A Prussian blue analog-porous carbon composite material and its preparation method and application
Through the combination of Prussian blue analogues and porous carbon composite materials, highly selective lithium ion recovery electrode materials are designed, and capacitive deionization technology is used to achieve efficient recovery of lithium ions, solving the high cost and pollution problems in lithium battery recovery and achieving Effective recycling of lithium resources.
Patent Information
- Application Number
- CN202410299366.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-03-15
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2044-03-15
AI Technical Summary
Existing lithium battery recycling technology is costly, prone to secondary pollution and takes a long time, and the recycling rate of lithium resources is low, making it difficult to effectively solve the problem of lithium battery waste.
Prussian blue analogue-porous carbon composite material is used as the negative electrode material in capacitive deionization technology. By combining with biomass-derived tertiary porous carbon material, a highly selective and efficient lithium ion recovery electrode material is designed, utilizing capacitance Deionization device performs selective recovery of lithium ions.
It achieves efficient and selective recovery of lithium ions, reduces production costs, avoids secondary pollution, and the process is simple and easy for industrial production, solving the problem of lithium resource recycling.
Smart Images

Figure CN117976423B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of capacitive deionization, and in particular to a Prussian blue analog-porous carbon composite material and a preparation method and application thereof. Background Art
[0002] With the rapid growth of the mobile device, electric vehicle and large-scale energy storage system markets, the consumption of lithium has reached an unprecedented high level in recent years. The core component of lithium batteries is the positive electrode material, which is mostly lithium-ion material. The positive electrode materials of lithium batteries currently sold on the market mainly include lithium cobalt oxide materials, lithium iron phosphate materials, lithium manganese oxide materials and the latest developed nickel cobalt manganese oxide ternary composite materials. Research and investigation found that the service life of lithium batteries equipped with common electronic products is only 5-20 years, and the average life is only 8 years. The service life of lithium batteries loaded on new energy electric vehicles is only 3-5 years. Therefore, the generation and treatment of waste lithium batteries has become the focus of global environmental protection and resource recycling. From the perspective of green and sustainable development, lithium urgently needs to be recycled, but less than 1% of lithium waste in the world is recycled. Waste lithium batteries contain 5-15% cobalt and 2-7% lithium, which are industrial waste, and metals such as lithium, nickel, cobalt, copper and manganese are scarce resources. Therefore, this "waste" stream is a potential "urban mine". In addition, lithium extraction from salt lakes is also an effective way to solve the shortage of lithium resources.
[0003] Researchers often use precipitation, extraction and ion exchange to achieve metal separation and recovery. The commonly used precipitation method is to add a precipitant to the leaching solution to react with the metal to form a precipitate, thereby separating the metal. Traditional lithium recovery methods have problems such as high cost, easy to cause secondary pollution and long time consumption. Summary of the invention
[0004] Purpose of the invention: In order to address the deficiencies in the prior art, the present invention aims to provide a Prussian blue analogue-porous carbon composite material with high selectivity for lithium ions, and the present invention also provides a preparation method and application of the Prussian blue analogue-porous carbon composite material.
[0005] Technical solution: The Prussian blue analogue-porous carbon composite material of the present invention is composited with a porous carbon material and a Prussian blue analogue in a mass ratio of 1:0.2-1.2, preferably, the mass ratio is 1:0.4.
[0006] Furthermore, the porous carbon material is a tertiary porous carbon material derived from biomass; the biomass is plant straw (such as corn straw, sorghum straw, etc.), bamboo or wood, etc., preferably, the biomass is corn straw.
[0007] Furthermore, the porous carbon material is derived from biomass with a fixed framework structure, is a three-level porous interconnected network and maintains the original skeleton structure of the biomass, with a specific surface area of 1700-2000m 2 / g.
[0008] Furthermore, the Prussian blue analogue is CuHCF.
[0009] The method for preparing the Prussian blue analog-porous carbon composite material of the present invention comprises the following steps:
[0010] (1) first dispersing the porous carbon material in a solvent, then adding a transition metal salt to continue dissolving to obtain a mixed solution;
[0011] (2) dropping a solution containing potassium ferrocyanide or potassium ferrocyanide into the mixed solution, stirring the solution thoroughly and then performing an aging reaction. After the reaction is completed, collecting the precipitate by centrifugation, washing and drying the precipitate to obtain a Prussian blue analog-porous carbon composite material.
[0012] Furthermore, the usage ratio of the porous carbon material to potassium ferrocyanide or potassium ferrocyanide is 1g:0.005-0.015mol; the molar ratio of the transition metal salt to potassium ferrocyanide or potassium ferrocyanide is 2:1; the transition metal salt (the transition metal is Cu) exists in the form of chloride, sulfate, nitrate, etc.
[0013] Furthermore, the aging reaction conditions are: reacting at room temperature for 12-24 hours.
[0014] Furthermore, the preparation method of the porous carbon material is as follows: the biomass material with a fixed framework structure is activated by a pore-forming agent, calcined, cleaned and dried to obtain a porous carbon material; the parameters of the pore-forming agent activation are: soaking in the pore-forming agent solution for 12-24 hours; the parameters of the calcination are: heating to 700-900°C at a rate of 5-10°C / min and keeping warm for 2-4 hours under an inert atmosphere.
[0015] Furthermore, the pore-forming agent is potassium bicarbonate, sodium bicarbonate or sodium chloride, and the pore-forming agent solution is a saturated solution; the cleaning includes acid washing and water washing; the solution used for the acid washing is dilute hydrochloric acid, and the drying treatment also includes acid immersion, the acid is concentrated nitric acid, the acid immersion temperature is 70-80°C, and the time is 2-4h, so as to enhance the wetting performance of the surface of the porous carbon material.
[0016] The Prussian blue analogue-porous carbon composite material of the present invention is used as a capacitor deionization electrode material in selective lithium recovery.
[0017] Furthermore, the application method is: using a Prussian blue analog-porous carbon composite material as the negative electrode material of the CDI unit, using an aminated porous carbon material electrode as the positive electrode material of the CDI unit, and recovering lithium from the waste lithium battery leachate in a CDI device configured by a CDI unit, a conductivity meter, a peristaltic pump, a water storage tank, and a DC power supply.
[0018] Furthermore, in the above method: a Prussian blue analog-porous carbon composite material is used as a negative electrode material (pseudocapacitor) to selectively recover lithium ions in the lithium battery leachate; a porous carbon material functionalized with positively charged functional groups is used as a positive electrode material (double-layer capacitor) to efficiently adsorb anions in the leachate. The introduction of positively charged functional groups can inhibit the influence of co-existing ions during the electrical adsorption process, enhance the wettability of the carbon material surface, and play the role of an ion exchange membrane.
[0019] Furthermore, the concentration of lithium ions in the waste lithium battery leachate is 200-1000ppm, and the parameters of lithium recovery are: the adsorption applied voltage is 1.2-1.8V, and the desorption method is short circuit or applying a reverse voltage of 1.2-1.8V.
[0020] Principle of the invention: The present invention utilizes capacitive deionization technology to selectively recover lithium ions from waste lithium battery leachate. The core component of the capacitive deionization (CDI) device is the electrode material. Therefore, if the problem of efficient separation and recovery of lithium ions in lithium battery leachate is to be fundamentally solved, it is necessary to design a negative electrode material with specific selective electrical adsorption for lithium ions. Many battery electrode materials can interact with lithium ions. Prussian blue analogues (PBAs) have three-dimensional micro / nano structures and adjustable chemical compositions, and there are large gaps in the lattice. In addition, Prussian blue analogues (especially copper ferrocyanide CuHCF) are a typical inorganic electroactive material. The electroactivity and stability in an acidic environment are better than those under alkaline or neutral conditions. It has low cost, simple preparation method and is environmentally friendly. The Prussian blue analog is a face-centered cubic lattice (space Fm3m) structure, and the cyano group is connected to the iron ions at the vertices as the edges of the cube, wherein the iron ions of the same valence are diagonal to each other on each plane, and lithium ions can be wrapped in each cube and move between the center positions of the semi-filled body. The lattice size and negative potential properties of the Prussian blue analog show high selectivity for lithium ions, so the Prussian blue analog is the most potential CDI negative electrode material. In order to inhibit the agglomeration of Prussian blue analog particles, enhance their conductivity and fully expose the electrical adsorption sites, promote the transmission of lithium battery leachate inside the electrode, and improve the selective recovery efficiency of lithium ions, the present invention loads the Prussian blue analog on a tertiary porous carbon material derived from biomass to prepare a Prussian blue analog-porous carbon composite material.
[0021] The present invention utilizes capacitive deionization technology to achieve highly selective separation and recovery of lithium ions in lithium battery leachate. No toxic products are generated during the entire recovery process. The invention has broad application prospects and high commercial value. It can not only meet the needs of ecological environmental protection, but also realize the comprehensive utilization of resources in the lithium battery industry.
[0022] Beneficial effects: Compared with the prior art, the present invention has the following significant advantages:
[0023] (1) The Prussian blue analogue-porous carbon composite material prepared by the present invention uses a tertiary porous carbon material derived from biomass as a carrier. The lattice size and negative potential properties of the Prussian blue analogue show high selectivity for lithium ions, so the Prussian blue analogue is the CDI negative electrode material with the greatest application potential; at the same time, the porous carbon material as a carrier can inhibit the agglomeration of Prussian blue analogue particles, enhance its conductivity and fully expose the electrical adsorption sites, promote the transmission of lithium battery leachate inside the electrode, so as to improve the selective recovery efficiency of lithium ions.
[0024] (2) The present invention uses a biomass-derived tertiary porous carbon material functionalized with positively charged functional groups as a positive electrode material (double-layer capacitor) to efficiently adsorb anions in the leachate. The introduction of positively charged functional groups can inhibit the influence of co-existing ions during the electrical adsorption process, enhance the wettability of the carbon material surface, and act as an ion exchange membrane.
[0025] (3) The present invention recovers lithium ions and can solve the problem of insufficient lithium resources.
[0026] (4) The present invention uses cheap and abundant biomass materials as raw materials, has low production cost, is green and economical, has simple process, is easy to operate, and is easy to industrialize. It is conducive to further research on capacitive deionization technology and also provides a new choice and new idea for the design of electrode materials for capacitive deionization technology. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1 The high temperature carbonization scanning images of corn stalks as the initial material at different magnifications prepared in Example 1 of the present invention;
[0028] Figure 2 The (ab)KHCO prepared in Example 1 of the present invention using corn stalks as the starting material 3 Auxiliary pore scanning image; (c) KHCO 3 Transmission electron microscope image of assisted pore formation; (d) pore size distribution of three-dimensional porous carbon materials;
[0029] Figure 3The morphological structure characterization of the Prussian blue analog-porous carbon composite material prepared in Example 1 of the present invention: (a) scanning image; (b) XRD pattern, wherein PC is the abbreviation of porous carbon material;
[0030] Figure 4 This is a comparison diagram of the cyclic voltammetric performance of the Prussian blue analogue-porous carbon composite material and the porous carbon material prepared in Example 1 of the present invention, wherein PBA@PC is a Prussian blue analogue-porous carbon composite material, and PC is a porous carbon material;
[0031] Figure 5 This is a comparison chart of the charge and discharge performance of the Prussian blue analog-porous carbon composite material and the porous carbon material prepared in Example 1 of the present invention;
[0032] Figure 6 This is a graph showing the test results of the lithium recovery performance of the Prussian blue analog-porous carbon composite material prepared in Example 1 of the present invention as a capacitor deionization negative electrode material;
[0033] Figure 7 (a) Lithium adsorption curve of the Prussian blue analog-porous carbon composite material prepared in Example 1 of the present invention as a capacitor deionization negative electrode material, and (b) Kim-Yoon curve. DETAILED DESCRIPTION
[0034] The present invention is further described below in conjunction with specific embodiments and drawings.
[0035] Example 1: The Prussian blue analog-porous carbon composite material provided in this example is composed of a tertiary porous carbon material derived from biomass and CuHCF in a mass ratio of 1:0.4, and the preparation method specifically includes the following steps:
[0036] A1. Wash and dry the corn stalks, soak them in a saturated potassium bicarbonate solution for 24 hours, take them out and dry them, and place them in a tube furnace for high-temperature calcination in a nitrogen atmosphere at a heating rate of 10°C / min. When the calcination temperature reaches 800°C, keep it warm for 3 hours, then cool the calcined product to room temperature, wash it three times with a hydrochloric acid solution (the hydrochloric acid solution is a mixture of equal volumes of concentrated hydrochloric acid with a mass fraction of 37% and deionized water), filter it, wash it with deionized water until it is neutral, and dry it at 60°C to obtain a tertiary porous carbon material derived from biomass;
[0037] B1. The tertiary porous carbon material derived from biomass was mixed with the Prussian blue analog precursor reaction solution. 0.1 g of the tertiary porous carbon material derived from biomass was dissolved in 100 mL of deionized water and stirred for 15 min. The solution was marked as solution A. 0.01 mol Cu(NO 3 ) 2Dissolve in solution A and stir again for 15 min to obtain a mixed solution; add 0.005 mol K 4 [Fe(CN) 6 ] was dissolved in 100 mL of deionized water and marked as solution B, and stirred for 15 min. Solution B was added dropwise to the mixed solution using a burette, and stirred continuously for 15 min during the process, and then aged at room temperature for 24 h, centrifuged, and washed with deionized water and ethanol, and then the precipitate was collected and placed in an oven to obtain a Prussian blue analog-porous carbon composite material.
[0038] The prepared Prussian blue analog-porous carbon composite material was subjected to the following tests:
[0039] (1) The structure of the corn straw direct carbonization material prepared in this example was observed using a Quanta 200FEG field emission scanning electron microscope (FESEM). Figure 1 As shown in the figure, corn stover, which is abundant, cheap and renewable, is selected as the raw material. Due to its inherent porous skeleton structure, it is conducive to the pore-forming agent KHCO 3 Adsorption;
[0040] (2) The structure of the corn straw-derived porous carbon material prepared in this embodiment was observed using a Quanta 200FEG field emission scanning electron microscope (FESEM), a JEOL 2010 high-resolution transmission electron microscope, and a Tristar 3020M specific surface area and pore size distribution tester. Figure 2 As shown in (a), (b) and (c), KHCO 3 After auxiliary activation pyrolysis, a high specific surface area tertiary porous carbon material was successfully prepared, with a specific surface area of up to 1926m 2 g -1 , and from the pore size distribution diagram, we can see that ( Figure 2 In (d)), the obtained carbon material has a tertiary pore structure, which is very beneficial for the subsequent modification of Prussian blue analogs. As a CDI electrode material, it will also enhance the transmission of electrolyte solutions and promote efficient adsorption / desorption of ions;
[0041] (3) The structure and composition of the Prussian blue analog-porous carbon composite material prepared in this example were tested using a Quanta 200FEG field emission scanning electron microscope (FESEM) and a Philips X'Pert X-ray diffractometer. Figure 3 As shown, the Prussian blue analogue was successfully loaded on the porous carbon surface, and the crystal structure of the Prussian blue analogue was consistent with CuHCF (PDF#23-0215). Figure 3 (b) is the Prussian blue analog-porous carbon composite material obtained in the step of Example 1 of the present invention ( Figure 3X-ray diffraction pattern of CuHCF / PC in (the abscissa represents angle and the ordinate represents intensity).
[0042] (4) The biomass-derived tertiary porous carbon material and the Prussian blue analog-porous carbon composite material prepared in steps A1 and B1 of Example 1 of the present invention were tested using a CHI 660E electrochemical workstation to obtain the following: Figure 4 The electrochemical cyclic voltammetry performance test diagram shown in FIG. Figure 4 (a) is the material obtained in steps A1 and B1 in Example 1 of the present invention at 100 mv s -1 Cyclic voltammogram at scan rate (the horizontal axis represents voltage and the vertical axis represents current), Figure 4 (b) is the cyclic voltammogram of the Prussian blue analog-porous carbon composite material obtained in step B1 of Example 1 of the present invention at different scan rates. Figure 4 It can be seen that the Prussian blue analogue-porous carbon composite material (PBA@PC) prepared in step B1 in Example 1 of the present invention shows obvious redox peaks in the cyclic voltammetry curve compared with the tertiary porous carbon material (PC) derived from biomass, including double layer capacitance and partial pseudocapacitance, indicating that the capacitance performance of the tertiary porous carbon material is enhanced after modification with the Prussian blue analogue.
[0043] (5) The electrochemical performance of the biomass-derived tertiary porous carbon material and the Prussian blue analog-porous carbon composite material prepared in steps A1 and B1 of Example 1 of the present invention was tested using a CHI 660E electrochemical workstation, thereby obtaining the following: Figure 5 The constant voltage charge and discharge performance test diagram shown in FIG. Figure 5 (a) is the charge-discharge curve of the material obtained in step A1 of Example 1 of the present invention at different current densities (the abscissa represents time, and the ordinate represents voltage), Figure 5 (b) is the charge-discharge curve of the Prussian blue analog-porous carbon composite material prepared in step B1 of Example 1 of the present invention at different current densities. Figure 5 It can be seen that the Prussian blue analogue-porous carbon composite material prepared in step B1 of Example 1 of the present invention has a higher specific capacitance than the tertiary porous carbon material derived from biomass and has better stability at different current densities, indicating that the Prussian blue analogue modification enhances the capacitance performance of the tertiary porous carbon material. -1 When 160.06F g -1 Increased to 206.87F g -1 .
[0044] (7) The Prussian analog-porous carbon composite material finally obtained in Example 1 of the present invention was used as a CDI electrode material and assembled together with an aminated porous carbon material (preparation method: 100 mg of the biomass-derived tertiary porous carbon material obtained in step A1 was dispersed in an acetone solution, ultrasonically treated, 200 ul of a silane coupling agent aminopropyltriethoxysilane (APTES) was added dropwise, and ultrasonication was continued until the acetone was completely volatilized to obtain the aminated porous carbon material) into a CDI unit for lithium recovery performance testing. The test voltage was 1.2 V, and lithium recovery was performed in a lithium solution with a concentration of 500 mg / L, thereby obtaining the following: Figure 6 The schematic diagram of lithium recovery performance is shown; wherein, Figure 6 is a CDI unit lithium recovery performance cycle diagram (the horizontal axis represents time and the vertical axis represents conductivity), Figure 6 It can be seen that the CDI unit assembled with the Prussian blue analogue-porous carbon composite material prepared in step B1 of Example 1 of the present invention and the aminated biomass-derived tertiary porous carbon material has a faster lithium recovery rate (1.35 mg / g / min) and a higher lithium adsorption capacitance (34.59 mg / g) in a lithium solution with a concentration of 500 mg / L.
[0045] (8) The Prussian blue analog-porous carbon composite material finally prepared in Example 1 of the present invention is used as a CDI electrode material and assembled together with the aminated porous carbon material into a CDI unit for lithium recovery performance testing, and the test data is calculated and analyzed to obtain the following: Figure 7 The lithium recovery performance diagram shown in FIG. Figure 7 (a) is the curve of the change of the conductivity of the lithium solution over time. Figure 7 (b) Kim-Yoon curve diagram in . Figure 7 It can be seen that the CDI unit assembled with the Prussian blue analogue-porous carbon composite material prepared in step B1 of Example 1 of the present invention and the aminated porous carbon material has better lithium recovery performance.
[0046] Example 2: The Prussian blue analog-porous carbon composite material provided in this example is composited with a biomass-derived tertiary porous carbon material and CuHCF in a mass ratio of 1:0.2, and the preparation method specifically includes the following steps:
[0047] A2. Wash and dry the corn stalks, soak them in a saturated potassium bicarbonate solution for 24 hours, take them out and dry them, and place them in a tubular furnace for high-temperature calcination in a nitrogen atmosphere at a heating rate of 10°C / minute. When the calcination temperature reaches 700°C, keep it warm for 3 hours, then cool the calcined product to room temperature, wash it three times with a hydrochloric acid solution (the hydrochloric acid solution is a mixture of equal volumes of concentrated hydrochloric acid with a mass fraction of 37% and deionized water), filter it, wash it with deionized water until it is neutral, and then dry it at 60°C to obtain a tertiary porous carbon material derived from biomass.
[0048] B2. The tertiary porous carbon material derived from biomass was mixed with the Prussian blue analog precursor reaction solution, 0.1 g of the tertiary porous carbon material derived from biomass was dissolved in 100 mL of deionized water, stirred for 15 min, marked as solution A, and then 0.005 mol Cu(NO 3 ) 2 Dissolve in solution A and stir again for 15 min to obtain a mixed solution; add 0.0025 mol K 4 [Fe(CN) 6 ] was dissolved in 100 mL of deionized water and marked as solution B, and stirred for 15 min. Solution B was added dropwise to the mixed solution using a burette, and stirred continuously for 15 min during the process, and then aged at room temperature for 24 h, centrifuged, and washed with deionized water and ethanol, and then the precipitate was collected and placed in an oven to obtain a Prussian blue analog-porous carbon composite material.
[0049] After testing, the Prussian blue analog-porous carbon composite material obtained in this embodiment has a current density of 0.5A g -1 When the specific capacitance is 160.27F g -1 , the CDI unit assembled with the aminated porous carbon material has a lithium recovery rate (1.15 mg / g / min) and lithium adsorption capacitance (29.59 mg / g) in a lithium solution with a lithium ion concentration of 500 mg / L.
[0050] Example 3: The Prussian blue analog-porous carbon composite material provided in this example is composited with a tertiary porous carbon material derived from biomass and CuHCF in a mass ratio of 1:0.8, and the preparation method specifically includes the following steps:
[0051] A3. Wash and dry the corn stalks, soak them in a saturated potassium bicarbonate solution for 12 hours, take them out and dry them, and place them in a tubular furnace for high-temperature calcination in a nitrogen atmosphere at a heating rate of 10°C / minute. When the calcination temperature reaches 900°C, keep it warm for 3 hours, then cool the calcined product to room temperature, wash it three times with a hydrochloric acid solution (the hydrochloric acid solution is a mixture of equal volumes of concentrated hydrochloric acid with a mass fraction of 37% and deionized water), filter it, wash it with deionized water until it is neutral, and then dry it at 60°C to obtain a tertiary porous carbon material derived from biomass.
[0052] B3. The tertiary porous carbon material derived from biomass was mixed with the Prussian blue analog precursor reaction solution, 0.1 g of the tertiary porous carbon material derived from biomass was dissolved in 100 mL of deionized water, stirred for 15 min, marked as solution A, and then 0.02 mol Cu(NO 3 ) 2 Dissolve in solution A and stir again for 15 min to obtain a mixed solution; add 0.01 mol K 4 [Fe(CN) 6 ] was dissolved in 100 mL of deionized water and marked as solution B, and stirred for 15 min. Solution B was added dropwise to the mixed solution using a burette, and stirred continuously for 15 min during the process, and then aged at room temperature for 12 h, centrifuged, and washed with deionized water and ethanol, and then the precipitate was collected and placed in an oven to obtain a Prussian blue analog-porous carbon composite material.
[0053] After testing, the Prussian blue analog-porous carbon composite material obtained in this embodiment has a current density of 0.5A g -1 When the specific capacitance is 178.10F g -1 , the CDI unit assembled with the aminated porous carbon material has a lithium recovery rate (1.21 mg / g / min) and lithium adsorption capacitance (30.25 mg / g) in a lithium solution with a lithium ion concentration of 500 mg / L.
[0054] Example 4: The Prussian blue analog-porous carbon composite material provided in this example is composed of a three-dimensional porous carbon material derived from biomass and CuHCF in a mass ratio of 1:1.2, and the preparation method specifically includes the following steps:
[0055] A4. Wash and dry the corn stalks, soak them in a saturated potassium bicarbonate solution for 18 hours, take them out and dry them, and place them in a tubular furnace for high-temperature calcination in a nitrogen atmosphere at a heating rate of 10°C / minute. When the calcination temperature reaches 800°C, keep it warm for 3 hours, then cool the calcined product to room temperature, wash it three times with a hydrochloric acid solution (the hydrochloric acid solution is a mixture of equal volumes of concentrated hydrochloric acid with a mass fraction of 37% and deionized water), filter it, wash it with deionized water until it is neutral, and then dry it at 60°C to obtain a tertiary porous carbon material derived from biomass.
[0056] B4. The tertiary porous carbon material derived from biomass was mixed with the Prussian blue analog precursor reaction solution, 0.1 g of the tertiary porous carbon material derived from biomass was dissolved in 100 mL of deionized water, stirred for 15 min, marked as solution A, and then 0.03 mol Cu(NO 3 ) 2 Dissolve in solution A and stir again for 15 min to obtain a mixed solution; add 0.015 mol K 4 [Fe(CN) 6 ] was dissolved in 100 mL of deionized water and marked as solution B, and stirred for 15 min. Solution B was added dropwise to the mixed solution using a burette, and stirred continuously for 15 min during the process, and then aged at room temperature for 24 h, centrifuged, and washed with deionized water and ethanol, and then the precipitate was collected and placed in an oven to obtain a Prussian blue analog-porous carbon composite material.
[0057] After testing, the Prussian blue analog-porous carbon composite material obtained in this embodiment has a current density of 0.5A g -1 When the specific capacitance is 158.10F g -1 , the CDI unit assembled with the aminated porous carbon material has a lithium recovery rate (1.13 mg / g / min) and lithium adsorption capacitance (28.25 mg / g) in a lithium solution with a lithium ion concentration of 500 mg / L.
[0058] Comparative Example 1: The difference from Example 1 is that: instead of using the tertiary porous carbon material derived from biomass as a carrier, the Prussian blue analogue is directly synthesized. 0.01 mol Cu(NO 3 ) 2 Dissolve in 100 mL of deionized water labeled solution A and stir for 15 min to obtain a mixed solution; add 0.005 mol K 4 [Fe(CN) 6] was dissolved in 100 mL of deionized water and marked as solution B, and stirred for 15 min. Solution B was added dropwise to the mixed solution using a burette, and stirred continuously during the process. After stirring for 15 min, the mixture was aged at room temperature for 24 h, centrifuged, and the precipitate was collected after washing with deionized water and ethanol and placed in an oven to obtain a Prussian blue analog.
[0059] After testing, the Prussian blue analogue obtained in this comparative example has a current density of 0.5A g -1 When the specific capacitance is 108.21Fg -1 , the CDI unit assembled with the aminated porous carbon material has a lithium recovery rate (1.02 mg / g / min) and lithium adsorption capacitance (25.51 mg / g) in a lithium solution with a lithium ion concentration of 500 mg / L.
[0060] Comparative Example 2: The Prussian blue analog-porous carbon composite material provided in this comparative example is composited with a three-dimensional porous carbon material derived from biomass and NiHCF in a mass ratio of 1:0.4, and the preparation method specifically includes the following steps:
[0061] A1. Wash and dry the corn stalks, soak them in a saturated potassium bicarbonate solution for 18 hours, take them out and dry them, and place them in a tubular furnace for high-temperature calcination in a nitrogen atmosphere at a heating rate of 10°C / minute. When the calcination temperature reaches 800°C, keep it warm for 3 hours, then cool the calcined product to room temperature, wash it three times with a hydrochloric acid solution (the hydrochloric acid solution is a mixture of equal volumes of concentrated hydrochloric acid with a mass fraction of 37% and deionized water), filter it, wash it with deionized water until it is neutral, and then dry it at 60°C to obtain a tertiary porous carbon material derived from biomass.
[0062] B1. The tertiary porous carbon material derived from biomass was mixed with the Prussian blue analog precursor reaction solution, 0.1 g of the tertiary porous carbon material derived from biomass was dissolved in 100 mL of deionized water, stirred for 15 min, marked as solution A, and then 0.01 mol Ni(NO 3 ) 2 Dissolve in solution A and stir again for 15 min to obtain a mixed solution; add 0.005 mol K 4 [Fe(CN) 6 ] was dissolved in 100 mL of deionized water and marked as solution B, and stirred for 15 min. Solution B was added dropwise to the mixed solution using a burette, and stirred continuously for 15 min during the process, and then aged at room temperature for 24 h, centrifuged, and washed with deionized water and ethanol, and then the precipitate was collected and placed in an oven to obtain a Prussian blue analog-porous carbon composite material.
[0063] After testing, the Prussian blue analog-porous carbon composite material obtained in this comparative example has a current density of 0.5A g-1 When the specific capacitance is 118.10F g -1 , the CDI unit assembled with the aminated porous carbon material has a lithium recovery rate (0.82 mg / g / min) and lithium adsorption capacitance (20.12 mg / g) in a lithium solution with a lithium ion concentration of 500 mg / L.
[0064] Comparative Example 3: The Prussian blue analog-porous carbon composite material provided in this comparative example is composited with a three-dimensional porous carbon material derived from biomass and CoHCF in a mass ratio of 1:0.4, and the preparation method specifically includes the following steps:
[0065] A2. Wash and dry the corn stalks, soak them in a saturated potassium bicarbonate solution for 18 hours, take them out and dry them, and place them in a tubular furnace for high-temperature calcination in a nitrogen atmosphere at a heating rate of 10°C / minute. When the calcination temperature reaches 800°C, keep it warm for 3 hours, then cool the calcined product to room temperature, wash it three times with a hydrochloric acid solution (the hydrochloric acid solution is a mixture of equal volumes of concentrated hydrochloric acid with a mass fraction of 37% and deionized water), filter it, wash it with deionized water until it is neutral, and then dry it at 60°C to obtain a tertiary porous carbon material derived from biomass.
[0066] B2. The tertiary porous carbon material derived from biomass was mixed with the Prussian blue analog precursor reaction solution, 0.1 g of the tertiary porous carbon material derived from biomass was dissolved in 100 mL of deionized water, stirred for 15 min, marked as solution A, and then 0.01 mol Co(NO 3 ) 2 Dissolve in solution A and stir again for 15 min to obtain a mixed solution; add 0.005 mol K 4 [Fe(CN) 6 ] was dissolved in 100 mL of deionized water and marked as solution B, and stirred for 15 min. Solution B was added dropwise to the mixed solution using a burette, and stirred continuously for 15 min during the process, and then aged at room temperature for 24 h, centrifuged, and washed with deionized water and ethanol, and then the precipitate was collected and placed in an oven to obtain a Prussian blue analog-porous carbon composite material.
[0067] After testing, the Prussian blue analog-porous carbon composite material obtained in this comparative example has a current density of 0.5A g -1 When the specific capacitance is 123.22F g -1 , the CDI unit assembled with the aminated porous carbon material has a lithium recovery rate (0.84 mg / g / min) and lithium adsorption capacitance (20.33 mg / g) in a lithium solution with a lithium ion concentration of 500 mg / L.
[0068] Comparative Example 4: The Prussian blue analog-porous carbon composite material provided in this comparative example is composited with a three-dimensional porous carbon material derived from biomass and ZnHCF in a mass ratio of 1:0.4, and the preparation method specifically includes the following steps:
[0069] A3. Wash and dry the corn stalks, soak them in a saturated potassium bicarbonate solution for 18 hours, take them out and dry them, and place them in a tubular furnace for high-temperature calcination in a nitrogen atmosphere at a heating rate of 10°C / minute. When the calcination temperature reaches 800°C, keep it warm for 3 hours, then cool the calcined product to room temperature, wash it three times with a hydrochloric acid solution (the hydrochloric acid solution is a mixture of equal volumes of concentrated hydrochloric acid with a mass fraction of 37% and deionized water), filter it, wash it with deionized water until it is neutral, and then dry it at 60°C to obtain a tertiary porous carbon material derived from biomass.
[0070] B3. The tertiary porous carbon material derived from biomass was mixed with the Prussian blue analog precursor reaction solution, 0.1 g of the tertiary porous carbon material derived from biomass was dissolved in 100 mL of deionized water, stirred for 15 min, marked as solution A, and then 0.01 mol Zn(NO 3 ) 2 Dissolve in solution A and stir again for 15 min to obtain a mixed solution; add 0.005 mol K 4 [Fe(CN) 6 ] was dissolved in 100 mL of deionized water and marked as solution B, and stirred for 15 min. Solution B was added dropwise to the mixed solution using a burette, and stirred continuously for 15 min during the process, and then aged at room temperature for 24 h, centrifuged, and washed with deionized water and ethanol, and then the precipitate was collected and placed in an oven to obtain a Prussian blue analog-porous carbon composite material.
[0071] After testing, the Prussian blue analog-porous carbon composite material obtained in this comparative example has a current density of 0.5A g -1 When the specific capacitance is 103.77F g -1 , the CDI unit assembled with the aminated porous carbon material has a lithium recovery rate (0.76 mg / g / min) and lithium adsorption capacitance (18.87 mg / g) in a lithium solution with a lithium ion concentration of 500 mg / L.
[0072] Comparative Example 5: The Prussian blue-porous carbon composite material provided in this comparative example is composited with a three-dimensional porous carbon material derived from biomass and FeHCF in a mass ratio of 1:0.4, and the preparation method specifically includes the following steps:
[0073] A3. Wash and dry the corn stalks, soak them in a saturated potassium bicarbonate solution for 18 hours, take them out and dry them, and place them in a tubular furnace for high-temperature calcination in a nitrogen atmosphere at a heating rate of 10°C / minute. When the calcination temperature reaches 800°C, keep it warm for 3 hours, then cool the calcined product to room temperature, wash it three times with a hydrochloric acid solution (the hydrochloric acid solution is a mixture of equal volumes of concentrated hydrochloric acid with a mass fraction of 37% and deionized water), filter it, wash it with deionized water until it is neutral, and then dry it at 60°C to obtain a tertiary porous carbon material derived from biomass.
[0074] B3. The tertiary porous carbon material derived from biomass was mixed with the Prussian blue analog precursor reaction solution, 0.1 g of the tertiary porous carbon material derived from biomass was dissolved in 100 mL of deionized water, stirred for 15 min, marked as solution A, and then 0.01 mol Fe(NO 3 ) 2 Dissolve in solution A and stir again for 15 min to obtain a mixed solution; add 0.005 mol K 4 [Fe(CN) 6 ] was dissolved in 100 mL of deionized water and marked as solution B, and stirred for 15 min. Solution B was added dropwise to the mixed solution using a burette, and stirred continuously for 15 min during the process, and then aged at room temperature for 24 h, centrifuged, and washed with deionized water and ethanol, and then the precipitate was collected and placed in an oven to obtain a Prussian blue analog-porous carbon composite material.
[0075] After testing, the Prussian blue analog-porous carbon composite material obtained in this comparative example has a current density of 0.5A g -1 When the specific capacitance is 128.31F g -1 , the CDI unit assembled with the aminated porous carbon material has a lithium recovery rate (0.86 mg / g / min) and lithium adsorption capacitance (25.14 mg / g) in a lithium solution with a lithium ion concentration of 500 mg / L.
[0076] The materials and performance test results obtained in Examples 1 to 4 and Comparative Examples 1 to 5 are summarized in Table 1.
[0077] Table 1 Materials and performance test table of Example 1-Example 4 and Comparative Example 1-Comparative Example 5
[0078]
[0079] It can be seen from the analysis of Examples 1 to 4 in Table 1 that when the mass ratio between the tertiary porous carbon and CuHCF in Example 1 is 1:0.4, the specific capacitance is as high as 206.87 F g -1The CuHCF and tertiary porous carbon are composited in an appropriate proportion and evenly distributed, which is beneficial to the exposure of adsorption sites and the transmission of adsorption solution within the material. The lithium recovery rate and lithium adsorption capacitance are also significantly higher than those of other embodiments.
[0080] When only pure CuHCF was used in Comparative Example 1, the specific capacitance was low and the lithium ion recovery effect was poor. At the same time, the Prussian blue analogs in Comparative Examples 2 to 5 used NiHCF, CoHCF, ZnHCF and FeHCF, and the measured specific capacitance and lithium ion adsorption effect were significantly lower than those of CuHCF in Examples 1 to 4.
[0081] The present invention utilizes the pore structure of the electrode material and the intercalation reaction to achieve ion selective adsorption. CuHCF and the three-level porous carbon composite material can achieve the adsorption of lithium ions at specific sites due to the presence of suitable open lithium ion embedding and de-embedding channels.
Claims
1. A Prussian blue analog-porous carbon composite material, characterized in that: It is composed of a porous carbon material and a Prussian blue analogue in a mass ratio of 1:0.4; the Prussian blue analogue is CuHCF; The preparation method of the Prussian blue analog-porous carbon composite material comprises the following steps: (1) first dispersing the porous carbon material in a solvent, then adding a transition metal salt to continue dissolving to obtain a mixed solution; (2) dropping a solution containing potassium ferrocyanide or potassium ferrocyanide into the mixed solution, stirring the solution thoroughly and then performing an aging reaction. After the reaction is completed, collecting the precipitate by centrifugation, washing and drying the precipitate to obtain a Prussian blue analog-porous carbon composite material.
2. The Prussian blue analog-porous carbon composite material according to claim 1, characterized in that: The porous carbon material is a tertiary porous carbon material derived from biomass.
3. The Prussian blue analog-porous carbon composite material according to claim 1, characterized in that: The usage ratio of the porous carbon material to potassium ferrocyanide or potassium ferrocyanide is 1g:0.005-0.015 mol.
4. The Prussian blue analog-porous carbon composite material according to claim 1, characterized in that: The aging reaction conditions are: reacting at room temperature for 12-24 hours.
5. The Prussian blue analog-porous carbon composite material according to claim 1, characterized in that: The preparation method of the porous carbon material is as follows: a biomass material with a fixed framework structure is activated by a pore-forming agent, calcined, cleaned and dried to obtain a porous carbon material; the parameters of the pore-forming agent activation are: soaking in a pore-forming agent solution for 12-24 hours; the parameters of the calcination are: heating to 700-900°C at a rate of 5-10°C / min and keeping warm for 2-4 hours under an inert atmosphere.
6. Use of the Prussian blue analog-porous carbon composite material according to claim 1 as a capacitive deionization electrode material in selective lithium recovery.
7. The use according to claim 6, characterized in that: The application method is: using a Prussian blue analog-porous carbon composite material as the negative electrode material of the CDI unit, using an aminated porous carbon material electrode as the positive electrode material of the CDI unit, and recovering lithium from waste lithium battery leaching liquid in a CDI device configured by a CDI unit, a conductivity meter, a peristaltic pump, a water storage tank, and a DC power supply.
8. The use according to claim 7, characterized in that: The concentration of lithium ions in the waste lithium battery leachate is 200-1000 ppm, and the parameters of lithium recovery are: the adsorption applied voltage is 1.2-1.8 V, and the desorption method is short circuit or applying a reverse voltage of 1.2-1.8 V.
Citation Information
Patent Citations
Negative electrode material of lithium ion battery and preparation method of negative electrode material
CN106252621A
Carbon-based Prussian blue analogue composite material, preparation method and applications thereof
CN110540216A
Novel porous carbon electrode material for capacitive deionization and application of novel porous carbon electrode material