effectively improves the synthesis efficiency of hydroxyapatite and improves the adsorption efficiency of hydroxyapatite on cadmium.

[0023] 3) The present invention breaks up the chitosan source through the mechanical force of a ball mill, promotes the leaching of chitosan (α-chitosan), and more chitosan is modified on the surface of hydroxyapatite with a larger specific surface area to form a new type of hydroxyapatite, which significantly improves the adsorption performance of the new type of hydroxyapatite for cadmium and arsenic, and realizes the simultaneous extraction and repair of cadmium and arsenic in cadmium-arsenic contaminated wastewater. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 Scanning electron microscope images of hydroxyapatite synthesized by different processes.

[0025] Figure 2 XRD patterns of hydroxyapatite synthesized by different processes.

[0026] Figure 3 The removal rates of cadmium and arsenic by hydroxyapatite synthesized by different processes.

[0027] Figure 4 Schematic diagram of the removal rates of cadmium and arsenic by the novel hydroxyapatite according to different embodiments of the present invention. DETAILED DESCRIPTION

[0028] The following describes the embodiments of the present invention by specific examples, and those skilled in the art can easily understand other advantages and effects of the present invention from the contents disclosed in this specification. The present invention can also be implemented or applied through other different specific embodiments, and the details in this specification can also be modified or changed in various ways based on different viewpoints and applications without departing from the spirit of the present invention. It should be noted that the following embodiments and features in the embodiments can be combined with each other without conflict.

[0029] It should be noted that the illustrations provided in the following embodiments are only schematic illustrations of the basic concept of the present invention, and thus the drawings only show components related to the present invention rather than being drawn according to the number, shape and size of components in actual implementation. In actual implementation, the type, quantity and proportion of each component may be changed arbitrarily, and the component layout may also be more complicated.

[0030] All directional indications in the embodiments of the present invention (such as up, down, left, right, front, back, horizontal, vertical...) are only used to explain the relative position relationship, movement status, etc. between the components in a certain specific posture. If the specific posture changes, the directional indication will also change accordingly.

[0031] Due to installation errors and other reasons, the parallel relationship referred to in the embodiments of the present invention may actually be an approximately parallel relationship, and the vertical relationship may actually be an approximately vertical relationship.

[0032] Embodiment 1:

[0033] A novel method for preparing hydroxyapatite comprises the following steps:

[0034] Step S1: respectively place shells, fish bones, shrimp shells, crab shells and lobster shells in water and heat them to boil, rinse the surface of the waste and dry them for later use;

[0035] Step S2: 15.0 g of shells, 15.0 g of fish bones, 5.0 g of shrimp shells, 2.5 g of crab shells and 2.5 g of lobster shell wastes were mixed and ground in a grinder and passed through a 0.75 mm sieve to obtain a mixed powder sample;

[0036] Step S3: Mix the mixed powder sample with 13.44 g (NH 4 ) 2 HPO 4 、15.42gNH 4 H 2 PO 4 Mix with 360 ml of distilled water and place in a ball mill for ball milling. The ball milling speed of the ball mill is 600 rpm. The ball milling time is 3 hours. Take out and obtain a novel hydroxyapatite slurry.

[0037] Step S4: washing the novel hydroxyapatite slurry once with anhydrous ethanol and twice with deionized water, drying it in an oven at 60° C., and grinding it after drying to obtain the novel hydroxyapatite.

[0038] Shells and fish bones are used as calcium sources, shrimp shells, crab shells and lobster shells are used as chitosan sources, diammonium hydrogen phosphate and ammonium dihydrogen phosphate are used as phosphorus sources, and step S3 is to ball-mill the mixed powder of the calcium source and chitosan source with the phosphorus source and distilled water to obtain a new hydroxyapatite slurry; during the ball milling process, the ball mill generates a mechanical force due to the collision of the balls, and the mechanical force breaks the calcium source, and calcium carbonate, diammonium hydrogen phosphate and ammonium dihydrogen phosphate are used to synthesize hydroxyapatite with a smaller particle size, which effectively improves the synthesis efficiency of hydroxyapatite and improves the specific surface area of ​​the synthesized hydroxyapatite. At the same time, the mechanical force breaks the chitosan source, which can promote the leaching of chitosan (α-chitosan), and more chitosan is modified on the surface of hydroxyapatite with a larger specific surface area to form a new hydroxyapatite. The new hydroxyapatite of the present application has a better chitosan modification effect, which greatly improves the adsorption performance of cadmium and arsenic.

[0039] Hydroxyapatite has excellent adsorption performance for cadmium. In the present application, the adsorption performance of the novel hydroxyapatite for arsenic is improved by improving the modification effect of chitin on the surface of hydroxyapatite.

[0040] Embodiment 2:

[0041] A novel method for preparing hydroxyapatite comprises the following steps:

[0042] Step S1: respectively place shells, fish bones, shrimp shells, crab shells and lobster shells in water and heat them to boil, rinse the surface of the waste and dry them for later use;

[0043] Step S2: 15.0 g of shells, 15.0 g of fish bones, 5.0 g of shrimp shells, 2.5 g of crab shells and 2.5 g of lobster shell wastes were mixed and ground in a grinder and passed through a 0.75 mm sieve to obtain a mixed powder sample;

[0044] Step S3: Mix the mixed powder sample with 13.44 g (NH 4 ) 2 HPO 4 、15.42gNH 4 H 2 PO 4 The mixture was mixed with 360 ml of distilled water and placed in a ball mill for ball milling at a speed of 600 rpm for 4.5 hours to obtain a novel hydroxyapatite slurry;

[0045] Step S4: washing the novel hydroxyapatite slurry once with anhydrous ethanol and twice with deionized water, drying it in an oven at 60° C., and grinding it after drying to obtain the novel hydroxyapatite.

[0046] Embodiment three:

[0047] A novel method for preparing hydroxyapatite comprises the following steps:

[0048] Step S1: respectively place shells, fish bones, shrimp shells, crab shells and lobster shells in water and heat them to boil, rinse the surface of the waste and dry them for later use;

[0049] Step S2: 15.0 g of shells, 15.0 g of fish bones, 5.0 g of shrimp shells, 2.5 g of crab shells and 2.5 g of lobster shell wastes were mixed and ground in a grinder and passed through a 0.75 mm sieve to obtain a mixed powder sample;

[0050] Step S3: Mix the mixed powder sample with 13.44 g (NH 4 ) 2 HPO 4 、15.42gNH 4 H 2 PO 4 Mix with 360 ml of distilled water and place in a ball mill for ball milling. The ball milling speed of the ball mill is 600 rpm. The ball milling time is 6 hours. Take out and obtain a novel hydroxyapatite slurry.

[0051] Step S4: washing the novel hydroxyapatite slurry once with anhydrous ethanol and twice with deionized water, drying it in an oven at 60° C., and grinding it after drying to obtain the novel hydroxyapatite.

[0052] Embodiment 4:

[0053] A novel method for preparing hydroxyapatite comprises the following steps:

[0054] Step S1: respectively place shells, fish bones, shrimp shells, crab shells and lobster shells in water and heat them to boil, rinse the surface of the waste and dry them for later use;

[0055] Step S2: 13.0 g of shells, 13.0 g of fish bones, 5.0 g of shrimp shells, 5.0 g of crab shells and 4.0 g of lobster shell wastes were mixed and ground in a grinder, and passed through a 0.75 mm sieve to obtain a mixed powder sample;

[0056] Step S3: Mix the mixed powder sample with 13.44 g (NH 4 ) 2 HPO 4 、15.42gNH 4 H 2 PO 4 The mixture was mixed with 360 ml of distilled water and placed in a ball mill for ball milling at a speed of 600 rpm for 4.5 hours to obtain a novel hydroxyapatite slurry;

[0057] Step S4: washing the novel hydroxyapatite slurry once with anhydrous ethanol and twice with deionized water, drying it in an oven at 60° C., and grinding it after drying to obtain the novel hydroxyapatite.

[0058] In the above embodiment:

[0059] In step S3, the ratio of the mixed powder sample to distilled water is 1:10-12 (w / v);

[0060] In step S3, the ball milling speed is 400-600 rpm, and the ball milling time is 3-6 hours.

[0061] The novel hydroxyapatite synthesized by mechanical force in Examples 1-4 and the conventional hydroxyapatite synthesized by hydrothermal method were subjected to solution cadmium and arsenic removal tests, scanning electron microscopy and XRD tests, and the following results were obtained: Figure 1-4 of the test results.

[0062] The test conditions for solution cadmium and arsenic removal remain the same, specifically:

[0063] At room temperature (25°C), weigh 0.05g of the new hydroxyapatite and conventional hydroxyapatite in 50mL centrifuge tubes, add 30mL of cadmium and arsenic solutions, respectively, where the concentrations of cadmium and arsenic in the solutions are 50.6mg / L and 11.2mg / L, respectively. Place the centrifuge tube in a constant temperature air bath oscillator and oscillate at 250 rpm for 24h, then take it out, centrifuge and filter it with a 0.45μm microporous filter membrane, and determine the concentrations of cadmium and arsenic in the solution by ICP-MS. The test results are as follows: Figure 3-4 shown.

[0064] like Figure 1-Figure 2 As shown, it can be seen that the particle size of the new hydroxyapatite synthesized under the action of mechanical force is smaller than that of conventional hydroxyapatite, and the surface chitosan peak intensity and content of the new hydroxyapatite synthesized by mechanical force are higher, indicating that the new hydroxyapatite with smaller particle size can load more chitosan. Therefore, it is obtained that mechanical force synthesis has the effect of enhancing the chitosan modification of hydroxyapatite, and as the ball milling time increases, the formed hydroxyapatite has a smaller particle size, a higher chitosan peak intensity, a higher content, and a more significant chitosan modification effect.

[0065] like Figure 3-Figure 4 As shown, the removal efficiency of the new hydroxyapatite synthesized by mechanical force for cadmium and arsenic is in the range of 78.43% to 94.63% and 67.05% to 91.43%, respectively, which is significantly higher than that of the conventional hydroxyapatite synthesized by hydrothermal method; with the increase of ball milling time, the removal efficiency of the new hydroxyapatite for cadmium and arsenic first increases and then slowly decreases and remains in a stable range. The removal efficiency of the new hydroxyapatite for cadmium and arsenic is greatly affected by the ball milling time. With the increase of ball milling time, the particle size of hydroxyapatite gradually decreases, indicating that the reduction of hydroxyapatite particle size can promote the synthesis efficiency of hydroxyapatite and increase the specific surface area. Mechanical force promotes the leaching of chitin, thereby improving the modification of chitin on the surface of hydroxyapatite. However, the reduction of hydroxyapatite particle size to a certain extent may cause material agglomeration, slightly affecting the adsorption performance of the new hydroxyapatite material. The preferred ball milling time is controlled at 3-6 hours, and the adsorption performance is optimal at 4.5 hours.

[0066] From the test results of the above embodiments, it can be seen that the present invention uses shell, fish bone, shrimp shell, crab shell and lobster shell waste to synthesize chitin-modified new hydroxyapatite in one step by mechanical force, which significantly improves the adsorption performance of the new hydroxyapatite for cadmium and arsenic.

[0067] The present invention not only realizes the resource utilization of aquatic product waste, but also the new hydroxyapatite has the advantages of low cost, simple preparation process and excellent adsorption performance, which is of great significance in industrial application and large-scale wastewater treatment.

[0068] The present application also provides an application of a novel hydroxyapatite prepared by the above preparation method in the restoration of heavy metal polluted water bodies.

[0069] Obviously, the described embodiments are only some embodiments of the present invention, not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work should fall within the scope of protection of the present invention.

Claims

1. A novel method for preparing hydroxyapatite, characterized in that: The following steps are involved: Step S1: Rinse the calcium source and chitosan source and dry them for later use; The calcium source is configured as shells or fish bones; The chitosan source is shrimp shell, crab shell, lobster shell; Step S2: mixing the calcium source and the chitosan source in a grinder, grinding and sieving to obtain a mixed powder sample; Step S3: mixing the mixed powder sample with a phosphorus source and distilled water and subjecting the mixture to ball milling treatment in a ball mill to obtain a novel hydroxyapatite slurry; The mechanical force of ball milling breaks the calcium source, and the calcium source and phosphorus source synthesize hydroxyapatite with a smaller particle size. The mechanical force of ball milling breaks the chitosan source, which promotes the leaching of chitosan. Chitosan is modified on the surface of hydroxyapatite with a larger specific surface area to form a new type of hydroxyapatite. Step S4: washing, drying and grinding the novel hydroxyapatite slurry to obtain novel hydroxyapatite.

2. The method for preparing a novel hydroxyapatite according to claim 1, characterized in that: The molar ratio of calcium contained in the mixed powder sample to phosphorus contained in the phosphorus source in step S3 is 1.

67.

3. The method for preparing a novel hydroxyapatite according to claim 2, characterized in that: The calcium source and the chitosan source are 65-75 parts by weight and 25-35 parts by weight, respectively.

4. The method for preparing a novel hydroxyapatite according to claim 1, characterized in that: The phosphorus source is set to (NH4)2HPO4, NH4H2PO4.

5. The method for preparing a novel hydroxyapatite according to claim 1, characterized in that: In step S2, the mixed powder sample is passed through a 0.75 mm sieve.

6. Use of the novel hydroxyapatite prepared by the preparation method according to any one of claims 1 to 5 in the restoration of heavy metal polluted water bodies.