A hydrogel polymer electrolyte and its preparation method and application
Through the preparation method of hydrogel polymer electrolyte, the problem of freezing of traditional solid electrolytes at low temperatures is solved, and the efficient work of zinc air batteries in extremely cold environments is achieved, which demonstrates excellent low-temperature cycling performance and simple preparation process.
Patent Information
- Application Number
- CN202410065586.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-01-17
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2044-01-17
AI Technical Summary
Traditional solid electrolytes are prone to freeze under low temperature conditions, resulting in a degradation in zinc air battery performance and unable to work normally in extreme cold environments.
Using the preparation method of hydrogel polymer electrolyte, polymerization of alkaline acrylic acid, acrylamide or polyvinyl alcohol with metal salts and initiators under the action of crosslinking agents to form hydrogel polymer electrolytes and swelling method Prepared for assembly of zinc air batteries.
The hydrogel polymer electrolyte can remain soft at -40°C, ensuring battery performance, and the cycle time exceeds 483 hours, showing superior low-temperature cycle performance, and the preparation method is simple and low-cost.
Smart Images

Figure CN118027286B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a hydrogel polymer electrolyte and a preparation method and application thereof, belonging to the technical field of zinc-air batteries and preparation thereof. Background Art
[0002] Solid-state batteries designed for flexible electronic devices have attracted much attention due to their significant advantages in portability and safety. At the same time, there is a growing demand for high-energy-density secondary batteries that can operate under harsh conditions. It is worth noting that high-latitude, high-altitude and extremely cold climate regions have an urgent need for batteries that can withstand low temperatures. Zinc-air batteries have attracted much attention because their energy density is significantly better than that of traditional metal-ion batteries and they are positioned as the next-generation solution for energy conversion and storage. The main functions of low-temperature-resistant hydrogels are: (1) they can maintain a soft gel state at extremely low temperatures to prevent the electrolyte from freezing and ensure that the battery can work normally; (2) they can ensure the transmission capacity of ions at low temperatures and maintain the performance of the battery. Therefore, hydrogel polymer electrolytes are expected to replace alkaline electrolytes in zinc-air batteries due to their excellent low-temperature resistance. Summary of the invention
[0003] In order to solve the problem that traditional solid electrolytes freeze under low temperature conditions, the present invention provides a hydrogel polymer electrolyte and a preparation method and application thereof.
[0004] The technical solution of the present invention:
[0005] One of the objects of the present invention is to provide a method for preparing a hydrogel polymer electrolyte, the method comprising the following steps:
[0006] (1) firstly mixing the alkaline solution A, the solution B and the metal salt solution, then sequentially adding an initiator and a cross-linking agent, stirring evenly and then heating for cross-linking to obtain a hydrogel polymer;
[0007] (2) placing the hydrogel polymer in an electrolyte solution and taking it out after adsorption saturation to obtain a hydrogel polymer electrolyte.
[0008] It is further defined that the preparation process of the alkaline A solution is: dissolving acrylic acid in deionized water, then adding a strong base, and stirring until the solution is clear and transparent to obtain the alkaline A solution.
[0009] In a further limitation, the strong base is sodium hydroxide or potassium hydroxide.
[0010] It is further defined that the molar ratio of acrylic acid to strong base is 1:(1-10).
[0011] It is further defined that the solute in solution B is acrylamide, ethylene oxide or polyvinyl alcohol.
[0012] It is further defined that the molar ratio of acrylic acid to the solute in solution B is 1:(1-10).
[0013] It is further defined that the molar ratio of acrylic acid to the solute in solution B is 1:(1-5).
[0014] It is further defined that the metal salt is a soluble lithium salt.
[0015] It is further defined that the metal salt is a soluble lithium salt that can exist stably in the air.
[0016] It is further defined that the molar ratio of the metal salt to the solute in solution B is 1:(2-50).
[0017] It is further defined that the molar ratio of the metal salt to the solute in solution B is 1:(1-5).
[0018] It is further defined that the molar ratio of the metal salt to the solute in solution B is 1:(2-5).
[0019] It is further defined that the initiator is potassium persulfate or ammonium persulfate.
[0020] It is further defined that the cross-linking agent is N,N'-methylenebisacrylamide.
[0021] It is further defined that the ratio of the amount of the crosslinking agent to the amount of the initiator substance is 1:(1-10).
[0022] It is further defined that the ratio of the amount of the crosslinking agent to the amount of the initiator substance is 1:(1-5).
[0023] It is further defined that the ratio of the amount of the crosslinking agent to the amount of the initiator substance is 1:(1-3).
[0024] It is further defined that the heating cross-linking temperature is 50 to 70° C. and the time is 2 to 14 hours.
[0025] It is further defined that the electrolyte solution is a mixed solution of potassium hydroxide and zinc acetate.
[0026] It is further defined that the concentration of potassium hydroxide is 1 to 12 mol / L, and the concentration of zinc acetate is 0.2 to 0.4 mol / L.
[0027] It is further defined that the hydrogel polymer is immersed in the electrolyte solution for 24 to 72 hours.
[0028] The second object of the present invention is to provide a hydrogel polymer electrolyte obtained by the above preparation method.
[0029] It is further defined that the hydrogel polymer electrolyte is used to prepare a zinc-air battery.
[0030] The third object of the present invention is to provide a zinc-air battery, which comprises the above-mentioned hydrogel polymer electrolyte, zinc sheet, Pt / C and RuO 2 The carbon cloth, pretreated zinc sheet and nickel foam are assembled in a 1:1 loading ratio.
[0031] Beneficial effects:
[0032] The present invention initiates a polymerization reaction of two polymer monomers, namely, alkalized acrylic acid and polymer monomer, with metal salt under the action of a crosslinking agent and an initiator at a certain temperature to obtain a hydrogel polymer, and then prepares a hydrogel polymer electrolyte by a swelling method. The hydrogel polymer electrolyte is used to assemble a zinc-air battery and exhibits excellent low-temperature cycle performance. Test results show that at a low temperature of -40°C, it can circulate for more than 483 hours. In addition, the preparation method of the hydrogel polymer electrolyte provided by the present invention also has the advantages of being fast, effective, simple, and low-cost. BRIEF DESCRIPTION OF THE DRAWINGS
[0033] Figure 1 The solid electrolyte assembled battery prepared in Example 1 was heated at -40°C, 1 mA cm -2 The long cycle diagram below;
[0034] Figure 2 The solid electrolyte assembled battery prepared in Comparative Example 1 was heated to -40°C and 1 mA cm -2 The long cycle diagram below;
[0035] Figure 3 This is a physical picture of the open circuit voltage of the solid electrolyte assembled battery prepared in Example 1 at room temperature;
[0036] Figure 4 This is a physical picture of the open circuit voltage of the solid electrolyte assembled battery prepared in Comparative Example 1 at room temperature. DETAILED DESCRIPTION
[0037] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, the specific implementation methods of the present invention are described in detail below in conjunction with the embodiments of the specification.
[0038] In the following description, many specific details are set forth to facilitate a full understanding of the present invention, but the present invention may also be implemented in other ways different from those described herein, and those skilled in the art may make similar generalizations without violating the connotation of the present invention. Therefore, the present invention is not limited to the specific embodiments disclosed below.
[0039] Secondly, the term "one embodiment" or "embodiment" as used herein refers to a specific feature, structure, or characteristic that may be included in at least one implementation of the present invention. The term "in one embodiment" that appears in different places in this specification does not necessarily refer to the same embodiment, nor does it refer to a separate or selective embodiment that is mutually exclusive with other embodiments.
[0040] The experimental methods used in the following examples are conventional methods unless otherwise specified. The materials, reagents, methods and instruments used are conventional materials, reagents, methods and instruments in the art unless otherwise specified, and can be obtained through commercial channels by those skilled in the art.
[0041] Embodiment 1:
[0042] Step 1: Dissolve 0.1 mol of acrylic acid monomer in 14 mL of deionized water, then add 0.1 mol of potassium hydroxide and stir until the solution is clear and transparent to obtain an alkaline monomer solution.
[0043] Step 2: Dissolve 0.25 mol of acrylamide monomer in 7 mL of deionized water and stir until completely dissolved to obtain a monomer solution.
[0044] Step 3: Dissolve 0.01 mol lithium chloride in 7 mL deionized water and stir until completely dissolved to obtain a metal salt solution.
[0045] Step 4: Add the alkalized monomer solution obtained in step 1 and the metal salt solution obtained in step 3 to the monomer solution obtained in step 2 respectively, stir evenly, and obtain a mixed solution.
[0046] Step 5: Add 0.04 g of N,N'-methylenebisacrylamide and 0.1 g of ammonium persulfate to the mixed solution obtained in step 4, and stir evenly to obtain a quasi-gel solution.
[0047] Step 6: Pour the obtained quasi-gel solution into a rectangular parallelepiped mold and heat it at 60° C. for 2 hours to initiate a polymerization reaction to obtain a hydrogel polymer.
[0048] Step 7: Soak the obtained hydrogel polymer in a mixed strong alkaline solution of 3.3M potassium hydroxide and 0.3M zinc acetate for 48 hours to obtain a hydrogel polymer electrolyte.
[0049] The solid electrolyte prepared in this embodiment is used as the electrolyte, the zinc sheet is used as the negative electrode of the battery, and the Pt / C and RuO 2 The carbon cloth with a ratio of 1:1 was used as the positive electrode of the battery, and the nickel foam was used as the current collector. The zinc-air battery was assembled and the low-temperature charge and discharge cycle performance test was carried out. The results are as follows Figure 1 and 3 As shown, at -40°C and 1 mA cm -2When tested under current density conditions, the battery cycle time reached more than 483 hours, showing good cycle performance, and the open circuit voltage was 1.513V at room temperature.
[0050] Embodiment 2:
[0051] The difference between this embodiment and embodiment 1 is that no metal salt solution is added in step 4, and the other process steps and parameter settings are the same as those in embodiment 1. The specific operation process is as follows:
[0052] Step 1: Dissolve 0.1 mol of acrylic acid monomer in 14 mL of deionized water, then add 0.1 mol of potassium hydroxide and stir until the solution is clear and transparent to obtain an alkaline monomer solution.
[0053] Step 2: Dissolve 0.25 mol of acrylamide monomer in 7 mL of deionized water and stir until completely dissolved to obtain a monomer solution.
[0054] Step 3: Add the alkalized monomer solution obtained in step 1 to the monomer solution obtained in step 2, stir evenly, and obtain a mixed solution.
[0055] Step 4: Add 0.04 g of N,N'-methylenebisacrylamide and 0.1 g of ammonium persulfate to the mixed solution obtained in step 3, and stir evenly to obtain a quasi-gel solution.
[0056] Step 5: Pour the obtained quasi-gel solution into a rectangular parallelepiped mold and heat it at 60° C. for 2 hours to initiate a polymerization reaction to obtain a hydrogel polymer.
[0057] Step 6: Soak the obtained hydrogel polymer in a mixed strong alkaline solution of 3.3M potassium hydroxide and 0.3M zinc acetate for 48 hours to obtain a hydrogel polymer electrolyte.
[0058] The solid electrolyte prepared in this embodiment is used as the electrolyte, the zinc sheet is used as the negative electrode of the battery, and the Pt / C and RuO 2 The carbon cloth with a ratio of 1:1 was used as the positive electrode of the battery, and the nickel foam was used as the current collector. The zinc-air battery was assembled and the low-temperature charge and discharge cycle performance test was carried out. The results are as follows Figure 2 and 4 As shown, at -40°C and 1 mA cm -2 When tested under current density conditions, the battery cycle time reached more than 171 hours, showing good cycle performance, and the open circuit voltage was 1.345V at room temperature.
[0059] By comparing the cycle time of the zinc-air battery assembled in Example 1 and Comparative Example 1 at low temperature, it can be seen that the cycle time of the electrolyte with the addition of the metal salt solution is greatly improved compared with that without the addition of the metal salt solution. This is mainly due to the interaction between the anions and cations in the metal salt solution and the water molecules. After the hydrated ions are formed, the free water molecules are anchored to the gel polymer, which increases the content of bound water in the gel polymer, making it difficult for the gel polymer to lose water during the charge and discharge cycle; on the other hand, the ionic conductivity of the metal salt solution is higher than that of water, and the ion transport during the charge and discharge cycle is easier, which is beneficial to the kinetic process of the reaction; in addition, the saturated vapor pressure of the metal salt solution is lower than that of pure water, so the freezing point of the metal salt solution is also relatively low, which ensures that the hydrogel polymer electrolyte is not easy to freeze at low temperatures, ensuring the normal progress of the reaction.
[0060] Although the present invention has been disclosed as above in the preferred embodiment, it is not intended to limit the present invention. Anyone familiar with this technology can make various changes and modifications without departing from the spirit and scope of the present invention. Therefore, the scope of protection of the present invention should be based on the definition of the claims.
Claims
1. A method for preparing a hydrogel polymer electrolyte, characterized in that: include: (1) firstly mixing the alkaline solution A, the solution B and the metal salt solution, then sequentially adding an initiator and a cross-linking agent, stirring evenly and then heating for cross-linking to obtain a hydrogel polymer; The preparation process of the alkaline A solution is as follows: dissolving acrylic acid in deionized water, then adding a strong base, and stirring until the solution is clear and transparent to obtain the alkaline A solution; The solute in the B solution is acrylamide, ethylene oxide or polyvinyl alcohol; the molar ratio of acrylic acid to the solute in the B solution is 1:(1-10); The metal salt is a soluble lithium salt; the molar ratio of the metal salt to the solute in solution B is 1:(2-50); (2) placing the hydrogel polymer in an electrolyte solution and taking it out after adsorption saturation to obtain a hydrogel polymer electrolyte.
2. The preparation method according to claim 1, characterized in that: The molar ratio of acrylic acid to strong base is 1:(1-10).
3. The preparation method according to claim 1, characterized in that: The initiator is potassium persulfate or ammonium persulfate, the crosslinking agent is N,N'-methylenebisacrylamide, and the molar ratio of the crosslinking agent to the initiator is 1:(1-10).
4. The preparation method according to claim 1, characterized in that: The heating cross-linking temperature is 50-70°C and the time is 2-14h.
5. The preparation method according to claim 1, characterized in that: The electrolyte solution is a mixed solution of potassium hydroxide and zinc acetate, wherein the concentration of potassium hydroxide is 1-12 mol / L, and the concentration of zinc acetate is 0.2-0.4 mol / L; the immersion time is 24-72 hours.
6. A hydrogel polymer electrolyte prepared by the method according to any one of claims 1 to 5.
7. An application of the hydrogel polymer electrolyte according to claim 6, characterized in that: Used to prepare zinc-air batteries.