A method for preparing a fire-resistant high-strength plastic pipe
By combining heat-resistant polyolefins with nano-level strong temperature-resistant substances and antibacterial agents, high-strength plastic tubes with good heat-resistant and antibacterial properties are prepared, which solves the problems of insufficient antibacterial, strength and fire resistance of existing plastic tubes, and improves the Its stability and performance in high temperature and humid environments.
Patent Information
- Application Number
- CN202311580850.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-04-07
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2043-04-07
AI Technical Summary
The existing plastic tubes are insufficient in antibacterial, strength and fire resistance, especially in humid environments, which are prone to breeding microorganisms and causing the formation of dirt layers, affecting the performance of use.
Heat-resistant polyolefins are mixed with nano-level strong temperature-resistant substances, combined with antibacterial agents to prepare refractory high-strength plastic tubes, and the chalone structure and benzotriazole cyclic compounds are formed through specific chemical reactions to improve heat resistance and antibacterial properties.
It significantly improves the heat resistance and antibacterial effect of plastic tubes, and enhances its stability and performance in high temperature and humid environments.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of plastic pipes, in particular to a method for preparing a fire-resistant high-strength plastic pipe. Background Art
[0002] Plastic pipes are generally made of synthetic resins through extrusion in a pipe making machine. They are mainly used for water supply system piping, drainage, exhaust and sewage pipes, underground drainage pipe systems, rainwater pipes, and threading pipes for wire installation in buildings. The main advantages of plastic pipes are good corrosion resistance, light weight, easy molding, and easy processing. The disadvantages are poor antibacterial, strength and fire resistance.
[0003] Improving the fire resistance of plastic pipes mainly involves improving the heat resistance of synthetic resins and adding substances with strong heat resistance (such as ceramic powder, etc.), high heat-resistant resins and strong heat-resistant substances that gradually melt the sealed plastic under high temperature, maintaining the firmness and most of the strength of the plastic pipe structure to inhibit the spread of fire. At the same time, the addition of nano-scale strong heat-resistant substances can greatly improve the strength of plastic pipes. In addition, plastic pipes used in humid environments for a long time are very likely to breed microorganisms, and as the microorganisms continue to breed, a dirt layer is formed, which seriously affects the performance of the plastic pipe. In view of the above situation, the present invention uses heat-resistant polyolefins and nano-scale strong heat-resistant substances to mix to prepare fire-resistant and high-strength plastic pipes, and at the same time gives them antibacterial effects to meet market demand. Summary of the invention
[0004] The object of the present invention is to provide a fire-resistant high-strength plastic pipe and a preparation method thereof, so as to solve the problems existing in the prior art.
[0005] In order to solve the above technical problems, the present invention provides the following technical solutions:
[0006] A fire-resistant high-strength plastic pipe and a preparation method thereof. The fire-resistant high-strength plastic pipe is prepared by mixing heat-resistant polyolefin with other additives to obtain a plastic pipe, and then finishing with an antibacterial agent.
[0007] Furthermore, the heat-resistant polyolefin is prepared by reacting 2-butenyltriethoxysilane, p-isopropenylacetophenone, 2-methylacrolein, and 4,4'-dihydroxy-3,3'-glyoxalbiphenyl.
[0008] Furthermore, the other additives include anti-ultraviolet agent, nano-carbon fiber, fire retardant, and dispersant.
[0009] Furthermore, the anti-ultraviolet agent is nano titanium dioxide; the refractory agent is a mixture of antimony trioxide, zinc borate and ceramic powder; and the dispersant is dibutyl phthalate.
[0010] Furthermore, the antibacterial agent is prepared from 4-butyl-2-nitroaniline, sodium nitrite, 3-tert-butyl-4-hydroxybenzaldehyde and perfluorocarbazine.
[0011] Furthermore, a method for preparing a fire-resistant high-strength plastic pipe comprises the following preparation steps:
[0012] (1) Mix 30% sodium hydroxide solution, dichlorotoluene and polyolefin in a mass ratio of 130:50:27 to 130:50:31, stir at 0 to 5°C and 200 to 300 rpm for 20 to 30 min, add 0.3 to 0.5 times the mass of polyolefin 4,4'-dihydroxy-3,3'-glyoxal biphenyl, react at 200 to 300 rpm for 3 to 5 h, add hydrochloric acid until the solution pH is 1, filter, and vacuum dry at -0.08 MPa and 60°C for 24 h to obtain heat-resistant polyolefin;
[0013] (2) Heat-resistant polyolefin, anti-ultraviolet agent, nano-carbon fiber, refractory agent and dispersant are mixed in a mass ratio of 40:1:5:7:1-50:3:15:9:1, and the mass ratio of antimony trioxide, zinc borate and ceramic powder in the refractory agent is 3:1:6-5:1:8. Stir for 12 hours at 100-200 rpm and 180-200 °C, pour into a mold for molding, extrude and size determination to obtain a plastic tube with a diameter of 120 mm;
[0014] (3) Perfluorocarbazine and anhydrous ethanol are mixed in a mass ratio of 11:100-13:100, stirred at 200-300 rpm for 5-10 min, and then acetic acid is added until the pH of the solution is 6 to obtain a treatment solution; the plastic tube and the treatment solution are mixed in a mass ratio of 1:10-1:20, refluxed at 100-200 rpm and 40-80°C for 6-8 h, and then 1.5-2.5 times the mass of perfluorocarbazine cyclized product is added, and the reaction is continued for 6-8 h, and the tube is washed with anhydrous ethanol for 3-5 times and dried at room temperature for 1-2 h to obtain a fire-resistant high-strength plastic tube.
[0015] Furthermore, the polyolefin preparation method described in step (1) is as follows: 2-butenyltriethoxysilane, p-isopropenylacetophenone, 2-methylacrolein, and dibenzoyl peroxide are mixed in a mass ratio of 7:5:2:0.01-9:7:4:0.01, stirred at 100-200 rpm for 1-2 hours, reacted in a nitrogen atmosphere at 100-200 rpm and 80-100° C. for 6-8 hours, deionized water twice the mass of 2-butenyltriethoxysilane and triethylamine 0.002 times the mass of 2-butenyltriethoxysilane are added, the reaction is continued for 6-8 hours, cooled to 60° C., trichlorotrifluoroethane twice the mass of 2-butenyltriethoxysilane is added, and after standing for 1-3 hours, the lower layer of the mixed solution is removed and vacuum dried at -0.08 MPa and 50-60° C. for 12 hours to obtain the polyolefin.
[0016] Furthermore, the preparation method of the benzotriazole cyclized product in step (3) is as follows: the intermediate product 2, deionized water, anhydrous ethanol and sodium hydroxide are mixed in a mass ratio of 4:20:25:2~6:25:35:2, stirred at 200~300rpm and 80~100℃ for 10~20min, and sodium hydroxide powder with a mass of 1.1~1.3 times that of sodium hydroxide is added, and the reaction is continued for 2~3h, and deionized water is added at 0~5℃ until the precipitation is complete, and hydrochloric acid is added until the pH of the solution is 5~6, filtered, washed with anhydrous ethanol for 3~5 times, and dried at a vacuum degree of -0.085MPa and a temperature of 60~80℃ for 6~8h to obtain the benzotriazole cyclized product.
[0017] Furthermore, the preparation method of the intermediate product 2 is: mix the intermediate product 1, 3-tert-butyl-4-hydroxybenzaldehyde, sodium dodecylbenzene sulfonate, and methanol in a mass ratio of 22:22:2:70~50:24:3:70, reflux at 200~300rpm and 60~70°C for 4~6h, filter, wash with deionized water 3~5 times, and dry at a vacuum degree of -0.085MPa and 60~80°C for 6~8h to obtain the intermediate product 2.
[0018] Furthermore, the preparation method of the intermediate product 1 is: concentrated sulfuric acid, deionized water, and 4-butyl-2-nitroaniline are mixed in a mass ratio of 1:25:1.1~1:35:1.3, stirred at 0~5°C and 200~300rpm for 30~60min, and then 0.2~0.4 times the mass of concentrated sulfuric acid of sodium nitrite is added, and the reaction is continued for 2~3h, and 0.003~0.005 times the mass of concentrated sulfuric acid of aminosulfonic acid is added, filtered, and the solution is taken to obtain the intermediate product 1.
[0019] Compared with the prior art, the beneficial effects achieved by the present invention are:
[0020] The invention prepares a plastic pipe by mixing heat-resistant polyolefin with other additives, and then prepares the plastic pipe by finishing with an antibacterial agent to obtain a fire-resistant high-strength plastic pipe with heat-resistant and antibacterial effects.
[0021] Firstly, the heat-resistant polyolefin is prepared by the reaction of 2-butenyltriethoxysilane, p-isopropenylacetophenone, 2-methylacrolein and 4,4'-dihydroxy-3,3'-glyoxal biphenyl; 2-butenyltriethoxysilane, p-isopropenylacetophenone and 2-methylacrolein are polymerized to prepare the polyolefin, and the siloxane can be hydrolyzed and polymerized to form a silica network, and the thermal barrier effect, high temperature resistance effect and movement restriction effect on the polyolefin molecular chain of the silica network make the plastic pipe heat-resistant; the aldehyde group in 4,4'-dihydroxy-3,3'-glyoxal biphenyl reacts with the ketone group in p-isopropenylacetophenone to form a chalcone structure, so that the polyolefin is cross-linked and the cross-linking density of the polyolefin is increased. At the same time, the chalcone structure can react with the free radicals generated by the pipe under the action of high temperature to prevent them from damaging the thermal decomposition of the pipe, thereby enhancing the heat-resistant effect.
[0022] Secondly, the antibacterial agent is prepared from 4-butyl-2-nitroaniline, sodium nitrite, 3-tert-butyl-4-hydroxybenzaldehyde and perfluorocarbazine; the benzotriazole cyclized product is prepared by the reaction of 4-butyl-2-nitroaniline, sodium nitrite and 3-tert-butyl-4-hydroxybenzaldehyde, which can kill bacteria through the electrostatic adsorption of the triazole structure and the piercing effect of the alkyl chain in 4-butyl-2-nitroaniline, so that the plastic tube has an antibacterial effect; the aldehyde group in the benzotriazole cyclized product and the aldehyde group in the plastic tube react with the amino group in the perfluorocarbazine, so that the antibacterial agent is combined with the plastic tube, and a Schiff base structure is formed, which further enhances the antibacterial effect, and the fluorine chain is used to reduce the surface energy of the plastic tube, reduce the adhesion of bacteria to the tube wall, and enhance the antibacterial effect. DETAILED DESCRIPTION
[0023] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.
[0024] In order to more clearly illustrate the method provided by the present invention, the following examples are used to describe in detail the various index testing methods of the fire-resistant high-strength plastic pipes prepared in the following examples are as follows:
[0025] Heat resistance effect: After the same length of the embodiment and the comparative example were dried at 60°C for 12 hours, the 5% thermal decomposition temperature of the plastic tube was tested by a thermogravimetric analyzer under a nitrogen atmosphere, a flow rate of 50 mL / min, and a heating rate of 10°C / min;
[0026] Antibacterial effect: The antibacterial rate of the embodiment and the comparative example of the same length was tested according to GB / T31402.
[0027] Example 1
[0028] (1) 2-Butenyltriethoxysilane, 4-isopropenylacetophenone, 2-methylacrolein, and dibenzoyl peroxide were mixed in a mass ratio of 7:5:2:0.01, stirred at 100 rpm for 1 hour, reacted in a nitrogen atmosphere at 100 rpm and 80°C for 6 hours, and then deionized water twice the mass of 2-butenyltriethoxysilane and triethylamine 0.002 times the mass of 2-butenyltriethoxysilane were added, and the reaction was continued for 6 hours. The mixture was cooled to 60°C, and trichlorotrifluoroethane twice the mass of 2-butenyltriethoxysilane was added. After standing for 1 hour, the lower mixed liquid was taken out and vacuum dried at -0.08 MPa and 50°C for 12 hours to obtain polyolefin;
[0029] (2) Mix 30% sodium hydroxide solution, dichlorotoluene and polyolefin in a mass ratio of 130:50:27, stir at 0°C and 200 rpm for 20 min, add 0.3 times the mass of polyolefin 4,4'-dihydroxy-3,3'-glyoxal biphenyl, react at 200 rpm for 3 h, add hydrochloric acid until the pH of the solution is 1, filter, and vacuum dry at -0.08 MPa and 60°C for 24 h to obtain heat-resistant polyolefin;
[0030] (3) Heat-resistant polyolefin, nano-titanium dioxide, nano-carbon fiber, refractory agent, and dibutyl phthalate are mixed in a mass ratio of 40:1:5:7:1, and the mass ratio of antimony trioxide, zinc borate, and ceramic powder in the refractory agent is 3:1:6. The mixture is stirred at 100 rpm and 180°C for 12 h, poured into a mold, formed, extruded, and sized to obtain a plastic tube with a diameter of 120 mm.
[0031] (4) Concentrated sulfuric acid, deionized water, and 4-butyl-2-nitroaniline were mixed in a mass ratio of 1:25:1.1, stirred at 0°C and 200 rpm for 30 min, and then 0.2 times the mass of sodium nitrite as concentrated sulfuric acid was added. The reaction was continued for 2 h, and 0.003 times the mass of aminosulfonic acid as concentrated sulfuric acid was added. The mixture was filtered and the solution was obtained to obtain intermediate product 1.
[0032] (5) The intermediate product 1, 3-tert-butyl-4-hydroxybenzaldehyde, sodium dodecylbenzene sulfonate and methanol were mixed in a mass ratio of 22:22:2:70, refluxed at 200 rpm and 60°C for 4 h, filtered, washed with deionized water 3 times, and dried at a vacuum degree of -0.085 MPa and 60°C for 6 h to obtain the intermediate product 2;
[0033] (6) The intermediate product 2, deionized water, anhydrous ethanol and sodium hydroxide were mixed in a mass ratio of 4:20:25:2, stirred at 200 rpm and 80°C for 10 min, and sodium hydroxide powder with a mass of 1.1 times that of sodium hydroxide was added. The reaction was continued for 2 h, and deionized water was added at 0°C until the precipitation was complete. Hydrochloric acid was added until the pH of the solution was 5, filtered, washed with anhydrous ethanol for 3 times, and dried at a vacuum degree of -0.085 MPa and a temperature of 60°C for 6 h to obtain a benzotriazole cyclized product.
[0034] (7) Perfluorocarbazine and anhydrous ethanol were mixed in a mass ratio of 11:100, stirred at 200 rpm for 5 min, and then acetic acid was added until the pH of the solution was 6 to obtain a treatment solution; the plastic tube and the treatment solution were mixed in a mass ratio of 1:10, refluxed at 100 rpm and 40°C for 6 h, and then 1.5 times the mass of perfluorocarbazine cyclized product was added, and the reaction was continued for 6 h. The tube was washed with anhydrous ethanol for 3 times and dried at room temperature for 1 h to obtain a fire-resistant high-strength plastic tube.
[0035] Example 2
[0036] (1) 2-Butenyltriethoxysilane, 4-isopropenylacetophenone, 2-methylacrolein, and dibenzoyl peroxide were mixed in a mass ratio of 8:6:3:0.01, stirred at 150 rpm for 1.5 h, reacted in a nitrogen atmosphere at 150 rpm and 90°C for 7 h, then deionized water twice the mass of 2-butenyltriethoxysilane and triethylamine 0.002 times the mass of 2-butenyltriethoxysilane were added, and the reaction was continued for 7 h. The mixture was cooled to 60°C, and trichlorotrifluoroethane twice the mass of 2-butenyltriethoxysilane was added. After standing for 2 h, the lower mixed liquid was taken out and vacuum dried at -0.08 MPa and 55°C for 12 h to obtain polyolefin;
[0037] (2) Mix 30% sodium hydroxide solution, dichlorotoluene and polyolefin in a mass ratio of 130:50:29, stir at 3°C and 250 rpm for 25 min, add 0.4 times the mass of polyolefin 4,4'-dihydroxy-3,3'-glyoxal biphenyl, react at 250 rpm for 4 h, add hydrochloric acid until the pH of the solution is 1, filter, and vacuum dry at -0.08 MPa and 60°C for 24 h to obtain heat-resistant polyolefin;
[0038] (3) Heat-resistant polyolefin, nano-titanium dioxide, nano-carbon fiber, refractory agent, and dibutyl phthalate are mixed in a mass ratio of 45:2:10:8:1, and the mass ratio of antimony trioxide, zinc borate, and ceramic powder in the refractory agent is 4:1:7. The mixture is stirred at 150 rpm and 190°C for 12 h, poured into a mold, formed, extruded, and sized to obtain a plastic tube with a diameter of 120 mm.
[0039] (4) Concentrated sulfuric acid, deionized water, and 4-butyl-2-nitroaniline were mixed in a mass ratio of 1:30:1.2, stirred at 3°C and 250 rpm for 45 min, and then sodium nitrite in an amount 0.3 times the mass of concentrated sulfuric acid was added. The reaction was continued for 2.5 h, and aminosulfonic acid in an amount 0.004 times the mass of concentrated sulfuric acid was added. The mixture was filtered and the solution was obtained to obtain intermediate product 1;
[0040] (5) The intermediate product 1, 3-tert-butyl-4-hydroxybenzaldehyde, sodium dodecylbenzene sulfonate, and methanol were mixed in a mass ratio of 36:23:2.5:70, refluxed at 250 rpm and 65°C for 5 h, filtered, washed with deionized water 4 times, and dried at a vacuum degree of -0.085 MPa and 70°C for 7 h to obtain the intermediate product 2;
[0041] (6) The intermediate product 2, deionized water, anhydrous ethanol and sodium hydroxide were mixed in a mass ratio of 5:23:30:2, stirred at 250 rpm and 90°C for 15 min, and sodium hydroxide powder 1.2 times the mass of sodium hydroxide was added. The reaction was continued for 2.5 h, and deionized water was added at 3°C until the precipitation was complete. Hydrochloric acid was added until the pH of the solution was 5.5, filtered, washed with anhydrous ethanol for 4 times, and dried at a vacuum degree of -0.085 MPa and a temperature of 70°C for 7 h to obtain a benzotriazole cyclized product.
[0042] (7) Perfluorocarbazine and anhydrous ethanol were mixed in a mass ratio of 12:100, stirred at 250 rpm for 8 min, and then acetic acid was added until the pH of the solution was 6 to obtain a treatment solution; the plastic tube and the treatment solution were mixed in a mass ratio of 1:15, refluxed at 150 rpm and 60°C for 7 h, and then benzotriazole cyclized product with a mass twice that of perfluorocarbazine was added, and the reaction was continued for 7 h. The tube was washed with anhydrous ethanol for 4 times and dried at room temperature for 1.5 h to obtain a fire-resistant high-strength plastic tube.
[0043] Example 3
[0044] (1) 2-Butenyltriethoxysilane, 4-isopropenylacetophenone, 2-methylacrolein, and dibenzoyl peroxide were mixed in a mass ratio of 9:7:4:0.01, stirred at 200 rpm for 2 hours, reacted in a nitrogen atmosphere at 200 rpm and 100°C for 8 hours, and then deionized water twice the mass of 2-butenyltriethoxysilane and triethylamine 0.002 times the mass of 2-butenyltriethoxysilane were added, and the reaction was continued for 8 hours. The mixture was cooled to 60°C, and trichlorotrifluoroethane twice the mass of 2-butenyltriethoxysilane was added. After standing for 3 hours, the lower mixed liquid was taken out and vacuum dried at -0.08 MPa and 60°C for 12 hours to obtain polyolefin;
[0045] (2) Mix 30% sodium hydroxide solution, dichlorotoluene and polyolefin in a mass ratio of 130:50:31, stir at 5°C and 300 rpm for 30 min, add 0.5 times the mass of polyolefin 4,4'-dihydroxy-3,3'-glyoxal biphenyl, react at 300 rpm for 5 h, add hydrochloric acid until the solution pH is 1, filter, and vacuum dry at -0.08 MPa and 60°C for 24 h to obtain heat-resistant polyolefin;
[0046] (3) Heat-resistant polyolefin, nano-titanium dioxide, nano-carbon fiber, refractory agent, and dibutyl phthalate are mixed in a mass ratio of 50:3:15:9:1, and the mass ratio of antimony trioxide, zinc borate, and ceramic powder in the refractory agent is 5:1:8. The mixture is stirred at 200 rpm and 200°C for 12 hours, poured into a mold, formed, extruded, and sized to obtain a plastic tube with a diameter of 120 mm.
[0047] (4) Concentrated sulfuric acid, deionized water, and 4-butyl-2-nitroaniline were mixed in a mass ratio of 1:35:1.3, stirred at 5°C and 300 rpm for 60 min, and then sodium nitrite in an amount 0.4 times the mass of the concentrated sulfuric acid was added. The reaction was continued for 3 h, and aminosulfonic acid in an amount 0.005 times the mass of the concentrated sulfuric acid was added. The mixture was filtered and the solution was obtained to obtain an intermediate product 1.
[0048] (5) The intermediate product 1, 3-tert-butyl-4-hydroxybenzaldehyde, sodium dodecylbenzene sulfonate, and methanol were mixed in a mass ratio of 50:24:3:70, refluxed at 300 rpm and 70°C for 6 h, filtered, washed with deionized water 5 times, and dried at a vacuum degree of -0.085 MPa and 80°C for 8 h to obtain the intermediate product 2;
[0049] (6) The intermediate product 2, deionized water, anhydrous ethanol and sodium hydroxide were mixed in a mass ratio of 6:25:35:2, stirred at 300 rpm and 100°C for 20 min, and sodium hydroxide powder 1.3 times the mass of sodium hydroxide was added. The reaction was continued for 3 h, and deionized water was added at 5°C until the precipitation was complete. Hydrochloric acid was added until the pH of the solution was 6, filtered, washed with anhydrous ethanol 5 times, and dried at a vacuum degree of -0.085 MPa and a temperature of 80°C for 8 h to obtain a benzotriazole cyclized product.
[0050] (7) Perfluorocarbazine and anhydrous ethanol were mixed in a mass ratio of 13:100, stirred at 300 rpm for 10 min, and then acetic acid was added until the pH of the solution was 6 to obtain a treatment solution; the plastic tube and the treatment solution were mixed in a mass ratio of 1:20, refluxed at 200 rpm and 80°C for 8 h, and then benzotriazole cyclized product with a mass of 2.5 times that of perfluorocarbazine was added, and the reaction was continued for 8 h. The tube was washed with anhydrous ethanol for 5 times and dried at room temperature for 2 h to obtain a fire-resistant high-strength plastic tube.
[0051] Comparative Example 1
[0052] The difference between Comparative Example 1 and Example 2 is only that step (1) is different. Step (1) is changed to: p-isopropenylacetophenone, 2-methylacrolein, and dibenzoyl peroxide are mixed in a mass ratio of 6:3:0.01, stirred at 150 rpm for 1.5 hours, reacted at 150 rpm and 90° C. for 7 hours in a nitrogen atmosphere, and then deionized water 2.6 times the mass of p-isopropenylacetophenone and triethylamine 0.0026 times the mass of p-isopropenylacetophenone are added, and the reaction is continued for 7 hours. The mixture is cooled to 60° C., trichlorotrifluoroethane 2.6 times the mass of p-isopropenylacetophenone is added, and after standing for 2 hours, the lower mixed liquid is taken out and vacuum dried at -0.08 MPa and 55° C. for 12 hours to obtain a polyolefin. The remaining steps are the same as those in Example 2.
[0053] Comparative Example 2
[0054] The difference between Comparative Example 2 and Example 2 is that step (2) is omitted, and step (3) is changed to: polyolefin, nano-titanium dioxide, nano-carbon fiber, refractory agent, and dibutyl phthalate are mixed in a mass ratio of 45:2:10:8:1, and the mass ratio of antimony trioxide, zinc borate, and ceramic powder in the refractory agent is 4:1:7, and stirred at 150 rpm and 190° C. for 12 h, poured into a mold for molding, extruded, and sized to obtain a plastic tube with a diameter of 120 mm. The remaining steps are the same as those in Example 2.
[0055] Comparative Example 3
[0056] The difference between Comparative Example 3 and Example 2 is that there are no steps (4) to (6), and step (7) is changed to: perfluorocarbazine and anhydrous ethanol are mixed at a mass ratio of 12:100, stirred at 250 rpm for 8 minutes, and then acetic acid is added until the pH of the solution is 6 to obtain a treatment liquid; the plastic tube and the treatment liquid are mixed at a mass ratio of 1:15, refluxed at 150 rpm and 60° C. for 7 hours, and 3-tert-butyl-4-hydroxybenzaldehyde twice the mass of perfluorocarbazine is added, and the reaction is continued for 7 hours, washed with anhydrous ethanol 4 times, and dried at room temperature for 1.5 hours to obtain a fire-resistant high-strength plastic tube. The remaining steps are the same as those in Example 2.
[0057] Comparative Example 4
[0058] The difference between Comparative Example 4 and Example 2 is only that step (7) is different. Step (7) is changed to: benzotriazole cyclization product and anhydrous ethanol are mixed in a mass ratio of 24:100, stirred at 250 rpm for 8 minutes, and then acetic acid is added until the solution pH is 6 to obtain a treatment liquid; the plastic tube and the treatment liquid are mixed in a mass ratio of 1:15, refluxed at 150 rpm and 60° C. for 7 hours, washed with anhydrous ethanol 4 times, and dried at room temperature for 1.5 hours to obtain a fire-resistant high-strength plastic tube. The remaining steps are the same as those in Example 2.
[0059] Effect example
[0060] Table 1 below shows the performance analysis results of fire-resistant high-strength plastic pipes using Examples 1 to 3 of the present invention and Comparative Examples 1 to 4.
[0061] Table 1
[0062]
[0063] From the comparison of the 5% thermal decomposition temperature of the embodiment and the comparative example in Table 1, it can be found that the plastic pipe has good heat resistance. 2-Butenyltriethoxysilane, p-isopropenylacetophenone and 2-methylacrolein are polymerized to prepare polyolefin. The siloxane in 2-Butenyltriethoxysilane is hydrolyzed and polymerized to form a silica network. The thermal barrier effect, high temperature resistance effect and movement restriction effect of the silica network on the polyolefin molecular chain improve the heat resistance of the plastic pipe. The polyolefin further reacts with 4,4'-dihydroxy-3,3'-glyoxal biphenyl to form a chalcone structure, which crosslinks the polyolefin and improves the crosslinking density of the polyolefin. When the thermal oxidation reaction is inhibited, the heat resistance of the pipe is further improved; from the comparison of the antibacterial rate of the embodiment and the comparative example in Table 1, it can be found that the plastic pipe after antibacterial finishing has excellent antibacterial performance, 4-butyl-2-nitroaniline, sodium nitrite, and 3-tert-butyl-4-hydroxybenzaldehyde are reacted to prepare benzotriazole cyclized products, which can kill bacteria through the electrostatic adsorption of the triazole structure and the piercing effect of the alkyl chain in 4-butyl-2-nitroaniline. While the bacterial agent is combined with the plastic pipe through perfluorocarbazine, a Schiff base structure is formed, and the low surface energy of the fluorine chain is used to reduce the adhesion of bacteria to the pipe wall, thereby enhancing the antibacterial effect.
[0064] It will be apparent to those skilled in the art that the invention is not limited to the details of the exemplary embodiments described above and that the invention can be implemented in other specific forms without departing from the spirit or essential features of the invention. Therefore, the embodiments should be considered in all respects as exemplary and non-limiting, and the scope of the invention is defined by the appended claims rather than the foregoing description, and it is intended that all variations within the meaning and scope of the equivalent elements of the claims be included in the invention. Any marking in a claim should not be considered as limiting the claim to which it relates.
Claims
1. A method for preparing a fire-resistant high-strength plastic pipe, characterized in that: The method comprises the following preparation steps: (1) 2-Butenyltriethoxysilane, 4-isopropenylacetophenone, 2-methylacrolein, and dibenzoyl peroxide were mixed in a mass ratio of 8:6:3:0.01, stirred at 150 rpm for 1.5 h, reacted in a nitrogen atmosphere at 150 rpm and 90°C for 7 h, then deionized water twice the mass of 2-butenyltriethoxysilane and triethylamine 0.002 times the mass of 2-butenyltriethoxysilane were added, and the reaction was continued for 7 h. The mixture was cooled to 60°C, and trichlorotrifluoroethane twice the mass of 2-butenyltriethoxysilane was added. After standing for 2 h, the lower mixed liquid was taken out and vacuum dried at -0.08 MPa and 55°C for 12 h to obtain polyolefin; (2) Mix 30% sodium hydroxide solution, dichlorotoluene and polyolefin in a mass ratio of 130:50:29, stir at 3°C and 250 rpm for 25 min, add 0.4 times the mass of polyolefin 4,4'-dihydroxy-3,3'-glyoxal biphenyl, react at 250 rpm for 4 h, add hydrochloric acid until the pH of the solution is 1, filter, and vacuum dry at -0.08 MPa and 60°C for 24 h to obtain heat-resistant polyolefin; (3) Heat-resistant polyolefin, nano-titanium dioxide, nano-carbon fiber, refractory agent, and dibutyl phthalate are mixed in a mass ratio of 45:2:10:8:1, and the mass ratio of antimony trioxide, zinc borate, and ceramic powder in the refractory agent is 4:1:
7. The mixture is stirred at 150 rpm and 190°C for 12 h, poured into a mold, formed, extruded, and sized to obtain a plastic tube with a diameter of 120 mm. (4) Concentrated sulfuric acid, deionized water, and 4-butyl-2-nitroaniline were mixed in a mass ratio of 1:30:1.2, stirred at 3°C and 250 rpm for 45 min, and then sodium nitrite in an amount 0.3 times the mass of concentrated sulfuric acid was added. The reaction was continued for 2.5 h, and aminosulfonic acid in an amount 0.004 times the mass of concentrated sulfuric acid was added. The mixture was filtered and the solution was obtained to obtain intermediate product 1; (5) The intermediate product 1, 3-tert-butyl-4-hydroxybenzaldehyde, sodium dodecylbenzene sulfonate, and methanol were mixed in a mass ratio of 36:23:2.5:70, refluxed at 250 rpm and 65°C for 5 h, filtered, washed with deionized water 4 times, and dried at a vacuum degree of -0.085 MPa and 70°C for 7 h to obtain the intermediate product 2; (6) The intermediate product 2, deionized water, anhydrous ethanol and sodium hydroxide were mixed in a mass ratio of 5:23:30:2, stirred at 250 rpm and 90°C for 15 min, and sodium hydroxide powder 1.2 times the mass of sodium hydroxide was added. The reaction was continued for 2.5 h, and deionized water was added at 3°C until the precipitation was complete. Hydrochloric acid was added until the pH of the solution was 5.5, filtered, washed with anhydrous ethanol for 4 times, and dried at a vacuum degree of -0.085 MPa and a temperature of 70°C for 7 h to obtain a benzotriazole cyclized product. (7) Perfluorocarbazine and anhydrous ethanol were mixed in a mass ratio of 12:100, stirred at 250 rpm for 8 min, and then acetic acid was added until the pH of the solution was 6 to obtain a treatment solution; the plastic tube and the treatment solution were mixed in a mass ratio of 1:15, refluxed at 150 rpm and 60°C for 7 h, and then benzotriazole cyclized product with a mass twice that of perfluorocarbazine was added, and the reaction was continued for 7 h. The tube was washed with anhydrous ethanol for 4 times and dried at room temperature for 1.5 h to obtain a fire-resistant high-strength plastic tube.