A high-thermal-conductivity, wear-resistant, high-performance polytetrafluoroethylene plastic and a preparation method thereof
Through the combination of modified graphene oxide and polytetrafluoroethylene, electrophoretic deposition method and ion beam treatment, the problems of poor thermal conductivity and insufficient wear resistance of polytetrafluoroethylene plastics are solved, and the effects of high thermal conductivity, wear resistance and hydrophobicity are achieved. , improving its application performance.
Patent Information
- Application Number
- CN202311762153.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-12-20
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2043-12-20
AI Technical Summary
In high-demand applications, polytetrafluoroethylene plastics have problems such as poor thermal conductivity, insufficient wear resistance and viscoelastic deformation, and graphene oxide is difficult to take into account both thermal conductivity, hydrophobicity and wear resistance when used as fillers.
Modified graphene oxide is used as filler, mixed with polytetrafluoroethylene and cold pressing, and outer plating composite film is made. The composite film is obtained by fumigation alkali treatment of boron nitride, carboxylated graphene and silane coupling agent, combined with supercritical carbon dioxide Modified graphene oxide was formed, and a magnesium oxide film and dodecyl trimethoxysilane were added to the electrophoretic deposition method to improve hydrophobicity and density by ion beam bombardment.
It achieves high thermal conductivity, wear resistance and hydrophobic effects, improves the overall performance of PTFE plastics, and enhances its applicability in high-demand applications.
Smart Images

Figure BDA0004618883370000081
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of plastics, in particular to a high-heat-conductivity, wear-resistant and high-performance polytetrafluoroethylene plastic and a preparation method thereof. Background Art
[0002] As the main body of plastic, polytetrafluoroethylene has some excellent properties, such as chemical inertness and high temperature resistance. However, polytetrafluoroethylene also has some shortcomings, such as low strength, low hardness, high wear rate, large viscoelastic deformation under external force and poor thermal conductivity, which limit the application of polytetrafluoroethylene plastic in practice. In order to make it applicable in occasions with higher requirements, polytetrafluoroethylene must be appropriately modified. Adding fillers is a simple and effective method. Adding different fillers to polytetrafluoroethylene plastic can significantly change its physical and mechanical properties.
[0003] Graphene oxide has excellent thermal conductivity, but it cannot take into account both hydrophobicity and wear resistance; the active groups rich in graphene oxide itself have a hydrophilic effect, and its layered structure makes it easy to wear. At the same time, when added to plastics as a filler, it is easy to agglomerate due to van der Waals forces, affecting the performance effect. Therefore, the present invention innovates a high-thermal-conductivity, wear-resistant, and high-performance polytetrafluoroethylene plastic, using graphene oxide as a filler to solve some of the above problems. Summary of the invention
[0004] The purpose of the present invention is to provide a high-thermal-conductivity, wear-resistant and high-performance polytetrafluoroethylene plastic and a preparation method thereof, so as to solve the problems existing in the prior art.
[0005] In order to solve the above technical problems, the present invention provides the following technical solutions: a high thermal conductivity, wear-resistant and high-performance polytetrafluoroethylene plastic, wherein the high thermal conductivity, wear-resistant and high-performance polytetrafluoroethylene plastic is made by mixing modified graphene oxide as a filler with polytetrafluoroethylene and cold pressing, and then coating a composite film on the outside.
[0006] Furthermore, the modified graphene oxide is prepared by mixing the modified boron nitride after alkali fumigation with carboxylated graphene, and grinding is assisted by a silane coupling agent and a supercritical carbon dioxide fluid.
[0007] Furthermore, a method for preparing high-thermal-conductivity, wear-resistant and high-performance polytetrafluoroethylene plastic comprises the following preparation steps:
[0008] (1) adding 2-4 parts of boron nitride to 20 parts of deionized water, stirring at 200-300 r / min for 20 minutes, ultrasonically treating at 80°C, 150W, and 40kHz, while spraying with gaseous sodium hydroxide solution for 40-60 minutes, washing with deionized water for 3 times, and drying at a vacuum degree of 20 Pa and 60°C for 5 hours to obtain modified boron nitride;
[0009] (2) 10-12 parts of graphene oxide and 20 parts of deionized water were ultrasonically dispersed at 100 W and 30 kHz for 1 hour, 0.2-0.4 parts of methyl bromoacetate were added, and ultrasonically dispersed for 15 minutes under the same conditions, and the reaction was continued for 5 hours. The filtrate was filtered and washed with deionized water for 3 times, and dried at a vacuum degree of 20 Pa and 50° C. for 2-3 hours to obtain carboxylated graphene;
[0010] (3) Dispersing 0.1-0.6 parts of carboxylated graphene and 0.1-0.3 parts of modified boron nitride in 20 parts of solvent, ultrasonicating at 1000-1800W for 0.5-3h, centrifuging at 3000-5000rpm for 0.5-1h, and taking solid precipitate to obtain a composite material; placing 10 parts of the composite material in a ball mill, adding 0.2-0.6 parts of 3-triethoxysilyl-1-propylamine three times, adding one third of the total amount each time, and adding once every 6h. Zirconium oxide is used as a grinding ball medium, and after ball milling at 500r / min for 18h, it is dried at 25℃ for 12h to obtain a ball-milled product; 5 parts of the ball-milled product and 1-2 parts of methanol solution are stirred at 400-600r / min for 20min, placed in a 35℃ oil bath, filled with carbon dioxide, and heated and pressurized to 120℃ and 6.5MPa. After reacting for 2h, it is cooled to room temperature, and the precipitate is taken, washed with methanol for 5 times, and dried at 60℃ and a vacuum degree of 20Pa for 6h to obtain modified graphene oxide;
[0011] (4) 12-16 parts of polytetrafluoroethylene and 1-2 parts of modified graphene oxide were stirred at 1000-2000 r / min for 30 min, cold pressed, and then placed in a mold at 360-380° C., pressurized to 150-170 MPa, sintered for 2 h, cooled to 80-100° C., taken out, and naturally cooled to 25° C. to form a plastic cube of 1 cm×1 cm×1 cm;
[0012] (5) 0.1-0.3 parts of magnesium oxide, 6 parts of ethanol, 0.4-0.8 parts of cerium nitrate, and 0.1-0.3 parts of dodecyltrimethoxysilane are taken, and after ultrasonic treatment for 30 minutes, an electrophoretic suspension is obtained; a plastic block is immersed in the electrophoretic suspension, and an Au sheet is used as an anode and a Si substrate is used as a cathode. Electrophoretic deposition is performed for 3 minutes at a voltage of 200 V and a distance between the anode and the cathode of 2 cm, and the block is dried at 60° C. for 3 hours. While drying, the membrane surface is bombarded with argon ions to obtain a high-thermal-conductivity, wear-resistant, and high-performance polytetrafluoroethylene plastic.
[0013] Furthermore, in the step (1), the flow rate of sodium hydroxide sprayed is 2-6 mL / min, and the mass fraction of the sodium hydroxide solution is 10%.
[0014] Furthermore, the solvent in step (3) is a mixture of one or more of isopropanol, N-methylpyrrolidone or N,N-dimethylformamide.
[0015] Furthermore, the material-to-ball ratio of ball milling in step (3) is 1:10.
[0016] Furthermore, the methanol solution in step (3) is a mixed solution of methanol and deionized water in a mass ratio of 4:1.
[0017] Furthermore, the ultrasonic conditions in step (5) are 500W and 30kHz.
[0018] Furthermore, in step (5), the ion beam energy is 1 keV.
[0019] Furthermore, in the step (5), the incident angle of the ion beam is 45° to the normal of the substrate plane.
[0020] Compared with the prior art, the beneficial effects achieved by the present invention are:
[0021] The invention uses boron nitride modified graphene oxide as filler, melt-extrudes the plastic with polytetrafluoroethylene, and then electroplates a magnesium oxide film to achieve the effects of high thermal conductivity, wear resistance and hydrophobicity.
[0022] Firstly, the invention performs alkali fumigation treatment on boron nitride, and simultaneously performs ultrasonic microwave and gas phase alkaline solution to infiltrate and modify boron nitride under the action of ultrasound, so that the surface of boron nitride is rich in hydroxyl groups; then, methyl bromoacetate is used to modify graphene oxide to prepare carboxylated graphene, which is then mixed and ground with the modified boron nitride; during the grinding process, a silane coupling agent is continuously added to reduce friction and improve the wear resistance effect; and then a second grinding is performed, and supercritical carbon dioxide is used to assist, so that the boron nitride and the graphene oxide are more firmly and evenly combined, and the phenomenon that the graphene oxide is easy to agglomerate is improved, so that the plastic performance is better.
[0023] Secondly, the modified graphene oxide is mixed with polytetrafluoroethylene and cold-pressed into plastic. A magnesium oxide film is produced on the plastic surface by electrophoretic deposition. Dodecyltrimethoxysilane and electrolyte cerium nitrate are added to the electrolyte solution to react together to form cerium dioxide, which seals the microcracks in the coating to achieve a wear-resistant effect. The silane makes the surface of the composite coating have many short rod-like protrusions, thereby achieving a hydrophobic effect. The surface of the modified film is then bombarded with an ion beam to increase the density of the film, further improving the hydrophobicity and wear resistance of the film. DETAILED DESCRIPTION
[0024] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.
[0025] In order to more clearly illustrate the method provided by the present invention, the following examples are used to describe in detail the various index testing methods of the high thermal conductivity, wear resistance and high performance polytetrafluoroethylene plastics prepared in the following examples are as follows:
[0026] Wear resistance: A GCrl5 bearing steel ball with a diameter of d=10mm was used to slide on the sample, with a sliding reciprocating stroke of s=6mm, a time of 20min, a reciprocating frequency of 10Hz, and a load of F=10N. All friction and wear experiments were carried out at 20°C and repeated 3 times, and the average value was taken as the wear rate of the material.
[0027] Hydrophobicity: The material is tested based on the sessile drop method and the contact angle of the drop is measured using a surface contact angle meter.
[0028] Thermal conductivity: Take the coating material of the same thickness and test the thermal conductivity of the coating according to the standard ASTM D5470
[0029] Example 1
[0030] (1) Add 2 parts of boron nitride to 20 parts of deionized water, stir at 200 r / min for 20 min, and ultrasonically treat under the conditions of 80°C, 150 W, and 40 kHz. At the same time, spray a gaseous sodium hydroxide solution at a flow rate of 2 mL / min, and the mass fraction of the sodium hydroxide solution is 10%. After 40 min, wash with deionized water for 3 times, and dry at a vacuum degree of 20 Pa and 60°C for 5 h to obtain modified boron nitride;
[0031] (2) 10 parts of graphene oxide and 20 parts of deionized water were ultrasonically dispersed at 100 W and 30 kHz for 1 hour, 0.2 parts of ethyl methyl bromide were added, and ultrasonically dispersed for 15 minutes under the same conditions, and the reaction was continued for 5 hours. The filtrate was filtered and washed with deionized water for 3 times, and dried at a vacuum degree of 20 Pa and 50° C. for 2 hours to obtain carboxylated graphene;
[0032] (3) 0.1 parts of carboxylated graphene and 0.1 parts of modified boron nitride were dispersed in 20 parts of isopropanol, and after ultrasonication at 1000 W for 0.5 h, the mixture was centrifuged at 3000 rpm for 0.5 h, and the solid precipitate was obtained to obtain the composite material; 10 parts of the composite material were put into a ball mill, and 0.2 parts of 3-triethoxysilyl-1-propylamine were added three times, with one third of the total amount added each time, and the addition was made every 6 hours, with zirconium oxide as the ball medium, 500 r / min, and a material-ball ratio of 1:1 After ball milling at 0 for 18 hours, it was dried at 25°C for 12 hours to obtain a ball-milled product; 5 parts of the ball-milled product and 1 part of a methanol solution, in which the mass ratio of methanol to deionized water is 4:1, were taken, stirred at 400r / min for 20 minutes, placed in a 35°C oil bath, filled with carbon dioxide, and heated and pressurized to 120°C and 6.5MPa. After reacting for 2 hours, it was cooled to room temperature, the precipitate was taken, washed with methanol 5 times, and dried at 60°C and a vacuum degree of 20Pa for 6 hours to obtain modified graphene oxide;
[0033] (4) 12 parts of polytetrafluoroethylene and 1 part of modified graphene oxide were stirred at 1000 r / min for 30 min, cold pressed at 0°C, then placed in a mold at 360°C, pressurized to 150 MPa, sintered for 2 h, cooled to 80°C, taken out, and naturally cooled to 25°C to form a plastic cube of 1 cm×1 cm×1 cm;
[0034] (5) 0.1 parts of magnesium oxide, 6 parts of ethanol, 0.4 parts of cerium nitrate, and 0.1 parts of dodecyltrimethoxysilane were taken, and after being ultrasonicated at 500 W and 30 kHz for 30 minutes, an electrophoretic suspension was obtained; a plastic block was immersed in the electrophoretic suspension, and an Au sheet was used as an anode and a Si substrate was used as a cathode. Electrophoretic deposition was performed for 3 minutes at a voltage of 200 V and a distance between the anode and cathode of 2 cm, and the block was dried at 60° C. for 3 hours. While drying, the membrane surface was bombarded with argon ions. The incident angle of the ion beam was 45° to the normal of the substrate plane, and the ion beam energy was 1 keV, thereby obtaining a high-thermal-conductivity, wear-resistant, and high-performance polytetrafluoroethylene plastic.
[0035] Example 2
[0036] (1) Add 3 parts of boron nitride to 20 parts of deionized water, stir at 250 r / min for 20 min, and ultrasonically treat at 80°C, 150 W, and 40 kHz. At the same time, spray gaseous sodium hydroxide solution at a flow rate of 4 mL / min and a mass fraction of 10% for 50 min. Then, wash with deionized water for 3 times, and dry at a vacuum degree of 20 Pa and 60°C for 5 h to obtain modified boron nitride;
[0037] (2) 11 parts of graphene oxide and 20 parts of deionized water were ultrasonically dispersed at 100 W and 30 kHz for 1 hour, 0.3 parts of methyl bromoacetate were added, and ultrasonically dispersed for 15 minutes under the same conditions, and the reaction was continued for 5 hours. The filtrate was filtered and washed with deionized water for 3 times, and dried at a vacuum degree of 20 Pa and 50° C. for 2.5 hours to obtain carboxylated graphene;
[0038] (3) 0.3 parts of carboxylated graphene and 0.2 parts of modified boron nitride were dispersed in 20 parts of N-methylpyrrolidone solvent, and ultrasonicated at 1400 W for 1.75 h, and then centrifuged at 4000 rpm for 0.75 h, and solid precipitate was obtained to obtain a composite material; 10 parts of the composite material were put into a ball mill, and 0.4 parts of 3-triethoxysilyl-1-propylamine were added three times, each time adding one third of the total amount, and added once every 6 hours, with zirconium oxide as the ball medium, 500 r / min, and a material-to-ball ratio of 1:10 for 18 hours, and then dried at 25°C for 12 hours to obtain a ball-milled product; take 5 parts of the ball-milled product and 1.5 parts of a methanol solution, in which the mass ratio of methanol to deionized water is 4:1, stir at 500r / min for 20 minutes, place in a 35°C oil bath, fill with carbon dioxide, increase the temperature and pressure to 120°C and 6.5MPa, react for 2 hours, cool to room temperature, take the precipitate, wash it with methanol 5 times, and dry it at 60°C and a vacuum degree of 20Pa for 6 hours to obtain modified graphene oxide;
[0039] (4) 14 parts of polytetrafluoroethylene and 1.5 parts of modified graphene oxide were stirred at 1500 r / min for 30 min, cold-pressed at 2.5°C, then placed in a mold at 370°C, pressurized to 160 MPa, sintered for 2 h, cooled to 90°C, taken out, and naturally cooled to 25°C to form a plastic cube of 1 cm×1 cm×1 cm;
[0040] (5) 0.2 parts of magnesium oxide, 6 parts of ethanol, 0.6 parts of cerium nitrate, and 0.2 parts of dodecyltrimethoxysilane were taken, and after being ultrasonicated at 500 W and 30 kHz for 30 minutes, an electrophoretic suspension was obtained; a plastic block was immersed in the electrophoretic suspension, and an Au sheet was used as an anode and a Si substrate was used as a cathode. Electrophoretic deposition was performed for 3 minutes at a voltage of 200 V and a distance between the anode and cathode of 2 cm, and the block was dried at 60° C. for 3 hours. While drying, the membrane surface was bombarded with argon ions. The incident angle of the ion beam was 45° with respect to the normal line of the substrate plane, and the ion beam energy was 1 keV, thereby obtaining a high-thermal-conductivity, wear-resistant, and high-performance polytetrafluoroethylene plastic.
[0041] Example 3
[0042] (1) Add 4 parts of boron nitride to 20 parts of deionized water, stir at 300 r / min for 20 minutes, and ultrasonically treat under the conditions of 80°C, 150W, and 40kHz. At the same time, spray a gaseous sodium hydroxide solution at a flow rate of 6 mL / min, and the mass fraction of the sodium hydroxide solution is 10%. After 60 minutes, wash with deionized water for 3 times, and dry at a vacuum degree of 20 Pa and 60°C for 5 hours to obtain modified boron nitride;
[0043] (2) 12 parts of graphene oxide and 20 parts of deionized water were ultrasonically dispersed at 100 W and 30 kHz for 1 hour, 0.4 parts of methyl bromoacetate were added, and ultrasonically dispersed for 15 minutes under the same conditions, and the reaction was continued for 5 hours. The filtrate was filtered and washed with deionized water for 3 times, and dried at a vacuum degree of 20 Pa and 50° C. for 3 hours to obtain carboxylated graphene;
[0044] (3) 0.6 parts of carboxylated graphene and 0.3 parts of modified boron nitride were dispersed in 20 parts of N,N-dimethylformamide solvent, and ultrasonicated at 1800 W for 3 h, and then centrifuged at 5000 rpm for 1 h to obtain a solid precipitate, which is a composite material; 10 parts of the composite material were put into a ball mill, and 0.6 parts of 3-triethoxysilyl-1-propylamine were added three times, each time adding one third of the total amount, and added once every 6 hours, with zirconium oxide as the ball medium, 500 r / min, and a material-ball ratio of 1 :10 for 18 hours, and then dried at 25°C for 12 hours to obtain a ball-milled product; take 5 parts of the ball-milled product and 2 parts of a methanol solution, in which the mass ratio of methanol to deionized water is 4:1, stir at 600r / min for 20 minutes, place in a 35°C oil bath, fill with carbon dioxide, increase the temperature and pressure to 120°C and 6.5MPa, react for 2 hours, cool to room temperature, take the precipitate, wash it with methanol 5 times, and dry it at 60°C and a vacuum degree of 20Pa for 6 hours to obtain modified graphene oxide;
[0045] (4) 16 parts of polytetrafluoroethylene and 2 parts of modified graphene oxide were stirred at 2000 r / min for 30 min, cold pressed at 5°C, then placed in a mold at 380°C, pressurized to 170 MPa, sintered for 2 h, cooled to 100°C, taken out, and naturally cooled to 25°C to form a plastic cube of 1 cm×1 cm×1 cm;
[0046] (5) 0.3 parts of magnesium oxide, 6 parts of ethanol, 0.8 parts of cerium nitrate, and 0.3 parts of dodecyltrimethoxysilane were taken, and after being ultrasonicated at 500 W and 30 kHz for 30 minutes, an electrophoretic suspension was obtained; a plastic block was immersed in the electrophoretic suspension, and an Au sheet was used as an anode and a Si substrate was used as a cathode. Electrophoretic deposition was performed for 3 minutes at a voltage of 200 V and a distance between the anode and cathode of 2 cm, and the block was dried at 60° C. for 3 hours. While drying, the membrane surface was bombarded with argon ions. The incident angle of the ion beam was 45° to the normal of the substrate plane, and the ion beam energy was 1 keV, thereby obtaining a high-thermal-conductivity, wear-resistant, and high-performance polytetrafluoroethylene plastic.
[0047] Comparative Example 1
[0048] The difference between Comparative Example 1 and Example 2 is that there is no step (1), and step (3) is changed to: 0.3 parts of carboxylated graphene and 0.2 parts of boron nitride are dispersed in 20 parts of N-methylpyrrolidone, ultrasonicated at 1400W for 1.75h, centrifuged at 4000rpm for 0.75h, and solid precipitate is taken to obtain a composite material; 10 parts of the composite material are put into a ball mill, and 0.4 parts of 3-triethoxysilyl-1-propylamine are added three times, each time adding one third of the total amount, and once every 6h, using zirconium oxide as the grinding ball medium, 500r / m in, material-ball ratio of 1:10, after ball milling for 18 hours, dried at 25°C for 12 hours to obtain a ball-milled product; take 5 parts of the ball-milled product and 1.5 parts of a methanol solution, the mass ratio of methanol to deionized water in the methanol solution is 4:1, stir at 500r / min for 20 minutes, place in a 35°C oil bath, fill with carbon dioxide, increase the temperature and pressure to 120°C and 6.5MPa, react for 2 hours, cool to room temperature, take a precipitate, wash it with methanol 5 times, and dry it at 60°C and a vacuum degree of 20Pa for 6 hours to obtain modified graphene oxide; the remaining steps are the same as those in Example 2.
[0049] Comparative Example 2
[0050] The difference between Comparative Example 2 and Example 2 is that there is no step (2), and step (3) is changed to: 0.3 parts of graphene oxide and 0.2 parts of modified boron nitride are dispersed in 20 parts of N-methylpyrrolidone solvent, ultrasonicated at 1400W for 1.75h, centrifuged at 4000rpm for 0.75h, and solid precipitate is taken to obtain a composite material; 10 parts of the composite material are put into a ball mill, and 0.4 parts of 3-triethoxysilyl-1-propylamine are added three times, each time adding one third of the total amount, and once every 6h, using zirconium oxide as the ball medium, 500r / min, and a material-ball ratio of 1:10, after ball milling for 18 hours, drying at 25°C for 12 hours to obtain a ball-milled product; taking 5 parts of the ball-milled product and 1.5 parts of a methanol solution, wherein the mass ratio of methanol to deionized water in the methanol solution is 4:1, stirring at 500r / min for 20 minutes, placing in a 35°C oil bath, charging with carbon dioxide, raising the temperature and pressure to 120°C and 6.5MPa, reacting for 2 hours, cooling to room temperature, taking a precipitate, washing it with methanol 5 times, and drying it at 60°C and a vacuum degree of 20Pa for 6 hours to obtain modified graphene oxide; the remaining steps are the same as those in Example 2.
[0051] Comparative Example 3
[0052] The difference between Comparative Example 3 and Example 2 is that step (3) is different. Step (3) is changed to: 0.3 parts of carboxylated graphene and 0.2 parts of modified boron nitride are dispersed in 20 parts of N-methylpyrrolidone solvent, ultrasonicated at 1400W for 1.75h, centrifuged at 4000rpm for 0.75h, and solid precipitate is taken to obtain a composite material; 10 parts of the composite material are put into a ball mill, with zirconium oxide as the grinding ball medium, and ball milled at 500r / min and a material-ball ratio of 1:10 for 18h, 25 ℃ and dried for 12 hours to obtain a ball-milled product; take 5 parts of the ball-milled product and 1.5 parts of a methanol solution, in which the mass ratio of methanol to deionized water is 4:1, stir at 500 r / min for 20 minutes, place in a 35℃ oil bath, fill with carbon dioxide, increase the temperature and pressure to 120℃ and 6.5MPa, react for 2 hours, cool to room temperature, take a precipitate, wash it with methanol 5 times, and dry it at 60℃ and a vacuum degree of 20Pa for 6 hours to obtain modified graphene oxide; the remaining steps are the same as those in Example 2.
[0053] Comparative Example 4
[0054] The difference between Comparative Example 4 and Example 2 is that step (3) is different. Step (3) is changed to: 0.3 parts of carboxylated graphene and 0.2 parts of modified boron nitride are dispersed in 20 parts of N-methylpyrrolidone solvent, ultrasonicated at 1400W for 1.75h, centrifuged at 4000rpm for 0.75h, and solid precipitate is taken to obtain a composite material; 10 parts of the composite material are put into a ball mill, 0.4 parts of 3-triethoxysilyl are added three times, one third of the total amount is added each time, and added once every 6h, zirconium oxide is used as the grinding ball medium, ball milled at 500r / min, with a material-ball ratio of 1:10 for 18h, and dried at 25°C for 12h, to obtain modified graphene oxide; the remaining steps are the same as those in Example 2.
[0055] Comparative Example 5
[0056] The difference between Comparative Example 5 and Example 2 is that step (5) is different. Step (5) is changed to: take 0.2 parts of magnesium oxide, 6 parts of ethanol, and 0.2 parts of dodecyltrimethoxysilane, and after 500W, 30kHz ultrasound for 30 minutes, obtain an electrophoretic suspension; immerse the plastic block in the electrophoretic suspension, use Au sheet as anode and Si substrate as cathode, electrophoretically deposit for 3 minutes at a voltage of 200V and a cathode-cathode distance of 2cm, and dry at 60°C for 3 hours. While drying, bombard the film surface with argon ions, the incident angle of the ion beam and the normal of the substrate plane are 45°, and the ion beam energy is 1kev, to obtain a high thermal conductivity, wear-resistant and high-performance polytetrafluoroethylene plastic; the remaining steps are the same as Example 2.
[0057] Comparative Example 6
[0058] The difference between Comparative Example 6 and Example 2 lies in the difference in step (5). Step (5) is changed to: take 0.2 parts of magnesium oxide, 6 parts of ethanol, and 0.6 parts of cerium nitrate, and obtain an electrophoretic suspension after 500W, 30kHz ultrasound for 30 minutes; immerse the plastic block in the electrophoretic suspension, use Au sheet as anode and Si substrate as cathode, electrophoretically deposit for 3 minutes at a voltage of 200V and a cathode-cathode distance of 2cm, and dry at 60°C for 3 hours. While drying, bombard the film surface with argon ions, the incident angle of the ion beam and the normal of the substrate plane are 45°, and the ion beam energy is 1kev, to obtain a high thermal conductivity, wear-resistant and high-performance polytetrafluoroethylene plastic; the remaining steps are the same as those in Example 2.
[0059] Comparative Example 7
[0060] The difference between Comparative Example 7 and Example 2 lies in step (5), where step (5) is modified as follows: 0.2 parts of magnesium oxide, 6 parts of ethanol, 0.6 parts of cerium nitrate and 0.2 parts of dodecyltrimethoxysilane are taken, and after being ultrasonicated at 500 W and 30 kHz for 30 min, an electrophoretic suspension is obtained; a plastic block is immersed in the electrophoretic suspension, and an Au sheet is used as an anode and a Si substrate is used as a cathode. Electrophoretic deposition is performed for 3 min at a voltage of 200 V and a distance between the anode and cathode of 2 cm, and the electrophoretic deposition is performed at 60° C. for 3 h to obtain a high thermal conductivity, wear-resistant and high-performance polytetrafluoroethylene plastic; the remaining steps are the same as those in Example 2.
[0061] Effect example
[0062] Table 1 below shows the performance analysis results of high thermal conductivity, wear resistance and high performance polytetrafluoroethylene plastics using Examples 1 to 3 of the present invention and Comparative Examples 1 to 7.
[0063] Table 1
[0064]
[0065] From the comparison of the experimental data of wear resistance of the embodiment and the comparative example, it can be found that the present invention first performs alkali fumigation treatment on the boron nitride, and at the same time, ultrasonic microwaves and gas-phase alkaline solutions penetrate and modify the boron nitride under the action of ultrasound, thereby making the surface of the boron nitride rich in hydroxyl groups; then, methyl bromoacetate is used to modify graphene oxide to prepare carboxylated graphene, which is then mixed and ground with the modified boron nitride, and a silane coupling agent is continuously added during the grinding process to reduce friction and improve the wear resistance; the prepared modified graphene oxide is mixed with polytetrafluoroethylene and cold-pressed into a plastic, a magnesium oxide-containing film is prepared on the surface of the plastic by an electrophoretic deposition method, and dodecyltrimethoxysilane and electrolyte cerium nitrate are added to the electrolyte solution to react together to form cerium dioxide, and the coating The micro-crack sealing of the layer achieves a wear-resistant effect; from the comparison of the experimental data of the heat dissipation of the embodiment and the comparative example, it can be found that the graphene oxide with excellent heat dissipation performance is selected and mixed with boron nitride as a filler to improve its heat dissipation, and then a second grinding is performed, and supercritical carbon dioxide is assisted to make the boron nitride and graphene oxide more firmly and evenly combined, while also improving the phenomenon that graphene oxide is easy to agglomerate, so that the plastic performance is better; from the comparison of the experimental data of the hydrophobicity of the embodiment and the comparative example, it can be found that the present invention adds silane to the electrophoretic liquid so that the surface of the composite coating has many short rod-shaped protrusions, thereby achieving a hydrophobic effect, and then uses ion beams to bombard the surface of the modified film to improve the density of the film and further improve the hydrophobicity of the film.
[0066] It will be apparent to those skilled in the art that the invention is not limited to the details of the exemplary embodiments described above and that the invention can be implemented in other specific forms without departing from the spirit or essential features of the invention. Therefore, the embodiments should be considered in all respects as exemplary and non-limiting, and the scope of the invention is defined by the appended claims rather than the foregoing description, and it is intended that all variations within the meaning and scope of the equivalent elements of the claims be included in the invention. Any marking in a claim should not be considered as limiting the claim to which it relates.
Claims
1. A high thermal conductivity, wear-resistant and high-performance polytetrafluoroethylene plastic, characterized in that: The high thermal conductivity, wear-resistant and high-performance polytetrafluoroethylene plastic is prepared by mixing modified graphene oxide as a filler with polytetrafluoroethylene and cold pressing, and then coating a composite film on the outside; the preparation method of the high thermal conductivity, wear-resistant and high-performance polytetrafluoroethylene plastic comprises the following preparation steps: (1) Add 2-4 parts of boron nitride to 20 parts of deionized water, stir at 200-300 r / min for 20 minutes, ultrasonically treat at 80°C, 150W, and 40kHz, and spray gaseous sodium hydroxide solution at the same time for 40-60 minutes, wash with deionized water for 3 times, and dry at a vacuum degree of 20Pa and 60°C for 5 hours to obtain modified boron nitride; (2) 10-12 parts of graphene oxide and 20 parts of deionized water were ultrasonically dispersed at 100 W and 30 kHz for 1 hour, 0.2-0.4 parts of methyl bromoacetate were added, and ultrasonically dispersed for 15 minutes under the same conditions. The reaction was continued for 5 hours, and the filtrate was filtered and washed with deionized water for 3 times. The filtrate was dried at a vacuum degree of 20 Pa and 50° C. for 2-3 hours to obtain carboxylated graphene; (3) Disperse 0.1-0.6 parts of carboxylated graphene and 0.1-0.3 parts of modified boron nitride in 20 parts of solvent, ultrasonicate at 1000-1800W for 0.5-3h, centrifuge at 3000-5000rpm for 0.5-1h, and take solid precipitate to obtain a composite material; put 10 parts of the composite material into a ball mill, add 0.2-0.6 parts of 3-triethoxysilyl-1-propylamine three times, add one third of the total amount each time, and add once every 6h. Zirconium oxide is used as a grinding ball medium, and after ball milling at 500r / min for 18h, it is dried at 25℃ for 12h to obtain a ball-milled product; 5 parts of the ball-milled product and 1-2 parts of methanol solution are stirred at 400-600r / min for 20min, placed in a 35℃ oil bath, filled with carbon dioxide, and heated and pressurized to 120℃ and 6.5MPa. After reacting for 2h, it is cooled to room temperature, and the precipitate is taken, washed with methanol for 5 times, and dried at 60℃ and a vacuum degree of 20Pa for 6h to obtain modified graphene oxide; (4) 12-16 parts of polytetrafluoroethylene and 1-2 parts of modified graphene oxide were stirred at 1000-2000 r / min for 30 min, cold pressed, and then placed in a mold at 360-380°C, pressurized to 150-170 MPa, sintered for 2 h, cooled to 80-100°C, taken out, and naturally cooled to 25°C to form a plastic cube of 1 cm×1 cm×1 cm; (5) Take 0.1-0.3 parts of magnesium oxide, 6 parts of ethanol, 0.4-0.8 parts of cerium nitrate, and 0.1-0.3 parts of dodecyltrimethoxysilane, and after ultrasonic treatment for 30 minutes, obtain an electrophoretic suspension; immerse the plastic cube in the electrophoretic suspension, use the Au sheet as the anode and the Si substrate as the cathode, and perform electrophoretic deposition for 3 minutes at a voltage of 200V and a distance between the anode and the cathode of 2cm, and dry at 60°C for 3 hours. While drying, bombard the film surface with argon ions, and the incident angle of the ion beam is 45° to the normal of the substrate plane, so as to obtain high-thermal-conductivity, wear-resistant, and high-performance polytetrafluoroethylene plastic.
2. The method for preparing a high-thermal-conductivity, wear-resistant and high-performance polytetrafluoroethylene plastic according to claim 1, characterized in that: In the step (1), the flow rate of the sodium hydroxide solution sprayed is 2-6 mL / min, and the mass fraction of the sodium hydroxide solution is 10%.
3. The method for preparing a high thermal conductivity, wear-resistant and high-performance polytetrafluoroethylene plastic according to claim 1, characterized in that: The solvent in step (3) is a mixture of one or more of isopropanol, N-methylpyrrolidone or N,N-dimethylformamide.
4. The method for preparing a high thermal conductivity, wear-resistant and high-performance polytetrafluoroethylene plastic according to claim 1, characterized in that: The material-to-ball ratio in the ball milling in step (3) is 1:
10.
5. The method for preparing a high-thermal-conductivity, wear-resistant and high-performance polytetrafluoroethylene plastic according to claim 1, characterized in that: The methanol solution in step (3) is a mixed solution of methanol and deionized water in a mass ratio of 4:
1.
6. The method for preparing a high thermal conductivity, wear-resistant and high-performance polytetrafluoroethylene plastic according to claim 1, characterized in that: The ultrasonic conditions in step (5) are 500W and 30kHz.