A sulfide solid electrolyte film and its preparation method and application

Through physical mixing and in-situ curing of lithium conduction polymer precursors, lithium salts and crown ether compounds with sulfides, the problem of low conductivity of sulfide solid electrolyte films is solved, and high ionic conductivity and battery performance are improved.

CN118016980BActive Publication Date: 2024-11-05GAO NENG SHI DAI (SHEN ZHEN) XIN NENG YUAN KE JI YOU XIAN GONG SI
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202311574640.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-11-22
Publication Date
2024-11-05
Estimated Expiration
2043-11-22

AI Technical Summary

Technical Problem

In the prior art, the ionic conductivity of the sulfide solid electrolyte film is low, the traditional binder has no lithium conduction effect, and a large amount of organic solvents will destroy the sulfide structure and reduce the conductivity.

Method used

The lithium-conducting polymer precursor, lithium salt and crown ether compounds are physically mixed with sulfides and cured in situ to prepare a sulfide solid electrolyte film with high ionic conductivity, avoiding non-lithium-conducting polymerization in traditional wet coating introduction of binders and solvents.

Benefits of technology

The ionic conductivity of the sulfide solid electrolyte film is significantly improved, the battery performance is enhanced, and the film forming and chemical stability are improved through the three-dimensional mesh structure formed by the lithium-conducting polymer binder.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004566652340000111
    Figure BDA0004566652340000111
  • Figure BDA0004566652340000121
    Figure BDA0004566652340000121
  • Figure HDA0004566652360000011
    Figure HDA0004566652360000011
Patent Text Reader

Abstract

The present invention belongs to the technical field of battery materials, and discloses a sulfide solid electrolyte film and a preparation method and application thereof. The raw material components of the sulfide solid electrolyte film include sulfide, lithium-conductive polymer precursor, lithium salt, crown ether compound, and initiator. The lithium-conductive polymer precursor provided by the present invention is compounded with sulfide in the form of a liquid precursor and wet-coated, and in the presence of an initiator, lithium salt and crown ether compound, in-situ curing is performed, thereby avoiding the problem of the introduction of non-lithium-conductive polymer binders and a large amount of solvents in traditional wet coating, which reduces the ionic conductivity of the solid electrolyte, thereby improving the battery performance of the all-solid-state battery.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of battery materials, and in particular relates to a sulfide solid electrolyte film and a preparation method and application thereof. Background Art

[0002] All-solid-state batteries have attracted much attention due to their long cycle life, high energy density, and high safety compared to commercial liquid lithium-ion batteries. The core component of all-solid-state batteries is solid electrolytes. Currently, solid electrolytes in lithium-ion batteries include polymer electrolytes, oxide electrolytes, and sulfide electrolytes. Compared with polymer and oxide solid electrolytes, sulfide solid electrolytes have higher ionic conductivity (10 -4 -10 -2 S / cm), and has certain advantages such as flexibility and low hardness, and is considered to be the most promising type of solid electrolyte currently.

[0003] In order to enable the sulfide solid electrolyte to form a film over a large area, a certain amount of polymer binder needs to be added to ensure the film-forming property of the sulfide electrolyte. In the prior art, the binder of the sulfide electrolyte mainly adopts a rubber binder, including nitrile rubber (NBR), styrene butadiene rubber (SBR) and a fluorine-containing polymer binder, specifically polyvinylidene fluoride (PVDF), polyvinylidene fluoride-hexafluoropropylene (PVDF-HFP) and polytetrafluoroethylene (PTFE). These traditional binders have no lithium conductivity, and after compounding with the sulfide electrolyte, the overall electrolyte film ion conductivity will be reduced.

[0004] In addition, the existing technology often uses a large amount of organic solvent to mix sulfide and polymer evenly and then wet-coates them to prepare a large-area electrolyte film. The presence of a large amount of organic solvent will change or destroy the structure of the sulfide, thereby reducing the ionic conductivity of the electrolyte.

[0005] Therefore, in view of the defects of the prior art, it is urgently necessary to provide a sulfide solid electrolyte film with high ionic conductivity. Summary of the invention

[0006] The present invention aims to solve at least one of the technical problems existing in the above-mentioned prior art. To this end, the present invention provides a sulfide solid electrolyte film and a preparation method and application thereof, which can obtain a large-area high-ion conductivity sulfide solid electrolyte film.

[0007] A first aspect of the present invention provides a sulfide solid electrolyte film.

[0008] Specifically, a sulfide solid electrolyte film, the raw material components include sulfide, lithium-conducting polymer precursor, lithium salt, crown ether compound, and initiator.

[0009] Preferably, the lithium-conducting polymer precursor is a polymer precursor containing an ether bond (-COC-) and / or an ester group (-OC=O).

[0010] Preferably, the molecular weight of the lithium-conducting polymer precursor is 50.0-1000.0 g / mol, more preferably 100-800 g / mol.

[0011] Preferably, the lithium-conducting polymer precursor includes at least one of polyethylene glycol diacrylate, trimethylolpropane triacrylate, trimethylolpropane trimethacrylate, pentaerythritol triacrylate, pentaerythritol tetraacrylate, and 4-ethoxypentaerythritol tetraacrylate, and at least one of polyethylene glycol methyl ether acrylate, polyethylene glycol methacrylate, ethoxyethyl acrylate, methyl acrylate, methyl methacrylate, ethyl acrylate, butyl acrylate, 2-ethylhexyl acrylate, hydroxyethyl acrylate, hydroxyethyl methacrylate, allyl sulfonic acid, methacrylic acid, and 2-phenoxyethyl methacrylate.

[0012] Preferably, the sulfide is selected from Li3PS4, Li4P2S6 or Li 7-a PS 6-a X a At least one of, wherein X is at least one of Cl, Br, I, and the value of a is 0.5-2.

[0013] Preferably, the sulfide is in powder form, with a particle size of 0.1-150 μm, more preferably 0.1-100 μm.

[0014] Preferably, the lithium salt is selected from at least one of LiClO4, LiPF6, LiBF4, LiTFSI (lithium bis(trifluoromethanesulfonyl)imide), LiFSI (lithium bis(fluorosulfonyl)imide), LiBOB (lithium bis(oxalatoborate)) and LiPO2F2.

[0015] Preferably, the crown ether compound is selected from at least one of 12-crown-4, 15-crown-5, 18-crown-6, benzo-18-crown-6 and dibenzo-18-crown-6.

[0016] Preferably, the initiator comprises a thermal initiator and / or a photoinitiator. Specific initiators include azobisisobutyronitrile, benzoyl peroxide, 1-hydroxycyclohexyl phenyl ketone, and diphenylethanedione.

[0017] Preferably, the sulfide accounts for 55-93.5% of the mass of the sulfide solid electrolyte film, and more preferably 64-88.5%.

[0018] Preferably, the lithium-conducting polymer precursor accounts for 3-30% of the mass of the sulfide solid electrolyte film, and more preferably 5-20%. The lithium-conducting polymer precursor is used as a lithium-conducting polymer binder.

[0019] Preferably, the lithium salt accounts for 3-12% of the mass of the sulfide solid electrolyte film, and more preferably 5-10%.

[0020] Preferably, the crown ether compound accounts for 0.5-4% of the mass of the sulfide solid electrolyte film, and more preferably 1-2%.

[0021] Preferably, the initiator accounts for 0.1-1.5% of the mass of the lithium-conducting polymer precursor, and more preferably 0.1-1.0%.

[0022] Preferably, the thickness of the sulfide solid electrolyte film is 100-200 μm, more preferably 100-150 μm.

[0023] A second aspect of the present invention provides a method for preparing a sulfide solid electrolyte film.

[0024] Specifically, a method for preparing a sulfide solid electrolyte film comprises the following steps:

[0025] mixing the components to obtain a mixture;

[0026] The mixture is coated on a substrate for curing, drying and pressing to obtain the sulfide solid electrolyte film.

[0027] Preferably, the components are mixed in proportion and placed in a magnetic stirring apparatus for uniform mixing. More preferably, the magnetic stirring speed is 100-1000 rpm / min, and more preferably, the stirring time is 12h-48h.

[0028] Preferably, the curing conditions are a thermal curing temperature of 65-75°C or a curing wavelength of 365-385nm, and more preferably, a UV intensity of 5-20mW / cm 2 , UV irradiation time 10-20min.

[0029] Preferably, the drying temperature is 65-75°C, such as 65°C, 70°C, 75°C.

[0030] Preferably, the pressing is roller pressing, which plays a role of thinning.

[0031] Preferably, a roller press is used for pressing, the roller speed of the roller press is 0.5-10 m / min, the roller temperature is preferably 40° C.-55° C., and the sulfide solid electrolyte film after rolling is 100-150 μm.

[0032] A third aspect of the present invention provides an application of a sulfide solid electrolyte film.

[0033] A battery comprises the above-mentioned sulfide solid electrolyte film.

[0034] Preferably, the battery is a lithium-ion battery.

[0035] Compared with the prior art, the beneficial effects of the present invention are as follows:

[0036] (1) The lithium-conductive polymer precursor provided by the present invention is compounded with a sulfide (solid electrolyte) in the form of a liquid precursor and wet-coated, and in situ cured in the presence of an initiator, a lithium salt and a crown ether compound, thereby avoiding the problem of a decrease in the ionic conductivity of the solid electrolyte due to the introduction of a non-lithium-conductive polymer binder and a large amount of solvent in traditional wet coating, thereby improving the battery performance of the all-solid-state battery.

[0037] (2) The cured sulfide solid electrolyte film of the present invention has good film-forming property and chemical stability due to the three-dimensional network structure formed by the cured lithium-conducting polymer precursor (polymer binder).

[0038] (3) In the sulfide solid electrolyte film of the present invention, the sulfide (solid electrolyte), the lithium-conducting polymer precursor (polymer binder) cross-linked network and the crown ether compound provide lithium-conducting effects at the same time, thereby significantly improving the ionic conductivity of the sulfide solid electrolyte film. BRIEF DESCRIPTION OF THE DRAWINGS

[0039] Figure 1 It is a schematic diagram of the attack of solvent molecules on the sulfide electrolyte in the prior art wet coating;

[0040] Figure 2 It is a schematic diagram of the working principle of a solid electrolyte film formed by using a polymer binder to prepare a sulfide electrolyte in the prior art;

[0041] Figure 3 It is a schematic diagram of the working principle of the sulfide solid electrolyte film of the present invention;

[0042] Figure 4 is the Arrhenius fitting diagram of the ionic conductivity of the sulfide solid electrolyte film of the comparative example and embodiment 1-2;

[0043] Figure 5 It is the Arrhenius fitting diagram of the ionic conductivity of the sulfide solid electrolyte film of Example 3-8. DETAILED DESCRIPTION

[0044] In order to make the technical scheme of the present invention more clearly understood by those skilled in the art, the following embodiments are listed for illustration. It should be pointed out that the following embodiments do not limit the protection scope of the present invention.

[0045] Unless otherwise specified, the raw materials, reagents or devices used in the following examples can be obtained from conventional commercial sources or by existing known methods.

[0046] See also Figure 1 and Figure 2 ( Figure 1 It is a schematic diagram of the attack of solvent molecules on the sulfide electrolyte in the prior art wet coating; Figure 2 It is a schematic diagram of the working principle of a solid electrolyte film formed by preparing a sulfide electrolyte using a polymer binder in the prior art). When the existing sulfide electrolyte 12 is formed into a film on a large area, a certain amount of polymer binder 11 needs to be added to ensure the film-forming property of the sulfide electrolyte. During wet coating, the solvent molecules 10 in the composite electrolyte solution 100 will change or destroy the structure of the sulfide electrolyte 12, thereby reducing the ionic conductivity of the electrolyte film. In addition, the traditional polymer binder 11 has no lithium-conducting effect. The component that conducts lithium ions 13 in the electrolyte film 200 formed after coating is only the sulfide electrolyte itself.

[0047] Based on this, an embodiment of the present invention provides a sulfide solid electrolyte film and a preparation method thereof, wherein the raw material components include: sulfide, a lithium-conducting polymer precursor, a lithium salt and a crown ether compound; the lithium-conducting polymer precursor, the lithium salt and the crown ether compound are dispersed in the sulfide in a physically mixed form, and then in-situ cured to form a film.

[0048] See also Figure 3 ( Figure 3 is a schematic diagram of the working principle of the sulfide solid electrolyte film of the present invention, Figure 3 In one embodiment, the sulfide solid electrolyte film 300 contains sulfide ( Figure 3 In addition to the lithium-conducting function of the octagonal black dot in the middle, there are two other components that also have lithium-conducting functions, namely: the lithium-conducting polymer precursor 15 that is polymerized in situ to form a network structure and the lithium-conducting polymer precursor 15 that can react with Li + The crown ether compound 14 performs complexation and decomplexation, thereby improving the ionic conductivity of the sulfide electrolyte membrane.

[0049] In one embodiment, the lithium-conducting polymer precursor is a polymer precursor containing lithium-conducting ether bonds (—COC—) and / or ester groups (—OC═O).

[0050] In one embodiment, the lithium-conducting polymer precursor includes at least one of polyethylene glycol diacrylate, trimethylolpropane triacrylate, trimethylolpropane trimethacrylate, pentaerythritol triacrylate, pentaerythritol tetraacrylate and 4-ethoxypentaerythritol tetraacrylate with multiple functional groups, and polyethylene glycol methyl ether acrylate, polyethylene glycol methacrylate, ethoxyethyl acrylate, methyl acrylate, methyl methacrylate, ethyl acrylate, butyl acrylate, 2-ethylhexyl acrylate, hydroxyethyl acrylate, hydroxyethyl methacrylate, allyl sulfonic acid, methacrylic acid, 2-phenoxyethyl methacrylate, or one or more thereof.

[0051] The method for preparing the sulfide solid electrolyte film comprises the following steps:

[0052] mixing a sulfide, a polymer precursor, a lithium salt, a crown ether compound and an initiator to obtain a mixture;

[0053] After the mixture slurry is coated on a glass substrate, in-situ thermal curing or light curing is performed;

[0054] vacuum drying the solidified composite electrolyte;

[0055] The dried composite electrolyte is heated and rolled to be thinned to obtain a sulfide solid electrolyte film.

[0056] In one embodiment, the sulfide, polymer precursor, lithium salt, crown ether compound and initiator are placed in a magnetic stirring apparatus in proportion and mixed evenly, the magnetic stirring speed is 100-1000 rpm / min, and the stirring time is 12h-48h.

[0057] In one embodiment, the sulfide is Li3PS4, Li4P2S6 or Li 7-a PS 6-a X a One or more of, wherein X is at least one of Cl, Br, I, and the value of a is 0.5-2.

[0058] In one embodiment, the lithium salt is one or more of LiClO4, LiPF6, LiBF4, LiTFSI, LiFSI, LiBOB and LiPO2F2, and the lithium salt accounts for 5-10% of the total mass of the sulfide solid electrolyte film.

[0059] In one embodiment, the crown ether compound is one or more of 12-crown-4, 15-crown-5, 18-crown-6, benzo-18-crown-6 and dibenzo-18-crown-6, and the crown ether compound accounts for 1-2% of the total mass of the sulfide solid electrolyte film.

[0060] In one embodiment, the content of thermal initiator and photoinitiator accounts for 0.1-1.0% of the weight of polymer precursor; the thermal initiator is azobisisobutyronitrile and benzoyl peroxide; the thermal curing and drying temperature of polymer precursor is 70°C; the photocuring initiator is 1-hydroxycyclohexyl phenyl ketone and diphenylethanedione; the photocuring wavelength is 365-385nm, and the ultraviolet light intensity is 5-20mW / cm 2 , UV irradiation time is 10-20min.

[0061] In one embodiment, the lithium-conducting polymer precursor accounts for 5.0%-20.0% of the mass of the sulfide solid electrolyte film.

[0062] In one embodiment, a roller press is used in the roller thinning process, the roller speed of the roller press is 0.5-10 m / min, the roller temperature is 40° C.-55° C., and the thickness of the sulfide solid electrolyte film after rolling is 100-150 μm (the thickness before rolling is 150-200 μm).

[0063] In one embodiment, the molecular weight of the lithium-conducting polymer precursor is 50.0-1000.0 g / mol, and the particle size of the sulfide powder is 0.1-150 μm.

[0064] A lithium-ion battery, comprising a sulfide solid electrolyte film.

[0065] Ionic conductivity test of sulfide solid electrolyte film: In a glove box, CR2016 button battery components were used to assemble steel sheet | sulfide solid electrolyte film | steel sheet battery, and the test was performed using Chenhua CHI760E electrochemical workstation. The resistance (R / Ω) of the sulfide solid electrolyte film was obtained by the EIS AC impedance test method, and the thickness (L / cm) and area (S / cm 2 ), using the formula σ=L / (R*S), the ionic conductivity of the sulfide solid electrolyte film (σ / S*cm -1 ).

[0066] The ionic conductivity of the sulfide itself can be obtained by pressing the sulfide powder into a sheet at a pressure of 310 MPa in a tablet press mold, and then using a CR2016 button battery assembly to assemble a steel sheet | sheet sulfide | steel sheet battery for testing.

[0067] Example 1: Preparation of sulfide solid electrolyte film-1

[0068] The preparation method of sulfide solid electrolyte film-1 comprises the following steps:

[0069] S1: In a glove box filled with argon, 1.46 g of Li3PS4 sulfide, 0.1 g of LiTFSI, 0.04 g of 18-crown ether-6 and 4 mg of azobisisobutyronitrile were weighed into a beaker and mixed to obtain a mixture;

[0070] S2: Add 0.34 mmol of trimethylolpropane trimethacrylate (TMPTMA) and 2.3 mmol of butyl acrylate (BA) to the mixture of step S1, and stir magnetically for 24 hours at a magnetic stirring speed of 600 rpm to obtain an electrolyte slurry;

[0071] S3: placing the electrolyte slurry obtained in step S2 on a smooth polytetrafluoroethylene plate and coating it with a 200 μm coating surface in a four-sided coater;

[0072] S4: After the polytetrafluoroethylene plate coated with the electrolyte slurry in S3 was placed in a vacuum oven at 70°C for in-situ curing for 12 hours, the prepared sulfide solid electrolyte film was peeled off from the polytetrafluoroethylene plate. The thickness of the obtained sulfide solid electrolyte film was 160 μm.

[0073] S5: The sulfide solid electrolyte film prepared in S4 is placed on a roller mill for roller thinning treatment. The roller speed of the roller mill is 1.5 m / min, and the roller temperature is 50°C. The thickness of the sulfide solid electrolyte film after rolling is about 110 μm. Subsequently, a steel sheet | sulfide solid electrolyte film | steel sheet battery is assembled for testing.

[0074] Example 2: Preparation of sulfide solid electrolyte film-2

[0075] The preparation method of sulfide solid electrolyte film-2 comprises the following steps:

[0076] S1: In a glove box filled with argon, 1.46 g of Li3PS4 sulfide, 0.1 g of LiTFSI, 0.04 g of 18-crown ether-6 and 4 mg of azobisisobutyronitrile were weighed into a beaker and mixed to obtain a mixture;

[0077] S2: Add 0.3 mmol of polyethylene glycol diacrylate (PEGDA) and 0.28 mmol of polyethylene glycol methacrylate (PEGMA) to the mixture of step S1, and stir magnetically for 24 h at a magnetic stirring speed of 600 rpm to obtain an electrolyte slurry;

[0078] S3: placing the electrolyte slurry obtained in step S2 on a smooth polytetrafluoroethylene plate and coating it with a 200 μm coating surface in a four-sided coater;

[0079] S4: After the polytetrafluoroethylene plate coated with the electrolyte slurry in S3 was placed in a vacuum oven at 70°C for in-situ curing for 12 hours, the prepared sulfide solid electrolyte film was peeled off from the polytetrafluoroethylene plate. The thickness of the obtained sulfide solid electrolyte film was 180 μm.

[0080] S5: The sulfide solid electrolyte film prepared in S4 is placed on a roller mill for roller thinning treatment. The roller speed of the roller mill is 1.5 m / min, and the roller temperature is 50°C. The thickness of the sulfide solid electrolyte film after rolling is about 120 μm. Subsequently, a steel sheet | sulfide solid electrolyte film | steel sheet battery is assembled for testing.

[0081] Example 3: Preparation of sulfide solid electrolyte film-3

[0082] The preparation method of sulfide solid electrolyte film-3 comprises the following steps:

[0083] S1: In a glove box filled with argon, weigh 1.46 g of Li7P3S 11 Sulfide, 0.1 g of LiTFSI, 0.04 g of 18-crown ether-6 and 4 mg of azobisisobutyronitrile were mixed in a beaker to obtain a mixture;

[0084] S2: Add 0.3 mmol of polyethylene glycol diacrylate (PEGDA) and 0.28 mmol of polyethylene glycol methacrylate (PEGMA) to the mixture of step S1, and stir magnetically for 24 h at a magnetic stirring speed of 600 rpm to obtain an electrolyte slurry;

[0085] S3: placing the electrolyte slurry obtained in step S2 on a smooth polytetrafluoroethylene plate and coating it with a 200 μm coating surface in a four-sided coater;

[0086] S4: After the polytetrafluoroethylene plate coated with the electrolyte slurry in S3 was placed in a vacuum oven at 70°C for in-situ curing for 12 hours, the prepared sulfide solid electrolyte film was peeled off from the polytetrafluoroethylene plate. The thickness of the obtained sulfide solid electrolyte film was 180 μm.

[0087] S5: The sulfide solid electrolyte film prepared in S4 is placed on a roller mill for roller thinning treatment. The roller speed of the roller mill is 1.5 m / min, and the roller temperature is 50°C. The thickness of the sulfide solid electrolyte film after rolling is about 130 μm. Then, a steel sheet | sulfide solid electrolyte film | steel sheet battery is assembled for testing.

[0088] Example 4: Preparation of sulfide solid electrolyte film-4

[0089] The preparation method of sulfide solid electrolyte film-4 comprises the following steps:

[0090] S1: In a glove box filled with argon, 1.46 g of Li6PS5Br sulfide, 0.1 g of LiTFSI, 0.04 g of 18-crown ether-6 and 4 mg of azobisisobutyronitrile were weighed into a beaker and mixed to obtain a mixture;

[0091] S2: Add 0.3 mmol of polyethylene glycol diacrylate (PEGDA) and 0.28 mmol of polyethylene glycol methacrylate (PEGMA) to the mixture of step S1, and stir magnetically for 24 h at a magnetic stirring speed of 600 rpm to obtain an electrolyte slurry;

[0092] S3: placing the electrolyte slurry obtained in step S2 on a smooth polytetrafluoroethylene plate and coating it with a 200 μm coating surface in a four-sided coater;

[0093] S4: After the polytetrafluoroethylene plate coated with the electrolyte slurry in S3 was placed in a vacuum oven at 70°C for in-situ curing for 12 hours, the prepared sulfide solid electrolyte film was peeled off from the polytetrafluoroethylene plate. The thickness of the obtained sulfide solid electrolyte film was 180 μm.

[0094] S5: The sulfide solid electrolyte film prepared in S4 is placed on a roller mill for roller thinning treatment. The roller speed of the roller mill is 1.5 m / min, and the roller temperature is 50°C. The thickness of the sulfide solid electrolyte film after rolling is about 120 μm. Subsequently, a steel sheet | sulfide solid electrolyte film | steel sheet battery is assembled for testing.

[0095] Example 5: Preparation of sulfide solid electrolyte film-5

[0096] The preparation method of sulfide solid electrolyte film-5 comprises the following steps:

[0097] S1: In a glove box filled with argon, 1.46 g of Li6PS5Cl sulfide, 0.1 g of LiTFSI, 0.04 g of 18-crown ether-6 and 4 mg of azobisisobutyronitrile were weighed into a beaker and mixed to obtain a mixture;

[0098] S2: Add 0.3 mmol of polyethylene glycol diacrylate (PEGDA) and 0.28 mmol of polyethylene glycol methacrylate (PEGMA) to the mixture of step S1, and stir magnetically for 24 h at a magnetic stirring speed of 600 rpm to obtain an electrolyte slurry;

[0099] S3: placing the electrolyte slurry obtained in step S2 on a smooth polytetrafluoroethylene plate and coating it with a 200 μm coating surface in a four-sided coater;

[0100] S4: After the polytetrafluoroethylene plate coated with the electrolyte slurry in S3 was placed in a vacuum oven at 70°C for in-situ curing for 12 hours, the prepared sulfide solid electrolyte film was peeled off from the polytetrafluoroethylene plate. The thickness of the obtained sulfide solid electrolyte film was 180 μm.

[0101] S5: The sulfide solid electrolyte film prepared in S4 is placed on a roller mill for roller thinning treatment. The roller speed of the roller mill is 1.5 m / min, and the roller temperature is 50°C. The thickness of the sulfide solid electrolyte film after rolling is about 110 μm. Subsequently, a steel sheet | sulfide solid electrolyte film | steel sheet battery is assembled for testing.

[0102] Example 6: Preparation of sulfide solid electrolyte film-6

[0103] The preparation method of sulfide solid electrolyte film-6 comprises the following steps:

[0104] S1: In a glove box filled with argon, weigh 1.46 g of Li 5.6 PS 4.6 Cl 1.4 Sulfide, 0.1 g of LiTFSI, 0.04 g of 18-crown ether-6 and 4 mg of azobisisobutyronitrile were mixed in a beaker to obtain a mixture;

[0105] S2: Add 0.3 mmol of polyethylene glycol diacrylate (PEGDA) and 0.28 mmol of polyethylene glycol methacrylate (PEGMA) to the mixture of step S1, and stir magnetically for 24 h at a magnetic stirring speed of 600 rpm to obtain an electrolyte slurry;

[0106] S3: placing the electrolyte slurry obtained in step S2 on a smooth polytetrafluoroethylene plate and coating it with a 200 μm coating surface in a four-sided coater;

[0107] S4: After the polytetrafluoroethylene plate coated with the electrolyte slurry in S3 was placed in a vacuum oven at 70°C for in-situ curing for 12 hours, the prepared sulfide solid electrolyte film was peeled off from the polytetrafluoroethylene plate. The thickness of the obtained sulfide solid electrolyte film was 180 μm.

[0108] S5: The sulfide solid electrolyte film prepared in S4 is placed on a roller mill for roller thinning treatment. The roller speed of the roller mill is 1.5 m / min, and the roller temperature is 50°C. The thickness of the sulfide solid electrolyte film after rolling is about 120 μm. Subsequently, a steel sheet | sulfide solid electrolyte film | steel sheet battery is assembled for testing.

[0109] Example 7: Preparation of sulfide solid electrolyte film-7

[0110] The preparation method of sulfide solid electrolyte film-7 comprises the following steps:

[0111] S1: In a glove box filled with argon, weigh 1.46 g of Li 5.2 PS 4.2 Cl 0.8 Br 0.8 Sulfide, 0.1 g of LiTFSI, 0.04 g of 18-crown ether-6 and 4 mg of azobisisobutyronitrile were mixed in a beaker to obtain a mixture;

[0112] S2: Add 0.3 mmol of polyethylene glycol diacrylate (PEGDA) and 0.28 mmol of polyethylene glycol methacrylate (PEGMA) to the mixture of step S1, and stir magnetically for 24 h at a magnetic stirring speed of 600 rpm to obtain an electrolyte slurry;

[0113] S3: placing the electrolyte slurry obtained in step S2 on a smooth polytetrafluoroethylene plate and coating it with a 200 μm coating surface in a four-sided coater;

[0114] S4: After the polytetrafluoroethylene plate coated with the electrolyte slurry in S3 was placed in a vacuum oven at 70°C for in-situ curing for 12 hours, the prepared sulfide solid electrolyte film was peeled off from the polytetrafluoroethylene plate. The thickness of the obtained sulfide solid electrolyte film was 180 μm.

[0115] S5: The sulfide solid electrolyte film prepared in S4 is placed on a roller mill for roller thinning treatment. The roller speed of the roller mill is 1.5 m / min, and the roller temperature is 50°C. The thickness of the sulfide solid electrolyte film after rolling is about 120 μm. Subsequently, a steel sheet | sulfide solid electrolyte film | steel sheet battery is assembled for testing.

[0116] Example 8: Preparation of sulfide solid electrolyte film-8

[0117] The preparation method of sulfide solid electrolyte film-8 comprises the following steps:

[0118] S1: In a glove box filled with argon, weigh 1.46 g of Li 10 GeP2S 12 Sulfide, 0.1 g of LiTFSI, 0.04 g of 18-crown ether-6 and 4 mg of azobisisobutyronitrile were mixed in a beaker to obtain a mixture;

[0119] S2: Add 0.3 mmol of polyethylene glycol diacrylate (PEGDA) and 0.28 mmol of polyethylene glycol methacrylate (PEGMA) to the mixture of step S1, and stir magnetically for 24 h at a magnetic stirring speed of 600 rpm to obtain an electrolyte slurry;

[0120] S3: placing the electrolyte slurry obtained in step S2 on a smooth polytetrafluoroethylene plate and coating it with a 200 μm coating surface in a four-sided coater;

[0121] S4: After the polytetrafluoroethylene plate coated with the electrolyte slurry in S3 was placed in a vacuum oven at 70°C for in-situ curing for 12 hours, the prepared sulfide solid electrolyte film was peeled off from the polytetrafluoroethylene plate. The thickness of the obtained sulfide solid electrolyte film was 180 μm.

[0122] S5: The sulfide solid electrolyte film prepared in S4 is placed on a roller mill for roller thinning treatment. The roller speed of the roller mill is 1.5 m / min, and the roller temperature is 50°C. The thickness of the sulfide solid electrolyte film after rolling is about 130 μm. Then, a steel sheet | sulfide solid electrolyte film | steel sheet battery is assembled for testing.

[0123] Comparative Example

[0124] The method of preparing a sulfide solid electrolyte using a non-lithium conductive binder polyvinylidene fluoride comprises the following steps:

[0125] S1: In a glove box filled with argon, 1.46 g of Li3PS4 sulfide electrolyte and 0.4 g of polyvinylidene fluoride (PVDF, molecular weight Mn≈400000) were weighed into a beaker and mixed to obtain a mixture;

[0126] S2: Add 2 mL of tetrahydrofuran to the mixture of step S1 and stir magnetically for 24 h at a magnetic stirring speed of 600 rpm to obtain an electrolyte slurry;

[0127] S3: placing the electrolyte slurry obtained in step S2 on a smooth polytetrafluoroethylene plate and coating it with a 200 μm coating surface in a four-sided coater;

[0128] S4: After the polytetrafluoroethylene plate coated with the electrolyte slurry in S3 was placed in a vacuum oven at 70°C for in-situ curing for 12 hours, the prepared sulfide solid electrolyte film was peeled off from the polytetrafluoroethylene plate. The thickness of the obtained sulfide solid electrolyte film was 150 μm.

[0129] S5: The sulfide solid electrolyte film prepared in S4 is placed on a roller mill for roller thinning treatment. The roller speed of the roller mill is 1.5 m / min, and the roller temperature is 50°C. The thickness of the sulfide solid electrolyte film after rolling is about 110 μm. Subsequently, a steel sheet | sulfide solid electrolyte film | steel sheet battery is assembled for testing.

[0130] The relevant properties of Examples 1-8 and the comparative example were tested, and the results are shown in Table 1 (ionic conductivity in Table 1 = (ionic conductivity of sulfide solid electrolyte thin film - ionic conductivity of sulfide) / ionic conductivity of sulfide * 100%).

[0131] Table 1

[0132]

[0133]

[0134] Figure 4 It is the Arrhenius fitting diagram (Arrhenius linear fitting diagram) of the ionic conductivity of the sulfide solid electrolyte film of the comparative example and embodiment 1-2; Figure 5 It is the Arrhenius fitting diagram of the ionic conductivity of the sulfide solid electrolyte film of Example 3-8.

[0135] From Table 1 and Figure 4-5 By comparing the test results of the comparative example with those of Examples 1-2, it can be seen that the room temperature ionic conductivity of the in-situ cured sulfide solid electrolyte film prepared by the present invention in the EIS test is higher than the ionic conductivity of the sulfide solid electrolyte film prepared by using the traditional non-lithium conductive binder, indicating that the sulfide solid electrolyte film prepared by the present invention has a stronger ability to conduct lithium ions in the battery.

[0136] It can be seen from the comparative example in Table 1 that the room temperature ionic conductivity change rate of the sulfide decreased by 26.3% before and after being compounded with the PVDF binder. This is because PVDF itself does not have the lithium conductivity function, and the solvent tetrahydrofuran in the preparation process destroys the less stable PS chemical bonds in the sulfide, thereby changing the structure of the sulfide and reducing the ionic conductivity of the electrolyte film.

[0137] It can be seen from Examples 1-2 in Table 1 that the room temperature ionic conductivity of Examples 1-2 is higher than the ionic conductivity of the sulfide itself. This is mainly due to the fact that the lithium-conducting compound 18-crown ether-6 and the introduced polymer have lithium-conducting ether bonds (-COC-) and ester groups (-OC=O), and the improvement in the ionic conductivity of Example 2 is higher than that of Example 1. This is because, relative to Example 1, Example 2 has repeated lithium-conducting ether oxygen units (-COC-) in its polymer structure, which makes its ionic conductivity even better.

[0138] In summary, the sulfide solid electrolyte film of the present invention has a stronger ability to conduct lithium ions and a higher ion conductivity than the traditional sulfide solid electrolyte using a non-lithium-conductive binder, and is therefore of great significance for improving the battery performance of solid-state batteries.

[0139] The above embodiments only provide partial technical solutions of the present invention. Within the protection scope of the present invention, by changing the types or amounts of sulfide, lithium-conducting polymer precursor, lithium salt, crown ether compound, and initiator, the prepared sulfide solid electrolyte film has similar effects to those of the above embodiments.

Claims

1. A sulfide solid electrolyte film, It is characterized in that Its raw material components include sulfide, lithium-conducting polymer precursor, lithium salt, crown ether compound, and initiator; The lithium-conducting polymer precursor is a combination of trimethylolpropane trimethacrylate and butyl acrylate or a combination of polyethylene glycol diacrylate and polyethylene glycol methacrylate; The sulfide is Li 3 PS 4 , Li 7 P 3 S 11 , Li 5.6 PS 4.6 Cl 1.4 , Li 10 G 2 S 14 Any of .

2. The sulfide solid electrolyte film according to claim 1, It is characterized in that The lithium salt is selected from LiClO 4 、LiPF 6 , LiBF 4 , lithium bis(trifluoromethanesulfonyl imide), lithium bis(fluorosulfonyl imide) salt, lithium bis(oxalatoborate) and LiPO 2 F 2 At least one of .

3. The sulfide solid electrolyte film according to claim 1, It is characterized in that The crown ether compound is selected from at least one of 12-crown-4, 15-crown-5, 18-crown-6, benzo-18-crown-6 and dibenzo-18-crown-6.

4. The sulfide solid electrolyte film according to claim 1, It is characterized in that The initiator includes a thermal initiator and / or a photoinitiator.

5. The sulfide solid electrolyte film according to any one of claims 1 to 2, It is characterized in that The sulfide accounts for 55-93.5% of the mass of the sulfide solid electrolyte film; and / or, the lithium-conducting polymer precursor accounts for 3-30% of the mass of the sulfide solid electrolyte film; and / or, the lithium salt accounts for 3-12% of the mass of the sulfide solid electrolyte film; and / or, the crown ether compound accounts for 0.5-4% of the mass of the sulfide solid electrolyte film; and / or, the initiator accounts for 0.1-1.5% of the mass of the lithium-conducting polymer precursor.

6. The method for preparing the sulfide solid electrolyte film according to any one of claims 1 to 5, It is characterized in that The following steps are involved: mixing the components to obtain a mixture; The mixture is coated on a substrate for curing, drying and pressing to obtain the sulfide solid electrolyte film.

7. The preparation method according to claim 6, It is characterized in that The curing conditions are a thermal curing temperature of 65-75°C or a curing wavelength of 365-385nm; and / or, the pressing is roller pressing, using a roller press for pressing, the rolling speed of the roller press is 0.5-10m / min, and the roller temperature is 40°C-55°C.

8. A battery, It is characterized in that It comprises the sulfide solid electrolyte film according to any one of claims 1 to 5.