A method for preparing high-purity antimony

Through the reaction of antimony trioxide with ethylene glycol and sodium carbonate, the problem of difficult production of high-purity antimony in the existing technology is solved, and the effective preparation of high-purity antimony is achieved, which meets domestic and foreign market demands, and reduces production costs and processes. Complexity.

CN117965908BActive Publication Date: 2024-11-22XIKUANG SHANXING ANTIMONY CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202410092288.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-01-23
Publication Date
2024-11-22
Estimated Expiration
2044-01-23

AI Technical Summary

Technical Problem

The existing technology is difficult to effectively produce high-purity antimony, which has led to the failure to fully meet its domestic market demand, and the production process is complex and costly, which limits industrial scale production.

Method used

Antimony trioxide and ethylene glycol are used to form ethylene glycol antimony, and the reaction is removed by covering with sodium carbonate and heating at high temperature to remove impurities to obtain high-purity antimony. The method includes reacting for 2 to 4 hours under vacuum conditions of 140 to 150°C, followed by heating at 1100 to 1200°C for 2 to 6 hours, and producing antimony through the covering of sodium carbonate and high-temperature reaction, and floating impurities such as low-density carbon are formed, so as to achieve Purification of antimony.

Benefits of technology

It has achieved the preparation of high-purity antimony, with a total impurity content of ≤100ppm, a high direct yield, a short cycle and a low production cost. It is suitable for large-scale industrial production and meets the needs of high-tech fields at home and abroad.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

A method for preparing high-purity antimony, wherein antimony trioxide and ethylene glycol are used to generate ethylene glycol antimony, and the purified ethylene glycol antimony is heated and reacted with sodium carbonate to obtain high-purity antimony. The method has a good effect on the preparation of high-purity antimony, and can directly prepare 4N antimony with an impurity content of ≤100ppm; the direct yield is high, the cycle is short, and the production cost is low; the processing volume is large, suitable for industrial-scale production, and meets the market demand in the high-tech field at home and abroad; the production environment is not harsh, easy to operate and control, and convenient for management and maintenance; the equipment required is simple, the investment is small, and the start-up is fast.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a method for preparing antimony, and in particular to a method for preparing high-purity antimony. Background Art

[0002] my country is a major producer and consumer of antimony, and its antimony reserves rank first in the world. However, in addition to major products such as antimony ingots, antimony oxide, ethylene glycol antimony, and sodium antimonate, there are not many other antimony products in my country. The United States, Japan, and Western Europe are countries that lack antimony resources. They often import crude antimony from my country, and after deep processing, they sell it back to my country at high prices, making huge profits, especially high-tech products. With the development of high-tech, the use of high-purity metals is becoming more and more extensive. 4N, 5N, and 6N metal antimony have been widely used and have high economic value. However, due to the limitations of domestic production processes, its output is difficult to increase, and there are high technical requirements for various control links of the process, so there has been no large-scale industrial production.

[0003] High-purity antimony was previously mostly used in the military industry, but with the advancement of technology, it has begun to shift to civilian industries, such as electronics, energy, refrigeration, metallurgy, aerospace and other industries. New refrigeration materials made from high-purity antimony and other materials will promote the pace of my country's refrigeration equipment industry, making refrigeration equipment develop in the direction of miniaturization, noiselessness, refrigerant-free and pollution-free; whether it is solid or liquid fuel, or the comprehensive utilization of solar energy and waste heat, semiconductor materials containing high-purity antimony will be used. The research and development of high-purity antimony has a very broad application prospect and potential economic value. Summary of the invention

[0004] The technical problem to be solved by the present invention is to overcome the above-mentioned defects in the prior art and provide a method for preparing high-purity antimony with a simple method and good purification effect.

[0005] In order to meet the domestic market, especially the high-end technology field, demand for high-purity antimony materials, the present invention aims to provide a method for preparing high-purity antimony that is both economical and efficient and suitable for large-scale production. The high-purity antimony prepared by this method has a total impurity content of ≤100ppm, which can be used as a product to meet the needs of the domestic and foreign markets, and can also be used as a raw material to further produce 5N and 6N high-purity antimony products, providing strategic needs for the development of China's high-tech.

[0006] The technical solution adopted by the present invention to solve the technical problem is as follows: a method for preparing high-purity antimony, using antimony trioxide and ethylene glycol to generate ethylene glycol antimony, covering the purified ethylene glycol antimony with sodium carbonate, removing the covering slag after heating reaction, and obtaining high-purity antimony.

[0007] The high-purity antimony preparation of the present invention has good effect, high direct yield, short cycle, low production cost, simple equipment and low investment.

[0008] Preferably, the reaction conditions of antimony trioxide and ethylene glycol are: temperature 140-150° C., vacuum degree -0.85 MPa-0.95 MPa, and reaction time 2-4 hours.

[0009] By adopting the above technical solution, a better reaction effect is achieved.

[0010] Preferably, the mass ratio of antimony trioxide to ethylene glycol is 1:8-10.

[0011] By adopting the above technical solution, a better reaction effect is achieved.

[0012] Preferably, the mass of sodium carbonate is 5% to 10% of the purified antimony glycolate.

[0013] Preferably, the heating temperature is 1100-1200°C.

[0014] Preferably, the heating time is 2 to 6 hours.

[0015] When heated, antimony is generated through high-temperature reaction, and unnecessary foreign matter such as low-density carbon and bubbles float out of the antimony liquid.

[0016] By adopting the above technical solution, a better reaction effect is achieved.

[0017] Preferably, the purity of the antimony trioxide is above 99%.

[0018] By adopting the above technical solution, the purity of the product can be guaranteed.

[0019] More preferably, the purity of the antimony trioxide is above 99.5%.

[0020] By adopting the above technical solution, the purity of the product can be guaranteed.

[0021] Preferably, the ethylene glycol is industrial pure.

[0022] By adopting the above technical solution, the purity of the product can be guaranteed.

[0023] Preferably, the sodium carbonate is analytically pure.

[0024] By adopting the above technical solution, the purity of the product can be guaranteed.

[0025] Preferably, the method for purifying antimony glycolate includes: filtering using a filter disc made of carbon fiber material while hot and separating by cooling and crystallization.

[0026] By adopting the above technical solution, a better purification effect is achieved.

[0027] Preferably, the filtering temperature is 120-130°C.

[0028] By adopting the above technical solution, a better filtering effect is achieved.

[0029] Preferably, the temperature of the cooling crystallization separation is 30-40°C.

[0030] At this temperature, crystals are generated and grow larger and coarser, making them easier to separate. By adopting the above technical solution, a better purification effect is achieved.

[0031] Antimony trioxide and ethylene glycol raw materials contain a certain amount of impurities, but the impurity oxides such as arsenic, lead, iron, copper, bismuth, tellurium, selenium, and nickel basically do not react with ethylene glycol. After antimony trioxide and ethylene glycol generate ethylene glycol antimony, the impurity oxides still remain in the reaction solution. Through purification methods such as filtration, most of the impurities can be retained on the filter cloth and removed.

[0032] Cooling crystallization can be carried out directly after hot filtration, and crystallization can be promoted by cooling with the aid of coolant, stirring, etc. After the crystallization of ethylene glycol antimony, solid-liquid separation is achieved to realize the purification of ethylene glycol.

[0033] The purified ethylene glycol antimony is carbonized and self-reduced under high temperature conditions to obtain antimony element, and a small amount of sodium carbonate is used to remove arsenic.

[0034] Beneficial effects of the present invention:

[0035] (1) The high-purity antimony preparation effect of the present invention is very good, and 4N antimony with an impurity content of ≤100ppm can be directly prepared;

[0036] (2) The high-purity antimony preparation of the present invention has a high direct yield, a short cycle and low production cost;

[0037] (3) The high-purity antimony preparation and processing capacity of the present invention is large, which is suitable for industrial-scale production and meets the market demand in the high-tech field at home and abroad;

[0038] (4) The preparation of high-purity antimony according to the present invention is not demanding on the production environment and is easy to operate and control, and is convenient for management and maintenance;

[0039] (5) The method for preparing high-purity antimony of the present invention requires simple equipment, low investment, and quick start-up. DETAILED DESCRIPTION

[0040] The present invention will be further described below with reference to the embodiments.

[0041] The raw materials used in the embodiments of the present invention are all obtained through conventional commercial channels. Example 1

[0042] The present invention adopts 99.5% antimony trioxide as raw material, and its components are (mass percentage): Sb 83.32%, As 0.045%, Pb 0.077%, Fe 0.0018%, Cu 0.0012%, Bi 0.0005%, Se 0.0004%, Te 0, Ni 0.

[0043] The method for preparing high purity antimony in this embodiment:

[0044] Take 200g of the above antimony trioxide and 1600g of 99.8% industrial pure ethylene glycol, add them into a 2L vacuum reactor, control the temperature at 145℃, control the pressure at -0.85MPa, react for 2h, release the pressure, cool to 130℃, pump into a carbon fiber filter cylinder for filtration, and the purified ethylene glycol antimony enters the crystallization kettle for cooling and crystallization for about 4h at 30℃, filter, and obtain 266g of crystallized ethylene glycol antimony; the ethylene glycol mother liquor (filtrate) is reserved for other use. The crystallized ethylene glycol antimony was sent for inspection, and the composition was (mass percentage): Sb 56.45%, As 0.0006%, Pb 0.0012%, Fe 0.0015%, Cu 0.0002%, Bi 0.0001%, Se 0.0002%, Te 0.0001%, Ni 0;

[0045] Then take 250g of the above crystallized antimony glycol and put it into a corundum crucible, add 20g of analytical pure sodium carbonate to cover the crystallized antimony glycol, place it in a muffle furnace, heat it to 1200℃, react at constant temperature for 2h, keep it warm for clarification for 2h and remove the covering slag (heating for 4h in total), and stop heating. 98.8g of antimony is obtained and sent for inspection. The impurity components are (mass percentage): As 0.0005%, Pb 0.0036%, Fe0.0008%, Cu 0.0002%, Bi 0.0002%, Se 0.0002%, Te 0.0002%, Ni 0, the total impurity mass is 53ppm, and Sb 99.9947% is obtained by reduction method, which meets the 4N standard. Example 2

[0046] The present invention adopts 99.8% antimony trioxide as raw material, and its components are (mass percentage): Sb 83.37%, As 0.060%, Pb 0.030%, Fe 0.0008%, Cu 0.0020%, Bi 0.0006%, Se 0.0003%, Te 0.0009%, Ni 0.

[0047] The method for preparing high purity antimony in this embodiment:

[0048] Take 200g of the above antimony trioxide and 1600g of 99.8% industrial pure ethylene glycol, add them into a 2L vacuum reactor, control the temperature at 140℃, control the pressure at -0.95MPa, react for 4h, release the pressure, cool to 120℃, pump into a carbon fiber filter cylinder for filtration, and the purified ethylene glycol antimony enters the crystallization kettle for cooling and crystallization for about 3h at 40℃, filter, and obtain 263g of crystalline ethylene glycol antimony; the ethylene glycol mother liquor (filtrate) is reserved for other use. The crystallized ethylene glycol antimony was sent for inspection, and the composition was (mass percentage): Sb 56.39%, As 0.0005%, Pb 0.0016%, Fe 0.0018%, Cu 0.0002%, Bi 0.0001%, Se 0.0003%, Te 0.0001%, Ni 0;

[0049] Then take 250g of the above crystallized antimony glycol and put it into a corundum crucible, add 25g of analytical pure sodium carbonate to cover the crystallized antimony glycol, place it in a muffle furnace, heat it to 1100℃, react at constant temperature for 4h, keep it warm for clarification for 2h and remove the covering slag (heating for 6h in total), and stop heating. 98.1g of antimony is obtained and sent for inspection. The impurity components are (mass percentage): As 0.0002%, Pb 0.0010%, Fe0.0009%, Cu 0.0006%, Bi 0.00010%, Se 0.0005%, Te 0.0002%, Ni 0.0001%, total impurities 45ppm, Sb 99.9955% is obtained by reduction method, reaching 4N standard. Example 3

[0050] The present invention adopts 99.9% antimony trioxide as a raw material, and its composition is (mass percentage): Sb 83.47%, As 0.0028%, Pb 0.0033%, Fe 0.0012%, Cu 0.0018%, Bi 0.0005%, Se 0.0002%, Te 0.0003% and Ni 0.0002%.

[0051] The method for preparing high purity antimony in this embodiment:

[0052] Take 200g of the above antimony trioxide and 1600g of 99.8% industrial pure ethylene glycol, add them into a 2L vacuum reactor, control the temperature at 150℃, control the pressure at -0.90MPa, react for 3h, release the pressure, cool to 125℃, pump into a carbon fiber filter cylinder for filtration, and the purified ethylene glycol antimony enters the crystallization kettle for cooling and crystallization for about 5h at 35℃, filter, and obtain 269g of crystallized ethylene glycol antimony; the ethylene glycol mother liquor (filtrate) is reserved for other use. The crystallized ethylene glycol antimony was sent for inspection, and the composition was (mass percentage): Sb 56.58%, As 0.0001%, Pb 0.0002%, Fe 0.0013%, Cu 0.0004%, Bi 0.0004%, Se 0.0002%, Te 0.0006%, Ni 0.0001%;

[0053] Then take 250g of the above crystallized antimony glycol and put it into a corundum crucible, add 12.5g of analytical pure sodium carbonate to cover the crystallized antimony glycol, place it in a muffle furnace, heat it to 1150℃, react at constant temperature for 3h, keep it warm for clarification for 2h and remove the covering slag (heating for 5h in total), and stop heating. 98.9g of antimony is obtained and sent for inspection. The impurity components are (mass percentage): As 0.0001%, Pb 0.0006%, Fe0.0011%, Cu 0.0005%, Bi 0.0006%, Se 0.0003%, Te 0.0003%, Ni 0.0001%, total impurity content 36ppm, Sb 99.9964% is obtained by reduction method, reaching 4N standard. Example 4

[0054] The present invention adopts 99.5% antimony trioxide as raw material, and its components are (mass percentage): Sb 83.32%, As 0.045%, Pb 0.077%, Fe 0.0018%, Cu 0.0012%, Bi 0.0005%, Se 0.0004%, Te 0, Ni 0.

[0055] The method for preparing high purity antimony in this embodiment:

[0056] Take 300kg of the above antimony trioxide and 3000kg of 99.8% industrial pure ethylene glycol, add 5m 3In the vacuum reactor, the temperature was controlled at 145°C and the pressure was controlled at -0.85MPa. The reaction was continued for 4 hours. The pressure was released and the temperature was lowered to 130°C. The product was then pumped into a carbon fiber filter cylinder for filtration. The purified antimony glycol was then put into a crystallization kettle for cooling and crystallization. The temperature was 36°C for about 6 hours. After filtration, 398.5 kg of crystallized antimony glycol was obtained. The mother liquor (filtrate) of ethylene glycol was reserved for further use. The crystallized antimony glycol was sent for inspection, and the composition was (mass percentage): Sb 56.45%, As 0.0006%, Pb0.0016%, Fe 0.0015%, Cu 0.0002%, Bi 0.0003%, Se 0.0005%, Te 0.0001%, Ni 0.0001%;

[0057] Then take 500g of the above crystallized antimony glycol and put it into a corundum crucible, add 25g of analytical pure sodium carbonate to cover the crystallized antimony glycol, place it in a muffle furnace, heat it to 1100℃, react at constant temperature for 4h, keep it warm for clarification for 2h and remove the covering slag (heating for 6h in total), and stop heating. 197g of antimony is obtained and sent for inspection. The impurity components are (mass percentage): As 0.0004%, Pb 0.0028%, Fe0.0010%, Cu 0.0004%, Bi 0.0005%, Se 0.0006%, Te 0.0001%, Ni 0.0001%, the total impurity content is 59ppm, and Sb 99.9941% is obtained by reduction method, which meets the 4N standard. Example 5

[0058] The present invention adopts 99.5% antimony trioxide as raw material, and its components are (mass percentage): Sb 83.32%, As 0.045%, Pb 0.077%, Fe 0.0018%, Cu 0.0012%, Bi 0.0005%, Se 0.0004%, Te 0, Ni 0.

[0059] The method for preparing high purity antimony in this embodiment:

[0060] Take 400kg of the above antimony trioxide and 3200kg of 99.8% industrial pure ethylene glycol, add 5m 3 In the vacuum reactor, the temperature was controlled at 150°C and the pressure was controlled at -0.95MPa. The reaction was carried out for 4 hours, the pressure was released, the temperature was lowered to 120°C, and the purified antimony glycol was sent to the crystallization kettle for cooling and crystallization for about 8 hours at 30°C. After filtration, 530kg of crystallized antimony glycol was obtained, and the mother liquor (filtrate) of ethylene glycol was reserved for further use. The crystallized antimony glycol glycol was sent for inspection, and the composition was (mass percentage): Sb 56.48%, As 0.0005%, Pb0.0030%, Fe 0.0010%, Cu 0.0003%, Bi 0.0006%, Se 0.0004%, Te 0.0001%, Ni 0.0001%;

[0061] Then take 500g of the above crystallized antimony glycol and put it into a corundum crucible, add 40g of analytical pure sodium carbonate to cover the crystallized antimony glycol, place it in a muffle furnace, heat it to 1200℃, react at constant temperature for 3h, keep it warm for clarification for 2h and remove the covering slag (heating for 5h in total), and stop heating. 196g of antimony is obtained and sent for inspection. The impurity components are (mass percentage): As 0.0003%, Pb 0.0032%, Fe0.0009%, Cu 0.0004%, Bi 0.0005%, Se 0.0004%, Te 0.0001%, Ni 0.0001%, the total impurity content is 46ppm, and Sb 99.9954% is obtained by reduction method, reaching 4N standard.

Claims

1. A method for preparing high-purity antimony, characterized in that: Antimony trioxide and ethylene glycol are used to generate ethylene glycol antimony, and the purified ethylene glycol antimony is covered with sodium carbonate, and the covering slag is removed after heating reaction to obtain high-purity antimony; the heating temperature is 1100-1200°C; the heating time is 2-6 hours; the mass of sodium carbonate is 5%-10% of the purified ethylene glycol antimony.

2. The method for preparing high-purity antimony according to claim 1, characterized in that: The reaction conditions of antimony trioxide and ethylene glycol are: temperature 140-150° C., vacuum degree -0.85 MPa-0.95 MPa, and reaction time 2-4 hours.

3. The method for preparing high-purity antimony according to claim 1 or 2, characterized in that: The mass ratio of antimony trioxide to ethylene glycol is 1:8~10.

4. The method for preparing high-purity antimony according to claim 1, characterized in that: The purity of the antimony trioxide is above 99%.

5. The method for preparing high-purity antimony according to claim 1, characterized in that: The ethylene glycol is industrial grade; the sodium carbonate is analytical grade.

6. The method for preparing high-purity antimony according to claim 1, characterized in that: The purification method of ethylene glycol antimony includes: filtering with a carbon fiber filter while hot and cooling and crystallization separation.

7. The method for preparing high-purity antimony according to claim 6, characterized in that: The filtration temperature is 120-130°C.

8. The method for preparing high-purity antimony according to claim 6, characterized in that: The temperature of the cooling crystallization separation is 30-40°C.

Citation Information

Cited By

  • Preparation method of 5N high-purity antimony

    CN122168915A