A rare earth doped perovskite nanocrystal and preparation method thereof

The rare earth-doped perovskite nanocrystals were synthesized under vacuum through one-pot synthesis method, which solved the problem of complex operation and inability to mass production of the heat injection method, and achieved efficient and simple large-scale synthesis.

CN118006325BActive Publication Date: 2024-11-22HENAN DEXI BIOLOGICAL R&D TECH CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410089727.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-01-23
Publication Date
2024-11-22
Estimated Expiration
2044-01-23

AI Technical Summary

Technical Problem

In the prior art, the thermal injection method of rare earth-doped perovskite nanocrystals requires rapid injection and cooling at high temperatures, and the operation is complicated and cannot be achieved in batch or industrial production.

Method used

By using one-pot synthesis method, the cesium salt, lead salt, rare earth halide, alcohol, oleic acid, oleamine and 1-octene were mixed under vacuum, and the temperature and time were controlled to synthesize rare earth-doped perovskites. Nanocrystals, simplify process steps and improve product crystallinity and morphological rules.

Benefits of technology

It realizes efficient, simple and large-scale synthesis of rare earth-doped perovskite nanocrystals, reduces the operation complexity and the generation of product impurities, and is suitable for batch or industrial production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118006325B_ABST
    Figure CN118006325B_ABST
Patent Text Reader

Abstract

The invention discloses a rare earth doped perovskite nanocrystal and a preparation method thereof, and relates to the field of material technology. The rare earth doped perovskite nanocrystal of the invention comprises the following raw materials: cesium salt, lead salt, rare earth halide, alcohols, oleic acid, oleylamine, 1-octadecene, and the rare earth doped perovskite nanocrystal is obtained by a one-pot synthesis method from cesium salt, lead salt, rare earth halide, alcohols, oleic acid, oleylamine, and 1-octadecene, wherein the concentration of Cs in the cesium salt in the reaction system is 1-15 mmol / L; the concentration of Pb in the lead salt in the reaction system is 1-15 mmol / L; the concentration of the rare earth element in the rare earth halide in the reaction system is 1-45 mmol / L; the volume ratio of alcohols, oleic acid, oleylamine, and 1-octadecene is 1-10:1-10:1-10:10. The rare earth-doped perovskite nanocrystals of the present invention can be prepared by a one-pot synthesis method, which has the advantages of simple process steps, improved reaction efficiency, increased product yield and purity, and easy large-scale production.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of material technology, and in particular to a rare earth doped perovskite nanocrystal and a preparation method thereof. Background Art

[0002] Perovskite nanocrystals have unique optoelectronic properties, especially the adjustable band gap and high photoluminescence quantum yield in the visible light region, making them particularly suitable for many applications such as light-emitting diodes (LEDs), solar cells, and scintillators. Furthermore, by doping with certain rare earth elements, perovskite nanocrystals can further obtain advantages such as large absorption cross-section, good monochromaticity of emitted light, high energy transfer efficiency, and high photoluminescence quantum yield. In addition, rare earth ions can emit in the near-infrared region, and their wavelength can match the photovoltaic response region of crystalline silicon solar cells. Therefore, the synthesis of rare earth-doped perovskite nanomaterials with excellent performance is of great significance to photovoltaics, photoelectric detection, optical communications and other fields.

[0003] In the related art, rare earth doped perovskite nanocrystals are generally synthesized by hot injection method (i.e., injecting a certain solution into another solution at high temperature), and this method can prepare colloidal nanocrystals with controllable morphology, good dispersibility and high quantum efficiency. For example, patent CN116240019A discloses a method for preparing perovskite quantum dots by doping with rare earth and transition metals, and its preparation process is divided into two steps: cesium carbonate is used as a raw material to prepare cesium oleate solution in advance, and cesium oleate solution is solution 1; then lead, ytterbium and zinc halides are used as raw materials, oleic acid and oleylamine are used as ligands, and octadecene is used as solvent to prepare solution 2; at a higher temperature, solution 2 is quickly injected into solution 1, and the product is obtained after rapid cooling and separation. Patent CN112375566A discloses another preparation technology, which selects ytterbium oleate and lead oleate (both need to be prepared in advance) that are more easily soluble in the reaction system as reactants, and injects them into a chlorine source (TMS-Cl) at high temperature to obtain ytterbium-doped perovskite nanocrystals. This method avoids the problem of solid precipitation and turbidity of the solution at high temperature by reducing the presence of strong and weak acid ions in the solution.

[0004] It can be seen that the above-mentioned hot injection method requires the pre-synthesis of lead oleate, ytterbium oleate or cesium oleate, and then injects another reactant solution at high temperature. The reaction vessel needs to be immersed in ice water and cooled quickly within a few seconds after injection. Therefore, the hot injection method has high requirements on the operating speed and accuracy of the operator. In addition, the hot injection method can only inject a few milliliters of reactants. If the reaction system is increased, the precursor solution cannot be fully and quickly diffused during hot injection, which will cause problems such as uneven product particle size distribution and generation of impurities. Therefore, the hot injection method can only obtain samples less than 1 gram at a time, and cannot be mass-produced or industrialized.

[0005] Therefore, providing a method for mass production of rare earth-doped perovskite nanocrystals is a technical problem that needs to be solved urgently by those skilled in the art. Summary of the invention

[0006] The invention discloses a rare earth doped perovskite nanocrystal and a preparation method thereof, so as to solve the technical problems that a hot injection method is used in the related art to prepare rare earth doped perovskite nanocrystals, which requires two-step reactions, has high requirements on the speed and accuracy of operators, and cannot be mass-produced or industrialized.

[0007] In order to solve the above problems, the present invention adopts the following technical solutions:

[0008] A first aspect of the present invention provides a rare earth doped perovskite nanocrystal.

[0009] The rare earth doped perovskite nanocrystals of the present invention include the following raw materials: cesium salt, lead salt, rare earth halide, alcohols, oleic acid, oleylamine, 1-octadecene, and the rare earth doped perovskite nanocrystals are obtained from cesium salt, lead salt, rare earth halide, alcohols, oleic acid, oleylamine, 1-octadecene by a one-pot synthesis method, wherein:

[0010] The concentration of Cs in the cesium salt in the reaction system is 1 to 15 mmol / L;

[0011] The concentration of Pb in the lead salt in the reaction system is 1 to 15 mmol / L;

[0012] The concentration of the rare earth element in the rare earth halide in the reaction system is 1 to 45 mmol / L;

[0013] The volume ratio of the alcohol, the oleic acid, the oleylamine and the 1-octadecene is 1-10:1-10:1-10:10.

[0014] According to a preferred embodiment, the cesium salt is selected from one or more of cesium carbonate, cesium acetate, cesium oleate and cesium halide.

[0015] According to a preferred embodiment, the lead salt is selected from one or more of lead carbonate, lead acetate, lead oleate and lead halide.

[0016] According to a preferred embodiment, the rare earth element in the rare earth halide is one or more of La, Ce, Pr, Nd, Pm, Sm, Eu, Gd, Tb, Dy, Ho, Er, Tm, Yb, Lu, Y, and Sc, and the halogen element in the rare earth halide is one or more of Cl, Br, and I.

[0017] According to a preferred embodiment, the alcohol is methanol or ethanol.

[0018] The second aspect of the present invention provides a method for preparing rare earth-doped perovskite nanocrystals.

[0019] The method for preparing rare earth-doped perovskite nanocrystals according to any technical solution of the present invention comprises the following steps:

[0020] Step S100: taking cesium salt, lead salt, rare earth halide, alcohol, oleic acid, oleylamine, 1-octadecene, cesium salt, lead salt, rare earth halide, alcohol, oleic acid, oleylamine, 1-octadecene as reaction raw materials in proportion;

[0021] Step S200: placing cesium salt, lead salt, rare earth halide, alcohol, oleic acid, oleylamine, and 1-octadecene in a reaction container, and stirring and mixing at 100-160° C. under vacuum conditions;

[0022] Step S300: introducing nitrogen into the reaction container and maintaining the reaction container at normal pressure, heating the solution to 180-300° C. and keeping the temperature for 10-120 min;

[0023] Step S400: After cooling the reaction container, centrifuge and discard the supernatant, add a cleaning solvent for cleaning, centrifuge again and discard the supernatant, repeat the cleaning 1 to 3 times to obtain rare earth-doped perovskite nanocrystals.

[0024] According to a preferred embodiment, in step S200, the pressure in the reaction container is less than 1000 Pa;

[0025] The stirring speed is 600-1500 rpm and the stirring time is 1 h.

[0026] According to a preferred embodiment, in step S300, the solution is heated to 190-240°C and kept warm for 30 minutes.

[0027] According to a preferred embodiment, in step S400, the centrifugal speed is 5000-10000 r / min, and the centrifugal time is 5-20 min.

[0028] According to a preferred embodiment, in step S400, the cleaning solvent is one or more of n-hexane, cyclohexane, toluene, chloroform, methanol, and ethanol.

[0029] The technical solution adopted by the present invention can achieve the following beneficial effects:

[0030] In a first aspect, the rare earth-doped perovskite nanocrystals of the present invention include the following raw materials: cesium salt, lead salt, rare earth halide, alcohols, oleic acid, oleylamine, 1-octadecene, and the amount of each raw material is limited. Each raw material is a cheap and readily available chemical, and there is no need to prepare the reactants in advance. Each raw material can not only provide the elements required for the rare earth-doped perovskite nanocrystals, but also by adding alcohols to the raw materials, the alcohols are preferably polar solvents, more preferably easily removable polar solvents. The addition of alcohols can increase the solubility of each reactant, so that the rare earth-doped perovskite nanocrystals of the present invention can be synthesized by a one-pot synthesis method during preparation. Since the selected alcohols are easy to remove, the solvent can also be prevented from destroying the structure of the generated perovskite nanocrystals. The obtained perovskite nanocrystals have the advantages of high crystallinity and regular morphology.

[0031] In the second aspect, the preparation method of rare earth-doped perovskite nanocrystals of the present invention uses cesium salt, lead salt, rare earth halide, alcohol, oleic acid, oleylamine, and 1-octadecene as raw materials, and adopts a one-pot synthesis method to prepare rare earth-doped perovskite nanocrystals, that is, the preparation method of the present invention adds each raw material into the same reactor for reaction, and then obtains rare earth-doped perovskite nanocrystals after natural cooling and washing. It can be seen that the preparation method of the present invention can directly, simply, quickly, and synthesize rare earth-doped perovskite nanocrystals in large quantities, and has the advantages of simple process steps, improved reaction efficiency, improved product yield and purity, and easy large-scale production.

[0032] Compared with the hot injection method in the prior art, the one-pot synthesis method of the present invention does not require the pre-preparation of reactants such as cesium oleate and lead oleate, nor does it require the injection of another solution at high temperature, does not require a rapid cooling process, and has no restrictions on the amount of raw materials added, and has the possibility of large-scale preparation. Therefore, the one-pot synthesis method of the present invention solves the technical problems of the related art of using the hot injection method to prepare rare earth-doped perovskite nanocrystals, which requires two-step reactions, has high requirements on the speed and accuracy of the operator, and cannot be mass-produced or industrialized.

[0033] In a third aspect, the method for preparing rare earth-doped perovskite nanocrystals of the present invention comprises the following steps: adding the reaction raw materials to a reaction vessel, stirring and mixing the reaction raw materials at 100 to 160° C. under vacuum conditions. On the one hand, perovskite nanocrystals are sensitive to polar solvents, and alcohols or water in the raw materials will damage the structure of the perovskite nanocrystals. The stirring and mixing at 100 to 160° C. of the present invention is helpful in removing alcohols and water in the raw materials, thereby facilitating the maintenance of the integrity of the structure of the perovskite nanocrystals. On the other hand, oleic acid contains unsaturated double bonds, and is easily oxidized to generate products such as aldehydes, ketones and carboxylic acids under aerobic conditions. A higher reaction temperature will also accelerate the oxidation of oleic acid. The preparation method of the present invention maintains vacuum conditions in this step, and vacuum conditions are usually oxygen-free or have an extremely low oxygen content, thereby reducing or even avoiding the adverse effects caused by the oxidation of oleic acid. The preparation method of the present invention maintains vacuum conditions in this step, and can also avoid the problem that metal ions in the raw materials react with oxygen molecules to produce metal oxides, and impurities that are difficult to remove are introduced, resulting in reduced product yield and purity. BRIEF DESCRIPTION OF THE DRAWINGS

[0034] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0035] Figure 1 Yb in Examples 3, 6, and 9 3+ ∶X-ray diffraction (XRD) pattern of CsPbCl3 nanocrystals;

[0036] Figure 2 is Yb in Example 3 3+ ∶Transmission electron microscopy (TEM) image of CsPbCl3 nanocrystals;

[0037] Figure 3 Yb in Examples 1 to 9 3+ ∶Luminescence spectrum (PL) of CsPbCl3 nanocrystals;

[0038] Figure 4 The Yb of Examples 1 to 9 is shown. 3+ The ratio of the fluorescence emission peak intensity of CsPbCl3 nanocrystals in the near-infrared region and the visible region is related to the Yb 3+ Variation of doping amount. DETAILED DESCRIPTION

[0039] To make the purpose, technical solution and advantages of the present invention clearer, the technical solution of the present invention will be described in detail below. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments. Based on the embodiments of the present invention, all other implementation methods obtained by ordinary technicians in this field without creative work belong to the scope of protection of the present invention.

[0040] The terms "first", "second", etc. in the specification and claims of the present application are used to distinguish similar objects, and are not used to describe a specific order or sequence. It should be understood that the data used in this way can be interchangeable under appropriate circumstances, so that the embodiments of the present application can be implemented in an order other than those illustrated or described here, and the objects distinguished by "first", "second", etc. are generally of one type, and the number of objects is not limited. For example, the first object can be one or more. In addition, "and / or" in the specification and claims represents at least one of the connected objects, and the character " / " generally indicates that the objects associated with each other are in an "or" relationship.

[0041] In the related art, the hot injection method is used to prepare rare earth-doped perovskite nanocrystals. Generally, it is necessary to pre-synthesize lead oleate, ytterbium oleate or cesium oleate precursors (because in the solvent, lead oleate, ytterbium oleate and cesium oleate have better solubility than non-oleate cesium salts, lead salts and ytterbium salts), and then inject the prepared precursor into another reactant solution at high temperature. Within a few seconds after the injection, the reaction vessel needs to be immersed in ice water for rapid cooling. Therefore, the hot injection method has high requirements for the process and has high requirements for the operating speed and accuracy of the operator. In addition, the hot injection method can only inject a few milliliters of reactants. If the reaction system is enlarged, the precursor solution cannot be fully and quickly diffused during the hot injection, which will cause problems such as uneven product particle size distribution and impurities. Therefore, the hot injection method cannot be mass-produced.

[0042] To this end, the present application provides a rare earth-doped perovskite nanocrystal and a preparation method thereof. The rare earth-doped perovskite nanocrystal of the present application is synthesized by a one-pot synthesis method. The one-pot synthesis method directly uses a mixture of various raw materials as reactants, and the product can be obtained after heating to a specified temperature in a reaction container. Compared with the traditional hot injection method, the one-pot synthesis method of the present application does not require the pre-synthesis of lead oleate, ytterbium oleate or cesium oleate precursors, does not require precise control of the reaction time for several seconds, and does not require rapid immersion in an ice bath for cooling. Therefore, the one-pot synthesis method of the present application greatly reduces the complexity of the operation process and makes batch preparation or industrial preparation possible.

[0043] The one-pot synthesis method mentioned in this application is a chemical synthesis method, which refers to a method in which all raw materials are added to the same reaction container at one time, and the reaction process is completed by controlling the temperature, pressure and reaction time to finally obtain the target product.

[0044] The rare earth-doped perovskite nanocrystals and the preparation method thereof provided by the present invention are described in detail below.

[0045] The rare earth doped perovskite nanocrystals of the present invention are prepared by a one-pot synthesis method. Preferably, the rare earth doped perovskite nanocrystals include the following raw materials: cesium salt, lead salt, rare earth halide, alcohol, oleic acid, oleylamine, 1-octadecene. More preferably, the concentration of Cs in the cesium salt in the reaction system is 1 to 15 mmol / L; the concentration of Pb in the lead salt in the reaction system is 1 to 15 mmol / L; the concentration of the rare earth element in the rare earth halide in the reaction system is 1 to 45 mmol / L; the volume ratio of alcohol, oleic acid, oleylamine, and 1-octadecene is 1 to 10:1 to 10:1 to 10:10.

[0046] Preferably, the cesium salt is selected from one or more of cesium carbonate, cesium acetate, cesium oleate and cesium halide.

[0047] Preferably, the lead salt is selected from one or more of lead carbonate, lead acetate, lead oleate and lead halide.

[0048] Preferably, the rare earth element in the rare earth halide is one or more of La, Ce, Pr, Nd, Pm, Sm, Eu, Gd, Tb, Dy, Ho, Er, Tm, Yb, Lu, Y, and Sc, and the halogen element in the rare earth halide is one or more of Cl, Br, and I.

[0049] Preferably, the alcohol is methanol or ethanol.

[0050] The rare earth-doped perovskite nanocrystals of the present invention include the following raw materials: cesium salt, lead salt, rare earth halide, alcohol, oleic acid, oleylamine, 1-octadecene, and the amount of each raw material is limited. Each raw material is a cheap and readily available chemical, and there is no need to prepare the reactants in advance; each raw material can not only provide the elements required for the rare earth-doped perovskite nanocrystals, but also by adding alcohols to the raw materials, the alcohols are preferably polar solvents. By adding alcohols, the solubility of each reactant can be increased, so that the rare earth-doped perovskite nanocrystals of the present invention can be synthesized by a one-pot synthesis method during preparation; further, the alcohols added to the raw materials are more preferably easily removable polar solvents, so that the added polar solvents can be removed in subsequent steps to avoid the polar solvents from affecting the structure of the obtained product. Exemplarily, the easily removable polar solvent added is methanol or ethanol.

[0051] Furthermore, perovskite nanocrystals are sensitive to solvents. The alcohols selected in the present invention are methanol or ethanol, which are easy to remove. Therefore, the solvents can be prevented from destroying the structure of the generated perovskite nanocrystals. The obtained perovskite nanocrystals have the advantages of high crystallinity and regular morphology.

[0052] The method for preparing rare earth-doped perovskite nanocrystals according to any technical solution of the present invention comprises the following steps:

[0053] Step S100: Take cesium salt, lead salt, rare earth halide, alcohol, oleic acid, oleylamine, 1-octadecene as reaction raw materials in proportion. Specifically, each raw material is prepared in the following proportion: the concentration of Cs in the cesium salt in the reaction system is 1-15 mmol / L; the concentration of Pb in the lead salt in the reaction system is 1-15 mmol / L; the concentration of rare earth elements in the rare earth halide in the reaction system is 1-45 mmol / L; the volume ratio of alcohol, oleic acid, oleylamine, 1-octadecene is 1-10:1-10:1-10:10.

[0054] Step S200: Put cesium salt, lead salt, rare earth halide, alcohol, oleic acid, oleylamine and 1-octadecene into a reaction container, and stir and mix them at 100-160° C. under vacuum conditions. Preferably, the pressure in the reaction container is less than 1000 Pa.

[0055] The method for preparing rare earth doped perovskite nanocrystals of the present invention comprises the following steps: adding various reaction raw materials into a reaction container, stirring and mixing them at 100-160° C. and under vacuum conditions; on the one hand, the perovskite nanocrystals are sensitive to polar solvents, and alcohols or water in the raw materials will damage the structure of the perovskite nanocrystals; stirring and mixing at 100-160° C. in the present invention is helpful to remove alcohols and water in the raw materials, thereby facilitating the maintenance of the integrity of the structure of the perovskite nanocrystals; on the other hand, oleic acid contains unsaturated double bonds, and is easily oxidized to generate products such as aldehydes, ketones and carboxylic acids under aerobic conditions; a higher reaction temperature will also accelerate the oxidation of oleic acid; the method for preparing the present invention maintains vacuum conditions in this step, and the pressure in the reaction container is preferably less than 1000 Pa; under vacuum conditions, there is usually no oxygen or extremely low oxygen content, so the adverse effects caused by the oxidation of oleic acid can be reduced or even avoided; the method for preparing the present invention maintains vacuum conditions in this step, and can also avoid the problem that metal ions in the raw materials react with oxygen molecules to produce metal oxides, and impurities that are difficult to remove are introduced, resulting in reduced product yield and purity.

[0056] Preferably, the stirring speed is 600-1500 rpm, and the stirring time is 1 hour. Furthermore, in the method for preparing rare earth-doped perovskite nanocrystals of the present invention, after adding each reaction raw material to the reaction container, stirring at a speed of 600-1500 rpm for 1 hour, using a higher stirring intensity is helpful to obtain perovskite nanocrystals with high crystallinity and regular morphology. Specifically, in this step, using a higher stirring intensity can make each reaction raw material fully mixed before reaching the explosive nucleation temperature of the perovskite nanocrystal, avoiding the different nucleation of the perovskite nanocrystal and the uneven crystal growth.

[0057] Step S300: introduce nitrogen into the reaction container and keep the reaction container at normal pressure, heat the solution to 180-300° C., and keep the temperature for 10-120 min. Preferably, heat the solution to 190-240° C., and keep the temperature for 30 min.

[0058] The fluorescence peak intensity of rare earth doped perovskite nanocrystals is controlled by the rare earth doping amount. In the related technology, the fluorescence peak can only be regulated by changing the rare earth ratio in the raw materials. If you need to obtain crystals with different fluorescence intensities, you need to prepare different proportions of reactant solutions. Specifically, the existing hot injection synthesis method mainly controls the growth of rare earth doped perovskite nanocrystals by kinetics, and the reaction needs to be terminated by ice bath in a very short time. The doping of rare earth ions is to replace Pb 2+ The process of entering the perovskite lattice has a high energy barrier and is not completed instantly. Therefore, under the constraints of a certain reaction temperature and an extremely short reaction time, it is difficult to regulate the fluorescence emission peak intensity by controlling the reaction time. The fluorescence emission peak intensity can only be regulated by changing the rare earth ratio and the reaction temperature.

[0059] The method for preparing rare earth-doped perovskite nanocrystals of the present invention can control the thermodynamic and kinetic balance of rare earth ion doping by controlling the reaction temperature and reaction time of this step, that is, the rare earth doping amount can be adjusted, thereby adjusting the peak intensity of fluorescence emission of the nanocrystals. By controlling the reaction temperature and reaction time, the peak intensity of fluorescence emission of nanocrystals is controlled. Compared with the method of controlling the peak intensity of fluorescence emission of nanocrystals by the rare earth ratio, it is easier and more accurate to control the optical properties of nanocrystals; at the same time, there is no need to change the reaction system, which is more convenient in the actual production process, laying the foundation for the industrial application of rare earth-doped perovskite nanocrystals.

[0060] It can be seen that through the preparation method of rare earth-doped perovskite nanocrystals of the present invention, rare earth-doped perovskite nanocrystals with adjustable fluorescence properties can be obtained.

[0061] Step S400: After cooling the reaction container, centrifuge and discard the supernatant, add a cleaning solvent for cleaning, centrifuge again and discard the supernatant, repeat the cleaning 1 to 3 times to obtain rare earth doped perovskite nanocrystals. Preferably, the centrifugal speed is 5000 to 10000 r / min, and the centrifugal time is 5 to 20 min. Preferably, the cleaning solvent is one or more of n-hexane, cyclohexane, toluene, chloroform, methanol, and ethanol.

[0062] In the above technical scheme, the preparation method of rare earth-doped perovskite nanocrystals of the present invention uses cesium salt, lead salt, rare earth halide, alcohol, oleic acid, oleylamine, and 1-octadecene as raw materials, and adopts a one-pot synthesis method to prepare rare earth-doped perovskite nanocrystals, that is, the preparation method of the present invention adds each raw material into the same reactor for reaction, and then obtains rare earth-doped perovskite nanocrystals after natural cooling and washing. It can be seen that the preparation method of the present invention can directly, simply, quickly, and synthesize rare earth-doped perovskite nanocrystals in large quantities, and has the advantages of simple process steps (specifically, it can simplify the reaction steps, reduce the product separation and purification process, and simplify the complex synthesis route), improve reaction efficiency, improve product yield and purity, and be easy to scale production.

[0063] Compared with the hot injection method in the prior art, the one-pot synthesis method of the present invention does not require the pre-preparation of reactants such as cesium oleate and lead oleate, nor does it require the injection of another solution at high temperature, does not require a rapid cooling process, and has no restrictions on the amount of raw materials added, and has the possibility of large-scale preparation. Therefore, the one-pot synthesis method of the present invention solves the technical problems of the related art of using the hot injection method to prepare rare earth-doped perovskite nanocrystals, which requires two-step reactions, has high requirements on the speed and accuracy of the operator, and cannot be mass-produced or industrialized.

[0064] The following is combined with Figures 1 to 4 , the rare earth-doped perovskite nanocrystals and the preparation method thereof provided by the present invention are described in detail through specific embodiments.

[0065] The reagents, methods and equipment used in the following examples are conventional reagents, methods and equipment in the art unless otherwise specified. The glassware used was washed with deionized water and anhydrous ethanol and then dried before use.

[0066] Example 1

[0067] Yb in this embodiment 3+ :CsPbCl3 nanocrystals include the following raw materials: 0.492mmol cesium carbonate, 0.984mmol lead (II) acetate trihydrate, 2.46mmol ytterbium (III) chloride hexahydrate, 8ml methanol, 16ml oleic acid, 16ml oleylamine, and 80ml 1-octadecene.

[0068] Yb in this embodiment 3+ ∶The preparation method of CsPbCl3 nanocrystals comprises the following steps:

[0069] Step S100: 0.492 mmol cesium carbonate, 0.984 mmol lead (II) acetate trihydrate, 2.46 mmol ytterbium (III) chloride hexahydrate, 8 ml methanol, 16 ml oleic acid, 16 ml oleylamine, and 80 ml 1-octadecene are taken as reaction raw materials.

[0070] Step S200: Add cesium carbonate, lead (II) acetate trihydrate, ytterbium (III) chloride hexahydrate, methanol, oleic acid, oleylamine, and 1-octadecene into a three-necked flask, stir and mix at 110° C. and a pressure of 1000 Pa. The stirring speed is 1000 rpm and the stirring time is 1 hour.

[0071] Step S300: nitrogen is introduced into the three-necked flask to maintain normal pressure in the three-necked flask, the solution is heated to 190° C., and the temperature is kept to react for 10 minutes.

[0072] Step S400: The reaction solution was allowed to stand and cool, the reaction solution was collected, centrifuged at 7500 r / min for 10 min, the supernatant was discarded, 35 ml of n-hexane was added to the precipitate, and centrifuged at 10000 r / min for 8 min. This was repeated twice to further separate and purify Yb 3+ ∶CsPbCl3 nanocrystals.

[0073] Add 10 ml of n-hexane to the precipitate, redisperse the precipitate, and let it stand overnight. The supernatant is a stable Yb 3+ ∶CsPbCl3 nanocrystal colloidal solution. After standing, the Yb 3+ ∶CsPbCl3 nanocrystal colloidal solution, the crystals are evenly dispersed without serious aggregation, and are used for TEM sample preparation and optical performance testing. 3+ ∶CsPbCl3 nanocrystals were collected by vacuum freeze drying for bulk storage and phase and elemental composition analysis.

[0074] Example 2

[0075] Yb in this embodiment 3+ :CsPbCl3 nanocrystals include the following raw materials: 0.492mmol cesium carbonate, 0.984mmol lead (II) acetate trihydrate, 2.46mmol ytterbium (III) chloride hexahydrate, 8ml methanol, 16ml oleic acid, 16ml oleylamine, and 80ml 1-octadecene.

[0076] Yb in this embodiment 3+∶The preparation method of CsPbCl3 nanocrystals comprises the following steps:

[0077] Step S100: 0.492 mmol cesium carbonate, 0.984 mmol lead (II) acetate trihydrate, 2.46 mmol ytterbium (III) chloride hexahydrate, 8 ml methanol, 16 ml oleic acid, 16 ml oleylamine, and 80 ml 1-octadecene are taken as reaction raw materials.

[0078] Step S200: Add cesium carbonate, lead (II) acetate trihydrate, ytterbium (III) chloride hexahydrate, methanol, oleic acid, oleylamine, and 1-octadecene into a three-necked flask, stir and mix at 110° C. and a pressure of 1000 Pa. The stirring speed is 1000 rpm and the stirring time is 1 hour.

[0079] Step S300: nitrogen is introduced into the three-necked flask to maintain normal pressure in the three-necked flask, the solution is heated to 190° C., and the temperature is kept to react for 20 minutes.

[0080] Step S400: The reaction solution was allowed to stand and cool, the reaction solution was collected, centrifuged at 7500 r / min for 10 min, the supernatant was discarded, 35 ml of n-hexane was added to the precipitate, and centrifuged at 10000 r / min for 8 min. This was repeated twice to further separate and purify Yb 3+ ∶CsPbCl3 nanocrystals.

[0081] Add 10 ml of n-hexane to the precipitate, redisperse the precipitate, and let it stand overnight. The supernatant is a stable Yb 3+ ∶CsPbCl3 nanocrystal colloidal solution.

[0082] Example 3

[0083] Yb in this embodiment 3+ :CsPbCl3 nanocrystals include the following raw materials: 0.492mmol cesium carbonate, 0.984mmol lead (II) acetate trihydrate, 2.46mmol ytterbium (III) chloride hexahydrate, 8ml methanol, 16ml oleic acid, 16ml oleylamine, and 80ml 1-octadecene.

[0084] Yb in this embodiment 3+ ∶The preparation method of CsPbCl3 nanocrystals comprises the following steps:

[0085] Step S100: 0.492 mmol cesium carbonate, 0.984 mmol lead (II) acetate trihydrate, 2.46 mmol ytterbium (III) chloride hexahydrate, 8 ml methanol, 16 ml oleic acid, 16 ml oleylamine, and 80 ml 1-octadecene are taken as reaction raw materials.

[0086] Step S200: Add cesium carbonate, lead (II) acetate trihydrate, ytterbium (III) chloride hexahydrate, methanol, oleic acid, oleylamine, and 1-octadecene into a three-necked flask, stir and mix at 110° C. and a pressure of 1000 Pa. The stirring speed is 1000 rpm and the stirring time is 1 hour.

[0087] Step S300: nitrogen is introduced into the three-necked flask to maintain normal pressure in the three-necked flask, the solution is heated to 190° C., and the temperature is kept to react for 30 minutes.

[0088] Step S400: The reaction solution was allowed to stand and cool, the reaction solution was collected, centrifuged at 7500 r / min for 10 min, the supernatant was discarded, 35 ml of n-hexane was added to the precipitate, and centrifuged at 10000 r / min for 8 min. This was repeated twice to further separate and purify Yb 3+ ∶CsPbCl3 nanocrystals.

[0089] Add 10 ml of n-hexane to the precipitate, redisperse the precipitate, and let it stand overnight. The supernatant is a stable Yb 3+ ∶CsPbCl3 nanocrystal colloidal solution.

[0090] Example 4

[0091] Yb in this embodiment 3+ :CsPbCl3 nanocrystals include the following raw materials: 0.492mmol cesium carbonate, 0.984mmol lead (II) acetate trihydrate, 2.46mmol ytterbium (III) chloride hexahydrate, 8ml methanol, 16ml oleic acid, 16ml oleylamine, and 80ml 1-octadecene.

[0092] Yb in this embodiment 3+ ∶The preparation method of CsPbCl3 nanocrystals comprises the following steps:

[0093] Step S100: 0.492 mmol cesium carbonate, 0.984 mmol lead (II) acetate trihydrate, 2.46 mmol ytterbium (III) chloride hexahydrate, 8 ml methanol, 16 ml oleic acid, 16 ml oleylamine, and 80 ml 1-octadecene are taken as reaction raw materials.

[0094] Step S200: Add cesium carbonate, lead (II) acetate trihydrate, ytterbium (III) chloride hexahydrate, methanol, oleic acid, oleylamine, and 1-octadecene into a three-necked flask, stir and mix at 110° C. and a pressure of 1000 Pa. The stirring speed is 1000 rpm and the stirring time is 1 hour.

[0095] Step S300: nitrogen is introduced into the three-necked flask to maintain normal pressure in the three-necked flask, the solution is heated to 210° C., and the temperature is kept to react for 10 minutes.

[0096] Step S400: The reaction solution was allowed to stand and cool, the reaction solution was collected, centrifuged at 7500 r / min for 10 min, the supernatant was discarded, 35 ml of n-hexane was added to the precipitate, and centrifuged at 10000 r / min for 8 min. This was repeated twice to further separate and purify Yb 3+ ∶CsPbCl3 nanocrystals.

[0097] Add 10 ml of n-hexane to the precipitate, redisperse the precipitate, and let it stand overnight. The supernatant is a stable Yb 3+ ∶CsPbCl3 nanocrystal colloidal solution.

[0098] Example 5

[0099] Yb in this embodiment 3+ :CsPbCl3 nanocrystals include the following raw materials: 0.492mmol cesium carbonate, 0.984mmol lead (II) acetate trihydrate, 2.46mmol ytterbium (III) chloride hexahydrate, 8ml methanol, 16ml oleic acid, 16ml oleylamine, and 80ml 1-octadecene.

[0100] Yb in this embodiment 3+ ∶The preparation method of CsPbCl3 nanocrystals comprises the following steps:

[0101] Step S100: 0.492 mmol cesium carbonate, 0.984 mmol lead (II) acetate trihydrate, 2.46 mmol ytterbium (III) chloride hexahydrate, 8 ml methanol, 16 ml oleic acid, 16 ml oleylamine, and 80 ml 1-octadecene are taken as reaction raw materials.

[0102] Step S200: Add cesium carbonate, lead (II) acetate trihydrate, ytterbium (III) chloride hexahydrate, methanol, oleic acid, oleylamine, and 1-octadecene into a three-necked flask, stir and mix at 110° C. and a pressure of 1000 Pa. The stirring speed is 1000 rpm and the stirring time is 1 hour.

[0103] Step S300: nitrogen is introduced into the three-necked flask to maintain normal pressure in the three-necked flask, the solution is heated to 210° C., and the temperature is kept to react for 20 minutes.

[0104] Step S400: The reaction solution was allowed to stand and cool, the reaction solution was collected, centrifuged at 7500 r / min for 10 min, the supernatant was discarded, 35 ml of n-hexane was added to the precipitate, and centrifuged at 10000 r / min for 8 min. This was repeated twice to further separate and purify Yb 3+ ∶CsPbCl3 nanocrystals.

[0105] Add 10 ml of n-hexane to the precipitate, redisperse the precipitate, and let it stand overnight. The supernatant is a stable Yb 3+ ∶CsPbCl3 nanocrystal colloidal solution.

[0106] Example 6

[0107] Yb in this embodiment 3+ :CsPbCl3 nanocrystals include the following raw materials: 0.492mmol cesium carbonate, 0.984mmol lead (II) acetate trihydrate, 2.46mmol ytterbium (III) chloride hexahydrate, 8ml methanol, 16ml oleic acid, 16ml oleylamine, and 80ml 1-octadecene.

[0108] Yb in this embodiment 3+ ∶The preparation method of CsPbCl3 nanocrystals comprises the following steps:

[0109] Step S100: 0.492 mmol cesium carbonate, 0.984 mmol lead (II) acetate trihydrate, 2.46 mmol ytterbium (III) chloride hexahydrate, 8 ml methanol, 16 ml oleic acid, 16 ml oleylamine, and 80 ml 1-octadecene are taken as reaction raw materials.

[0110] Step S200: Add cesium carbonate, lead (II) acetate trihydrate, ytterbium (III) chloride hexahydrate, methanol, oleic acid, oleylamine, and 1-octadecene into a three-necked flask, stir and mix at 110° C. and a pressure of 1000 Pa. The stirring speed is 1000 rpm and the stirring time is 1 hour.

[0111] Step S300: nitrogen is introduced into the three-necked flask to maintain normal pressure in the three-necked flask, the solution is heated to 210° C., and the temperature is kept to react for 30 minutes.

[0112] Step S400: The reaction solution was allowed to stand and cool, the reaction solution was collected, centrifuged at 7500 r / min for 10 min, the supernatant was discarded, 35 ml of n-hexane was added to the precipitate, and centrifuged at 10000 r / min for 8 min. This was repeated twice to further separate and purify Yb 3+ ∶CsPbCl3 nanocrystals.

[0113] Add 10 ml of n-hexane to the precipitate, redisperse the precipitate, and let it stand overnight. The supernatant is a stable Yb 3+ ∶CsPbCl3 nanocrystal colloidal solution.

[0114] Example 7

[0115] Yb in this embodiment 3+:CsPbCl3 nanocrystals include the following raw materials: 0.492mmol cesium carbonate, 0.984mmol lead (II) acetate trihydrate, 2.46mmol ytterbium (III) chloride hexahydrate, 8ml methanol, 16ml oleic acid, 16ml oleylamine, and 80ml 1-octadecene.

[0116] Yb in this embodiment 3+ ∶The preparation method of CsPbCl3 nanocrystals comprises the following steps:

[0117] Step S100: 0.492 mmol cesium carbonate, 0.984 mmol lead (II) acetate trihydrate, 2.46 mmol ytterbium (III) chloride hexahydrate, 8 ml methanol, 16 ml oleic acid, 16 ml oleylamine, and 80 ml 1-octadecene are taken as reaction raw materials.

[0118] Step S200: Add cesium carbonate, lead (II) acetate trihydrate, ytterbium (III) chloride hexahydrate, methanol, oleic acid, oleylamine, and 1-octadecene into a three-necked flask, stir and mix at 110° C. and a pressure of 1000 Pa. The stirring speed is 1000 rpm and the stirring time is 1 hour.

[0119] Step S300: nitrogen is introduced into the three-necked flask to maintain normal pressure in the three-necked flask, the solution is heated to 240° C., and the reaction is carried out at this temperature for 10 minutes.

[0120] Step S400: The reaction solution was allowed to stand and cool, the reaction solution was collected, centrifuged at 7500 r / min for 10 min, the supernatant was discarded, 35 ml of n-hexane was added to the precipitate, and centrifuged at 10000 r / min for 8 min. This was repeated twice to further separate and purify Yb 3+ ∶CsPbCl3 nanocrystals.

[0121] Add 10 ml of n-hexane to the precipitate, redisperse the precipitate, and let it stand overnight. The supernatant is a stable Yb 3+ ∶CsPbCl3 nanocrystal colloidal solution.

[0122] Example 8

[0123] Yb in this embodiment 3+ :CsPbCl3 nanocrystals include the following raw materials: 0.492mmol cesium carbonate, 0.984mmol lead (II) acetate trihydrate, 2.46mmol ytterbium (III) chloride hexahydrate, 8ml methanol, 16ml oleic acid, 16ml oleylamine, and 80ml 1-octadecene.

[0124] Yb in this embodiment 3+ ∶The preparation method of CsPbCl3 nanocrystals comprises the following steps:

[0125] Step S100: 0.492 mmol cesium carbonate, 0.984 mmol lead (II) acetate trihydrate, 2.46 mmol ytterbium (III) chloride hexahydrate, 8 ml methanol, 16 ml oleic acid, 16 ml oleylamine, and 80 ml 1-octadecene are taken as reaction raw materials.

[0126] Step S200: Add cesium carbonate, lead (II) acetate trihydrate, ytterbium (III) chloride hexahydrate, methanol, oleic acid, oleylamine, and 1-octadecene into a three-necked flask, stir and mix at 110° C. and a pressure of 1000 Pa. The stirring speed is 1000 rpm and the stirring time is 1 hour.

[0127] Step S300: nitrogen is introduced into the three-necked flask to maintain normal pressure in the three-necked flask, the solution is heated to 240° C., and the temperature is kept to react for 20 minutes.

[0128] Step S400: The reaction solution was allowed to stand and cool, the reaction solution was collected, centrifuged at 7500 r / min for 10 min, the supernatant was discarded, 35 ml of n-hexane was added to the precipitate, and centrifuged at 10000 r / min for 8 min. This was repeated twice to further separate and purify Yb 3+ ∶CsPbCl3 nanocrystals.

[0129] Add 10 ml of n-hexane to the precipitate, redisperse the precipitate, and let it stand overnight. The supernatant is a stable Yb 3+ ∶CsPbCl3 nanocrystal colloidal solution.

[0130] Example 9

[0131] Yb in this embodiment 3+ :CsPbCl3 nanocrystals include the following raw materials: 0.492mmol cesium carbonate, 0.984mmol lead (II) acetate trihydrate, 2.46mmol ytterbium (III) chloride hexahydrate, 8ml methanol, 16ml oleic acid, 16ml oleylamine, and 80ml 1-octadecene.

[0132] Yb in this embodiment 3+ ∶The preparation method of CsPbCl3 nanocrystals comprises the following steps:

[0133] Step S100: 0.492 mmol cesium carbonate, 0.984 mmol lead (II) acetate trihydrate, 2.46 mmol ytterbium (III) chloride hexahydrate, 8 ml methanol, 16 ml oleic acid, 16 ml oleylamine, and 80 ml 1-octadecene are taken as reaction raw materials.

[0134] Step S200: Add cesium carbonate, lead (II) acetate trihydrate, ytterbium (III) chloride hexahydrate, methanol, oleic acid, oleylamine, and 1-octadecene into a three-necked flask, stir and mix at 110° C. and a pressure of 1000 Pa. The stirring speed is 1000 rpm and the stirring time is 1 hour.

[0135] Step S300: nitrogen is introduced into the three-necked flask to maintain the internal pressure of the three-necked flask, the solution is heated to 240° C., and the temperature is kept to react for 30 minutes.

[0136] Step S400: The reaction solution was allowed to stand and cool, the reaction solution was collected, centrifuged at 7500 r / min for 10 min, the supernatant was discarded, 35 ml of n-hexane was added to the precipitate, and centrifuged at 10000 r / min for 8 min. This was repeated twice to further separate and purify Yb 3+ ∶CsPbCl3 nanocrystals.

[0137] Add 10 ml of n-hexane to the precipitate, redisperse the precipitate, and let it stand overnight. The supernatant is a stable Yb 3+ ∶CsPbCl3 nanocrystal colloidal solution.

[0138] The Yb obtained in Examples 1 to 9 3+ ∶XRD, TEM, PL, fluorescence emission peak intensity and Yb 3+ Doping detection.

[0139] Yb 3+ The method for XRD detection of CsPbCl3 nanocrystals is as follows: using a Rigaku MiniFlex II X-ray diffractometer to identify the Yb in Examples 3, 6 and 9. 3+ ∶The crystal phase structure inside the CsPbCl3 nanocrystal, the 2θ range is 10° to 90°, the scanning speed is 5° per minute, and the position of the diffraction peak is compared with the peak position corresponding to the standard card JCPDS NO.75-0408. The test results are as follows Figure 1 shown.

[0140] Yb 3+ The method for TEM detection of CsPbCl3 nanocrystals is as follows: on a TALOS L120C G2 transmission electron microscope, the Yb 3+ ∶CsPbCl3 nanocrystals were observed under microscope. The results are as follows Figure 2 shown.

[0141] Yb 3+The method for PL detection of CsPbCl3 nanocrystals is as follows: the fluorescence spectrum in the visible light and near-infrared wavelength range is detected by PG2000-Pro fiber optic spectrometer, and the wavelength range is 195-1120nm. The data is plotted using origin software, and the peak intensity of the fluorescence peak in the visible light region and the near-infrared region is used as I Vis and I NIR , take I NIR with I Vis The ratio is I NIR :I Vis The results are as follows Figure 3 shown.

[0142] Yb 3+ The method for detecting the fluorescence emission peak intensity of CsPbCl3 nanocrystals is as follows: the PL detection data is imported into the origin data drawing software to draw the PL spectrum of the nanocrystals. The drawing results are as follows: Figure 3 As shown, the peak position and peak intensity are determined by the peak search function.

[0143] Yb 3+ ∶CsPbCl3 nanocrystals for Yb 3+ The method for detecting the doping amount is as follows: the Yb 3+ ∶The Yb and Pb content of CsPbCl3 nanocrystals was tested. 3+ The doping amount is expressed by Yb% = Ybat% / (Yb at% + Pb at%). The test results are as follows: Figure 4 shown.

[0144] The Yb obtained in Examples 1 to 9 3+ ∶XRD, TEM, PL, fluorescence emission peak intensity and Yb 3+ The results of the doping test are as follows Figure 1 to Figure 4 shown.

[0145] Figure 1 The Yb of Examples 3, 6 and 9 is shown. 3+ ∶X-ray diffraction (XRD) pattern of CsPbCl3 nanocrystals. Figure 1 As shown in the figure, Yb synthesized at reaction temperatures of 190°C, 210°C and 240°C and a holding time of 30 min 3+ The XRD diffraction peak position of CsPbCl3 nanocrystals is consistent with the cubic phase CsPbCl3 standard card (PDF#75-0408), indicating that Yb synthesized in Examples 3, 6 and 9 3+ ∶CsPbCl3 nanocrystals are single cubic phase with very high phase purity.

[0146] Figure 2 The Yb of Example 3 is shown 3+ ∶ Transmission electron microscopy (TEM) image of CsPbCl3 nanocrystals. Figure 2 As shown, Yb in Example 3 3+ : The CsPbCl3 nanocrystals are nanocrystals with clear morphology and regular shapes. 3+ ∶The side length of CsPbCl3 nanocrystals is less than 100nm.

[0147] Figure 3 The Yb of Examples 1 to 9 is shown. 3+ ∶The fluorescence spectrum (PL) of CsPbCl3 nanocrystals. Figure 3 As shown, the Yb synthesized in Examples 1 to 9 3+ ∶CsPbCl3 nanocrystals have perovskite emission peaks and Yb in the visible light region (around 410nm) and near infrared region (around 990nm). 3+ Emission peak.

[0148] from Figure 3 It can also be known that: through Yb 3+ The successful doping of CsPbCl3 perovskite nanocrystals (around 410nm) and Yb ions (around 990nm) simultaneously achieved efficient light emission.

[0149] Figure 4 The Yb of Examples 1 to 9 is shown. 3+ The ratio of the fluorescence emission peak intensity of CsPbCl3 nanocrystals in the near-infrared region and the visible region is related to the Yb 3+ The change of doping amount. With the increase of reaction temperature and the extension of reaction time, Yb 3+ The ratio of the fluorescence emission peak intensity of CsPbCl3 nanocrystals in the near-infrared region and the visible light region gradually increases. Yb 3+ ∶CsPbCl3 nanocrystals, Yb 3+ The doping amount gradually increases, Yb 3+ ∶ Fluorescence emission peak intensity of CsPbCl3 nanocrystals I NIR :I Vis At a reaction temperature of 240 °C, the reaction time was extended from 10 min to 30 min, and Yb 3+ As the doping level increases, the response I NIR :I Vis That is, the preparation method of the present invention can obtain different rare earth doping amounts by simply controlling the reaction temperature and reaction time, thereby regulating the Yb 3+∶Fluorescence emission peak intensity of CsPbCl3 nanocrystals.

[0150] It should be noted that, in this article, the terms "comprise", "include" or any other variant thereof are intended to cover non-exclusive inclusion, so that the process, method, article or device including a series of elements includes not only those elements, but also includes other elements not explicitly listed, or also includes elements inherent to such process, method, article or device. In the absence of further restrictions, the elements defined by the sentence "comprise one..." do not exclude the presence of other identical elements in the process, method, article or device including the element. In addition, it should be pointed out that the scope of the methods and devices in the embodiments of the present application is not limited to performing functions in the order shown or discussed, and may also include performing functions in a substantially simultaneous manner or in reverse order according to the functions involved, for example, the described method may be performed in an order different from that described, and various steps may also be added, omitted, or combined. In addition, the features described with reference to certain examples may be combined in other examples.

[0151] The above description is only a specific implementation mode of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can easily think of changes or substitutions within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.

Claims

1. A one-pot synthesis method for preparing rare earth-doped perovskite nanocrystals, characterized in that: The steps include: Step S100: taking cesium salt, lead salt, rare earth halide, alcohol, oleic acid, oleylamine, 1-octadecene, cesium salt, lead salt, rare earth halide, alcohol, oleic acid, oleylamine, 1-octadecene as reaction raw materials in proportion; Wherein, the cesium salt is cesium carbonate, and the concentration of Cs in the cesium salt in the reaction system is 8.2 mmol / L; The concentration of Pb in the lead salt in the reaction system is 8.2 mmol / L; The concentration of the rare earth element in the rare earth halide in the reaction system is 20.5 mmol / L; The volume ratio of the alcohol, the oleic acid, the oleylamine, and the 1-octadecene is 1-10:1-10:1-10:10; The alcohol is methanol or ethanol; Step S200: putting cesium salt, lead salt, rare earth halide, alcohol, oleic acid, oleylamine and 1-octadecene into a reaction container, and stirring and mixing at 100-160° C. under vacuum conditions; Wherein, the pressure in the reaction container is less than 1000Pa; The stirring speed is 600~1500rpm, and the stirring time is 1h; Step S300: introducing nitrogen into the reaction container and maintaining the reaction container at normal pressure, heating the solution to 190-240° C. and keeping the temperature for 30 min; Step S400: After cooling the reaction container, centrifuge and discard the supernatant, add a cleaning solvent for cleaning, centrifuge again and discard the supernatant, repeat the cleaning 1 to 3 times to obtain rare earth-doped perovskite nanocrystals.

2. The method for preparing rare earth-doped perovskite nanocrystals according to claim 1, characterized in that: In step S400, the centrifugal speed is 5000-10000 r / min, and the centrifugal time is 5-20 min.

3. The method for preparing rare earth-doped perovskite nanocrystals according to claim 1, characterized in that: In step S400, the cleaning solvent is one or more of n-hexane, cyclohexane, toluene, chloroform, methanol, and ethanol.