A shockproof thermoplastic elastomer material and its preparation method and application
Through the multi-step polymerization reaction of -2-hydroxyethyl methacrylate with olefins and trimethoxyboron oxygen hexanes, an anti-shock thermoplastic elastomer material with long-chain network structure and B-O cross-linking bond is formed, and the existing materials are solved Inadequate shock absorption and shock resistance performance have achieved high toughness and good energy absorption and shock absorption effects.
Patent Information
- Application Number
- CN202410218247.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-02-27
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2044-02-27
AI Technical Summary
Existing thermoplastic elastomer materials have shortcomings in shock absorption and shock resistance, especially the long vulcanization cycle and difficult forming of rubber materials. The mechanical properties of polyurethane materials are average after adding damping fillers, which cannot meet the industry's demand for high-performance shock absorption materials. .
Through the multi-step polymerization reaction of materials such as 2-hydroxyethyl methacrylate, olefins and trimethoxyboron oxygen hexane, a shock-proof thermoplastic elastomer material with long-chain network structure and B-O dynamic crosslinking bonds, the material is realized High toughness, good energy absorption and shock absorption and buffering performance.
It provides shock-proof thermoplastic elastomer materials with excellent mechanical properties, high elongation of break and low rebound. They can quickly harden and absorb energy during high-speed impact, have good self-healing and impact resistance, and are suitable for shock-absorbing materials.
Smart Images

Figure QLYQS_1 
Figure BDA0004717210970000021 
Figure BDA0004717210970000031
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of thermoplastic elastomer materials, and in particular to a shockproof thermoplastic elastomer material and a preparation method and application thereof. Background Art
[0002] Thermoplastic elastomers (TPE) have been widely used in aviation, navigation, automobiles, footwear, medical equipment, sporting goods and other fields. Commercially available TPE is mainly divided into six categories: styrene block copolymers (SBC), thermoplastic polyurethane (TPU), polyamide-based thermoplastic elastomers, polyester-based thermoplastic elastomers, rubber olefin blends and dynamically vulcanized polymer blends. Among them, the first four are composed of block copolymers, and the last two are mainly polymer blends.
[0003] Shock-absorbing materials are widely used in various fields, and different materials are suitable for different environments and occasions. Rubber is a common shock-absorbing material. Its superior shock-absorbing performance and aging resistance give it certain advantages. However, rubber has disadvantages such as long vulcanization cycle and difficult molding, which to a certain extent limit its large-scale use. The main material of shock-absorbing pads currently sold on the market is still rubber. Polyurethane materials also need to be added with damping fillers to meet the requirements, but adding fillers also brings many negative effects.
[0004] CN112457467A discloses a high damping thermoplastic polyurethane elastomer and a preparation method thereof, wherein the polyurethane elastomer comprises an A / B component, wherein the A component comprises a polyester diol, an antioxidant, a catalyst, and a light stabilizer, and the B component is an isocyanate, and a high damping thermoplastic polyurethane elastomer is obtained. The obtained elastomer has good damping performance, a simple production process, and strong controllability, but the product is a thermoplastic product and requires special process equipment for production, and cannot be used under normal or low temperature conditions.
[0005] CN114478972A high damping polyurethane elastomer for shock-absorbing pad and its preparation method, the polyurethane elastomer is made by mixing component A and component B; the raw materials of component A are as follows: polyether polyol A, polyether polyol B, vegetable oil polyol, plasticizer, anti-aging agent, catalyst; the raw materials of component B are as follows: polyether polyol C, isophorone diisocyanate, MDI, plasticizer; component B is a prepolymer with an isocyanate mass content of 15% to 22%. The present invention provides a high damping polyurethane elastomer for shock-absorbing pad, which has high damping. However, the polyurethane has more additives and general mechanical properties.
[0006] Therefore, it is necessary to further develop new thermoplastic elastomers that have excellent properties such as good elasticity, high strength, shock resistance and shock absorption to meet the development needs of industrial shock-absorbing and anti-vibration materials. Summary of the invention
[0007] The purpose of the present invention is to provide a shockproof thermoplastic elastomer material and a preparation method and application thereof. The thermoplastic elastomer has strong toughness, good tensile properties, low resilience, and good energy absorption, shock absorption and buffering properties.
[0008] The present invention achieves the purpose of the present invention through the following technical solutions:
[0009] The present invention provides a shockproof thermoplastic elastomer material, the structural formula of which is as follows:
[0010]
[0011] Wherein 1≤m≤50, 10≤n≤100, 1≤k≤50, m, n, k are all integers; and R1, R2, and R3 are each independently one of a phenyl atom, a methyl atom, and a hydrogen atom.
[0012] Exemplarily, the structure of the elastomer is:
[0013]
[0014] Wherein 1≤a≤50, 5≤b≤100, 1≤c≤50, 1≤d≤50, 5≤e≤100, 1≤f≤50, 1≤g≤50, 5≤h≤100, 1≤i≤50, a, b, c, d, e, f, g, h, i are all integers; and R1, R2, and R3 are each independently one of a phenyl group, a methyl group, and a hydrogen atom.
[0015] The present invention also provides a method for preparing a shockproof thermoplastic elastomer material, comprising the following steps:
[0016] (1) adding 2-hydroxyethyl methacrylate, olefin, and initiator into a reaction vessel, using isopropanol as solvent, and stirring at a constant speed at 50-70° C. to obtain prepolymer 1;
[0017] (2) adding 2 / 3 of the prepolymer 1 obtained in step (1) and trimethoxyboroxane to a reaction vessel, adding a catalyst, and stirring at a constant speed at 70-85° C. to obtain prepolymer 2;
[0018] (3) adding the remaining 1 / 3 of the prepolymer 1 and the initiator to the prepolymer 2 obtained in step (2), stirring at a constant speed at 50-70° C. for a period of time to obtain a polymer;
[0019] (4) The unreacted monomers in the polymer obtained in step (3) are eluted with an ethanol solvent to obtain an elastomer.
[0020] Furthermore, in step (1), the mass ratio of 2-hydroxyethyl methacrylate to olefin is (1-5):(1-5).
[0021] Furthermore, in step (1), the olefin is at least one of styrene, ethylene and propylene.
[0022] Furthermore, in the step (2), the weight ratio of prepolymer 1 to trimethoxyboroxane is (10-50):(0.2-5).
[0023] Furthermore, the initiator in step (1) or step (3) is one of azobisisobutyronitrile, a benzil derivative and a dialkoxyacetophenone.
[0024] Furthermore, the amount of the initiator in step (1) or step (3) is 0.005-2 wt %.
[0025] The catalyst in step (2) is one of hydrochloric acid, sodium hydroxide and potassium hydroxide.
[0026] Furthermore, the amount of the catalyst used in step (2) is 0.001-1 wt%.
[0027] Furthermore, the reaction time of step (1) or step (2) or step (3) is 3-12 hours.
[0028] Preferably, the reaction time of step (1) is 3-5 hours.
[0029] Preferably, the reaction time of step (2) is 8-12 hours.
[0030] Preferably, the reaction time of step (3) is 5-8 hours.
[0031] Furthermore, the stirring speed in step (1) or step (2) or step (3) is 100-500 r / min.
[0032] The invention also provides a use of a shockproof thermoplastic elastomer material as a shock-absorbing and energy-absorbing protective material.
[0033] Beneficial effects of the present invention:
[0034] The present invention provides a shockproof thermoplastic elastomer material having excellent mechanical properties, high elongation at break and low rebound rate. The elastomer material provided by the present invention is obtained by multi-step polymerization reaction of 2-hydroxyethyl methacrylate, olefins and trimethoxyboroxyhexacyclopentane, and the boric acid decomposed by trimethoxyboroxyhexacyclopentane is connected in an extended chain manner to form a network structure with long chains, and the overall structure is stable, the soft and hard segments are evenly polymerized and distributed, and the material has good soft-hard conversion capability. The BO dynamic cross-linking bonds in the elastomer enable the elastomer material to harden rapidly and absorb energy when subjected to high-speed impact, and exert an energy absorption and shock-absorbing effect, and has good self-healing and impact resistance. The shockproof thermoplastic elastomer material provided by the present invention has good application prospects in shock-absorbing materials. DETAILED DESCRIPTION
[0035] The specific implementation methods of the technical solution of this specification are further described below through specific examples. These examples are for the purpose of describing the technical solution in detail, rather than for limiting the technical solution. Based on the examples in this specification, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of this specification.
[0036] The reagents used in the following examples of the present invention can be purchased from the market. Reagents or materials not specified are obtained through existing technologies.
[0037] As a preferred technical solution in the embodiment of the present invention, the structural formula of the shockproof thermoplastic elastomer material provided by the present invention is as follows:
[0038]
[0039] Example 1
[0040] This embodiment provides a method for preparing a shock-proof thermoplastic elastomer material, comprising the following steps:
[0041] (1) 50 parts of 2-hydroxyethyl methacrylate, 30 parts of styrene, and 0.5 parts of azobisisobutyronitrile were added to a reaction container, and isopropanol was used as a solvent. The mixture was stirred at a constant speed at 60° C. for 5 hours to obtain a prepolymer 1;
[0042] (2) adding 2 / 3 of the prepolymer 1 obtained in step (1) and 2 parts of trimethoxyboroxane to a reaction container, adding sodium hydroxide, and stirring at a constant speed to react at 80° C. to obtain prepolymer 2;
[0043] (3) adding the remaining 1 / 3 of the prepolymer 1 and azobisisobutyronitrile to the prepolymer 2 obtained in step (2), and stirring the mixture at a constant speed at 60° C. for 6 h to obtain a polymer;
[0044] (4) The unreacted monomers in the polymer obtained in step (3) are eluted with an ethanol solvent to obtain an elastomer.
[0045] Example 2
[0046] This embodiment provides a method for preparing a shock-proof thermoplastic elastomer material, comprising the following steps:
[0047] (1) 50 parts of 2-hydroxyethyl methacrylate, 20 parts of styrene, and 0.5 parts of azobisisobutyronitrile were added to a reaction container, and isopropanol was used as a solvent. The mixture was stirred at a constant speed at 65° C. for 5 hours to obtain a prepolymer 1;
[0048] (2) adding 2 / 3 of the prepolymer 1 obtained in step (1) and 1.5 parts of trimethoxyboroxane to a reaction container, adding sodium hydroxide, and stirring at a constant speed at 80° C. to react to obtain prepolymer 2;
[0049] (3) adding the remaining 1 / 3 of the prepolymer 1 and azobisisobutyronitrile to the prepolymer 2 obtained in step (2), and reacting at 65° C. with uniform stirring for 6 hours to obtain a polymer;
[0050] (4) The unreacted monomers in the polymer obtained in step (3) are eluted with an ethanol solvent to obtain an elastomer.
[0051] Example 3
[0052] This embodiment provides a method for preparing a shock-proof thermoplastic elastomer material, comprising the following steps:
[0053] (1) 50 parts of 2-hydroxyethyl methacrylate, 40 parts of styrene, and 0.7 parts of azobisisobutyronitrile were added to a reaction container, and isopropanol was used as a solvent. The mixture was stirred at a constant speed at 60° C. for 6 hours to obtain a prepolymer 1;
[0054] (2) adding 2 / 3 of the prepolymer 1 obtained in step (1) and 1 part of trimethoxyboroxane to a reaction container, adding sodium hydroxide, and stirring at a constant speed at 85° C. to react to obtain prepolymer 2;
[0055] (3) adding the remaining 1 / 3 of the prepolymer 1 and azobisisobutyronitrile to the prepolymer 2 obtained in step (2), and stirring the mixture at a constant speed at 60° C. for 6 h to obtain a polymer;
[0056] (4) The unreacted monomers in the polymer obtained in step (3) are eluted with an ethanol solvent to obtain an elastomer.
[0057] Example 4
[0058] This embodiment provides a method for preparing a shock-proof thermoplastic elastomer material, comprising the following steps:
[0059] (1) 50 parts of 2-hydroxyethyl methacrylate, 20 parts of ethylene, and 0.5 parts of azobisisobutyronitrile were added to a reaction container, and isopropanol was used as a solvent. The mixture was stirred at a constant speed at 65° C. for 5 hours to obtain a prepolymer 1;
[0060] (2) adding 2 / 3 of the prepolymer 1 obtained in step (1) and 1.5 parts of trimethoxyboroxane to a reaction container, adding sodium hydroxide, and stirring at a constant speed at 80° C. to react to obtain prepolymer 2;
[0061] (3) adding the remaining 1 / 3 of the prepolymer 1 and azobisisobutyronitrile to the prepolymer 2 obtained in step (2), and stirring the mixture at a constant speed at 65° C. for 5 h to obtain a polymer;
[0062] (4) The unreacted monomers in the polymer obtained in step (3) are eluted with an ethanol solvent to obtain an elastomer.
[0063] Example 5
[0064] This embodiment provides a method for preparing a shock-proof thermoplastic elastomer material, comprising the following steps:
[0065] (1) 50 parts of 2-hydroxyethyl methacrylate, 30 parts of ethylene, and 0.5 parts of azobisisobutyronitrile were added to a reaction container, and isopropanol was used as a solvent. The mixture was stirred at a constant speed at 60° C. for 5 hours to obtain a prepolymer 1;
[0066] (2) adding 2 / 3 of the prepolymer 1 obtained in step (1) and 0.8 parts of trimethoxyboroxane to a reaction container, adding sodium hydroxide, and stirring at a constant speed at 75° C. to obtain prepolymer 2;
[0067] (3) adding the remaining 1 / 3 of the prepolymer 1 and azobisisobutyronitrile to the prepolymer 2 obtained in step (2), and stirring the mixture at a constant speed at 60° C. for 6 h to obtain a polymer;
[0068] (4) The unreacted monomers in the polymer obtained in step (3) are eluted with an ethanol solvent to obtain an elastomer.
[0069] Example 6
[0070] This embodiment provides a method for preparing a shock-proof thermoplastic elastomer material, comprising the following steps:
[0071] (1) 50 parts of 2-hydroxyethyl methacrylate, 40 parts of ethylene, and 0.5 parts of azobisisobutyronitrile were added to a reaction container, and isopropanol was used as a solvent. The mixture was stirred at a constant speed at 60° C. for 5 hours to obtain a prepolymer 1;
[0072] (2) adding 2 / 3 of the prepolymer 1 obtained in step (1) and 2 parts of trimethoxyboroxane to a reaction container, adding sodium hydroxide, and stirring at a constant speed at 85° C. to obtain prepolymer 2;
[0073] (3) adding the remaining 1 / 3 of the prepolymer 1 and azobisisobutyronitrile to the prepolymer 2 obtained in step (2), and stirring the mixture at 60° C. for 7 h to obtain a polymer;
[0074] (4) The unreacted monomers in the polymer obtained in step (3) are eluted with an ethanol solvent to obtain an elastomer.
[0075] Comparative Example 1
[0076] This comparative example provides a method for preparing an elastomer, comprising the following steps:
[0077] (1) 50 parts of 2-hydroxyethyl methacrylate, 30 parts of styrene, and 0.5 parts of azobisisobutyronitrile were added to a reaction container, and isopropanol was used as a solvent. The mixture was stirred at a constant speed at 60° C. for 5 hours to obtain a prepolymer 1;
[0078] (2) The unreacted monomers in the polymer obtained in step (1) are eluted with an ethanol solvent to obtain an elastomer.
[0079] Comparative Example 2
[0080] This comparative example provides a method for preparing an elastomer, comprising the following steps:
[0081] (1) 50 parts of 2-hydroxyethyl methacrylate, 30 parts of styrene, and 0.5 parts of azobisisobutyronitrile were added to a reaction container, and isopropanol was used as a solvent. The mixture was stirred at a constant speed at 60° C. for 5 hours to obtain a prepolymer 1;
[0082] (2) adding the prepolymer 1 obtained in step (1) and 0.2 parts of trimethoxyboroxane to a reaction container, adding sodium hydroxide, and stirring at a constant speed at 80° C. to react to obtain a polymer;
[0083] (3) The unreacted monomers in the polymer obtained in step (2) are eluted with an ethanol solvent to obtain an elastomer.
[0084] Performance Test:
[0085] The elastomers prepared in Examples 1-6 and Comparative Examples 1-2 were extruded and tested for performance.
[0086] 1. Tensile properties: Refer to GB / T 1040.1-2018 Determination of tensile properties of plastics. Test the sample at a speed of 50 mm / min. Test at least 5 specimens and take the average value of the results.
[0087] 2. Tensile resilience: Refer to JIS K6255-1996 standard to test the tensile resilience of the sample. Test at least 5 specimens and take the average value of the results.
[0088] The performance test results of the shockproof thermoplastic elastomers prepared in Examples 1-6 and the elastomers prepared in Comparative Examples 1-2 are shown in Table 1.
[0089] Table 1 Performance test results
[0090] sample Tensile strength(MPa) Elongation at break (%) Resilience(%) Example 1 12.0 985 12 Example 2 10.1 1140 8 Example 3 11.8 1005 10 Example 4 11.2 1065 9 Example 5 10.7 1250 6 Example 6 12.9 971 15 Comparative Example 1 8.3 674 25 Comparative Example 2 18.2 560 35
[0091] As can be seen from Table 1, the shockproof thermoplastic elastomer material provided by the present invention has better mechanical properties and low resilience, has shock absorption and energy absorption effects, and meets the requirements of elastomeric materials for damping and shock absorption. In the preparation of the elastomer in Comparative Example 1, trimethoxyboroxyhexacyclopentane was not added, and the prepared elastomer did not contain BO bonds, so the mechanical properties and the ability to alternate between soft and hard hardware became poor. In the preparation process of Comparative Example 2, because a lower content of trimethoxyboroxyhexacyclopentane was added, and the prepolymer 1 and trimethoxyboroxyhexacyclopentane reacted at one time, the BO bond structure formed by batch reaction was more dispersed and random, and the resilience of the elastomer was higher. It can be seen that the thermoplastic elastomer prepared by the preparation method provided by the present invention has more excellent mechanical properties and shock resistance.
[0092] Although the embodiments of the present description have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present description, the scope of which is defined by the appended claims and their equivalents.
Claims
1. A method for preparing a shockproof thermoplastic elastomer material, characterized in that: The following steps are involved: (1) adding 2-hydroxyethyl methacrylate, olefin and initiator to a reaction vessel, using isopropanol as solvent, and stirring at a constant speed at 50-70°C to obtain prepolymer 1; (2) adding 2 / 3 of prepolymer 1 obtained in step (1) and trimethoxyboroxane to a reaction vessel, adding a catalyst, and stirring at a constant speed at 70-85°C to obtain prepolymer 2; (3) adding the remaining 1 / 3 of prepolymer 1 and initiator to the prepolymer 2 obtained in step (2), and stirring at a constant speed at 50-70°C. ℃, stirring at a constant speed for a period of time to obtain a polymer; (4) eluting the unreacted monomer in the polymer obtained in step (3) with an ethanol solvent to obtain an elastomer; the olefin in step (1) is at least one of styrene, ethylene and propylene; the mass ratio of 2-hydroxyethyl methacrylate to olefin in step (1) is (1-5):(1-5); the weight ratio of prepolymer 1 to trimethoxyboroxane in step (2) is (10-50):(0.2-5); the initiator in step (1) or step (3) is one of azobisisobutyronitrile, benzyl derivatives and dialkoxyacetophenone; the amount of the initiator is 0.005-2 wt%; the catalyst in step (2) is one of hydrochloric acid, sodium hydroxide and potassium hydroxide; the amount of the catalyst is 0.001-1 wt%; the reaction time of step (1) or step (2) or step (3) is 3-12 h; the stirring speed in step (1) or step (2) or step (3) is 100-500 r / min; the structural formula of the shockproof thermoplastic elastomer material is as follows: , Wherein 1≤m≤50, 5≤n≤100, 1≤k≤50, m, n, k are all integers; and R1 is one of a phenyl group, a methyl group and a hydrogen atom.
Citation Information
Patent Citations
High-damping thermoplastic polyurethane elastomer and preparation method thereof
CN112457467A
High-damping polyurethane elastomer for shock pad and preparation method of high-damping polyurethane elastomer
CN114478972A
Energy-absorbing method based on hybrid cross-linked network dynamic polymer
CN108342037A
Preparation method of boron modified acrylic ester rubber material
CN108727759A
Resin, blade for wind power generation, electronic component, motor coil and cable
JP2015214661A