A low-density lightweight foamed TPE material and its preparation method and application

By optimizing the formula and preparation method of TPE materials, the problem of high density after foaming of TPE materials has been solved, and the high-performance application of low-density and lightweight foamed TPE materials has been realized. It is suitable for shoe materials and other fields and improves the comfort of the materials. and resilience.

CN118027534BActive Publication Date: 2024-10-01GUANGDONG HONGCHAO RUBBER & PLASTIC CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410204559.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-02-24
Publication Date
2024-10-01
Estimated Expiration
2044-02-24

AI Technical Summary

Technical Problem

The existing TPE material has a high density after foaming, which limits its further application in the field of shoe materials, especially in terms of improving elasticity and reducing weight. It is difficult to make major breakthroughs.

Method used

The formula adopts low-density lightweight foamed TPE materials, including styrene-butadiene thermoplastic elastomer, polystyrene, white oil, maleic anhydride-grafted styrene elastomer, nano-diatomaceous earth, montmorillonite, foaming agent, three Raw materials such as phenylphosphine oxide, zinc stearate and tartaric acid are used to optimize the foaming performance and mechanical properties through specific preparation methods and process parameters.

Benefits of technology

It significantly reduces the density of foamed TPE materials and improves its comfort and resilience. It is suitable for preparing high-performance shoe materials and also shows excellent performance in other fields such as pillow cores and sofa linings.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004712612660000061
    Figure BDA0004712612660000061
Patent Text Reader

Abstract

The present invention relates to the technical field of polymer materials, and specifically discloses a low-density, lightweight foamed TPE material, a preparation method and an application thereof. A low-density, lightweight foamed TPE material comprises butadiene-styrene thermoplastic elastomer, polystyrene, white oil, maleic anhydride grafted styrene elastomer, nano-diatomaceous earth, montmorillonite, a foaming agent, triphenylphosphine oxide, zinc stearate and tartaric acid. A preparation method of a low-density, lightweight foamed TPE material comprises the steps of mixing, banburying, injection molding and foaming, cooling and molding, etc., to obtain a low-density, lightweight foamed TPE material. The low-density, lightweight foamed TPE material provided in the present application effectively solves the problem of high density of TPE materials after foaming, realizes high performance and high-value applications of low-density, lightweight foamed TPE materials, and has broad market prospects.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of polymer materials, and in particular to a low-density lightweight foamed TPE material and a preparation method and application thereof. Background Art

[0002] Thermoplastic elastomer (TPE) is a polymer material between vulcanized rubber and thermoplastic plastics. Its molecular structure consists of two parts: "soft segment" and "hard segment". The "soft segment" is a soft linear long molecular chain, and the "hard segment" is a shorter rigid chain, which makes TPE material have certain elasticity, rigidity and heat resistance. Styrene-based thermoplastic elastomer is the most widely used thermoplastic elastomer at present, especially SBS, which accounts for more than 90% of the application.

[0003] With the development of the times, the existing TPE foaming materials can no longer meet the market demand, especially in the field of footwear. Comfortable, lightweight and elastic sole materials have become the mainstream direction of footwear development. However, although TPE materials have the advantages of easy processing and low cost, the foaming ratio of TPE materials is low and not high. After the foaming is completed, there is still a problem of high density, which directly leads to the difficulty of reducing the weight of footwear materials mainly based on TPE materials. It is difficult to make great breakthroughs in improving elasticity, which limits the further application of TPE materials in the field of footwear. Therefore, it is necessary to solve the problem of high density of TPE materials after foaming. Summary of the invention

[0004] In order to solve the problem of high density of TPE materials after foaming, the present application provides a low-density lightweight foamed TPE material and its preparation method and application. The present application provides a low-density lightweight foamed TPE material, which effectively solves the problem of high density of TPE materials after foaming, realizes high performance and high-value application of low-density lightweight foamed TPE materials, and has broad market prospects.

[0005] The low-density lightweight foamed TPE material provided in this application adopts the following technical solution:

[0006] A low-density light foamed TPE material comprises, based on the mass fraction of the low-density light foamed TPE material, 60-80 parts of styrene-butadiene thermoplastic elastomer, 10-20 parts of polystyrene, 25-30 parts of white oil, 6-8 parts of maleic anhydride grafted styrene elastomer, 7-10 parts of nano diatomaceous earth, 3-5 parts of montmorillonite, 1-2 parts of foaming agent, 0.2-0.4 parts of triphenylphosphine oxide, 0.1-0.2 parts of zinc stearate and 0.1-0.2 parts of tartaric acid.

[0007] In the above technical scheme, the present application adopts raw materials such as butadiene-styrene thermoplastic elastomer, polystyrene, white oil, maleic anhydride grafted styrene elastomer, etc., so that the foamed TPE material has good processing and molding properties and anti-slip properties; the present application further improves the strength of the foamed TPE material and reduces the cost of raw materials by introducing montmorillonite and nano-diatomaceous earth; the present application further improves the foaming performance of the foamed TPE material by adopting a specific foaming agent and three foaming aids, namely triphenylphosphine oxide, zinc stearate and tartaric acid, and significantly reduces the density of the foamed TPE material with the foaming agent, making the foaming process more uniform and the pores more delicate, while improving the two-phase interface adhesion between the rubber and montmorillonite and nano-diatomaceous earth, further improving the mechanical properties of the material and improving the support of the two inorganic fillers, montmorillonite and nano-diatomaceous earth, for the pores, so that the foamed TPE material has better comfort and higher resilience.

[0008] Preferably, the low-density lightweight foamed TPE material includes 65 to 70 parts of styrene-butadiene thermoplastic elastomer, 12 to 15 parts of polystyrene, 27 to 28 parts of white oil, 6 to 7 parts of maleic anhydride grafted styrene elastomer, 8 to 9 parts of nano-diatomaceous earth, 3.5 to 4 parts of montmorillonite, 1.2 to 1.6 parts of foaming agent, 0.25 to 0.27 parts of triphenylphosphine oxide, 0.18 to 0.2 parts of zinc stearate, and 0.13 to 0.14 parts of tartaric acid.

[0009] In the above technical scheme, the present application further optimizes the dosage range of each raw material of the low-density lightweight foamed TPE material, further improves the coordination between the raw materials, and obtains a foamed TPE material with better foaming performance and higher resilience.

[0010] Preferably, the mass ratio of triphenylphosphine oxide, zinc stearate and tartaric acid is 0.26:0.19:0.13.

[0011] In the above technical scheme, when the mass ratio of triphenylphosphine oxide, zinc stearate and tartaric acid is 0.26:0.19:0.13, the coordination effect between triphenylphosphine oxide, zinc stearate and tartaric acid is optimal, which can better cooperate with the foaming agent, significantly reduce the density of the foamed TPE material, and make the pores more delicate, while significantly improving the two-phase interface adhesion between the rubber and montmorillonite and nano-diatomaceous earth, further improving the mechanical properties of the material and improving the support of the two inorganic fillers of montmorillonite and nano-diatomaceous earth for the pores, so that the foamed TPE material has better comfort and higher resilience.

[0012] Preferably, the particle size of the nano-diatomaceous earth is 30 to 35 nm.

[0013] Preferably, the particle size of the montmorillonite is 10 to 20 mm.

[0014] In the above technical scheme, the present application limits the particle size of nano-diatomite to 30-35nm and the particle size of montmorillonite to 10-20mm. Nano-diatomite can control the size of pores during the foaming process, avoid excessive coarseness of pores after foaming, further improve the uniformity of foaming pores, and increase the strength of the foaming material. The addition of montmorillonite further balances the improvement of the strength and toughness of the foaming material, while also being able to appropriately reduce the thermal conductivity of the foaming material, ensuring the good thermal stability of the foaming material, making the foaming process more uniform, the pores more delicate, and further improving the resilience of the foamed TPE material.

[0015] In a second aspect, the present application provides a method for preparing a low-density lightweight foamed TPE material using the following technical solution: A method for preparing a low-density lightweight foamed TPE material comprises the following steps:

[0016] Step 1: premixing butadiene styrene thermoplastic elastomer and polystyrene at 100-120° C. for 8-10 minutes to obtain a premix;

[0017] Step 2: knead the blend, white oil, maleic anhydride grafted styrene elastomer, montmorillonite, and nano-diatomaceous earth at 110-120° C. for 5-7 minutes, then add the remaining raw materials in the formula, continue kneading for 1-2 minutes, and extrude and granulate to obtain a mixture;

[0018] Step 3: Injection mold the mixture for foaming and cool it to below 50°C to obtain a low-density, lightweight foamed TPE material.

[0019] In the above technical solution, the present application ensures the excellent performance of the low-density lightweight foamed TPE material by adopting a specific preparation method. The present application realizes the preparation of the low-density lightweight foamed TPE material by the above method. This material has the advantages of light weight, high elasticity, good anti-slip properties, etc., and is suitable for preparing products such as shoe materials.

[0020] Preferably, the injection molding temperature in step 3 is 170-180°C, the injection molding pressure is 55-60 MPa, and the injection molding rate is 0.57-0.58 g / cm 3 The cooling time is 50 to 70 seconds.

[0021] In the above technical solution, the present application ensures the uniformity of the foaming process and the performance of the foamed TPE material by optimizing the injection molding parameters. During the injection molding process, precise control of the injection molding temperature, injection molding pressure, injection molding rate and cooling time helps to form a uniform and delicate pore structure, further improving the comfort and resilience of the foamed TPE material.

[0022] In a third aspect, the present application provides an application of a low-density, lightweight foamed TPE material using the following technical solution: an application of a low-density, lightweight foamed TPE material, characterized in that it is used to prepare shoe materials.

[0023] In the above technical solution, the present application uses low-density lightweight foamed TPE materials to prepare shoe materials, making full use of the advantages of low-density lightweight foamed TPE materials, which can significantly improve the comfort and resilience of shoe materials and prepare shoe materials with excellent performance. Such shoe materials can meet consumers' needs for comfort, lightness, etc.

[0024] In addition, the present application also provides the application of low-density lightweight foamed TPE materials in other fields, such as pillow cores, sofa liners, etc. The application in these fields can also bring into play the advantages of high elasticity and light weight of low-density lightweight foamed TPE materials, further improving product performance and user experience.

[0025] In summary, the present application includes at least one of the following beneficial technical effects:

[0026] 1. This application uses specific foaming agents and foaming aids to make the foaming process more uniform and the pores more delicate, thereby improving the foaming performance of the foamed TPE material and enhancing the resilience of the foamed TPE material.

[0027] 2. This application improves the strength, uniformity and thermal stability of the foaming material by controlling the particle size of nano diatomaceous earth and montmorillonite.

[0028] 3. The low-density, lightweight foamed TPE material provided in this application is applied to the field of shoe materials, which can significantly improve the comfort, resilience and lightness of the product. DETAILED DESCRIPTION

[0029] In order to better illustrate the purpose, technical solutions and advantages of the present invention, the present invention will be further described below in conjunction with specific embodiments.

[0030] Example 1

[0031] A low-density light foamed TPE material comprises 60kg of styrene-butadiene thermoplastic elastomer, 20kg of polystyrene, 30kg of white oil, 6kg of maleic anhydride grafted styrene elastomer, 7kg of nano diatomaceous earth, 5kg of montmorillonite, 1kg of foaming agent, 0.4kg of triphenylphosphine oxide, 0.1kg of zinc stearate and 0.1kg of tartaric acid.

[0032] Among them, the styrene-butadiene thermoplastic elastomer is SBS4402 produced by Sinopec.

[0033] Among them, the polystyrene is Chimei GPPS PG-33.

[0034] Among them, white oil was purchased from Changzhou Jiaye Chemical Co., Ltd.

[0035] Among them, maleic anhydride grafted styrene elastomer was purchased from Dongguan Shenghao Plastic Raw Materials Co., Ltd., item number 5541254.

[0036] Among them, nano diatomaceous earth was purchased from Fuchen (Tianjin) Chemical Reagent Co., Ltd., with a particle size of 30 to 35 nm.

[0037] Among them, montmorillonite was purchased from Shanghai Yuanye Biotechnology Co., Ltd. with a particle size of 10 to 20 mm.

[0038] Wherein, the foaming agent is azodimethylamine (AC) foaming agent.

[0039] Among them, triphenylphosphine oxide was purchased from Sigma-Aldrich (Shanghai) Trading Co., Ltd. with the catalog number T84603.

[0040] Zinc stearate was purchased from Sigma-Aldrich (Shanghai) Trading Co., Ltd., item number 307564.

[0041] Among them, tartaric acid was purchased from Shanghai Yuanye Biotechnology Co., Ltd., product number S30452.

[0042] The method for preparing the low-density lightweight foamed TPE material comprises the following steps:

[0043] Step 1: Premix butadiene styrene thermoplastic elastomer and polystyrene at 100° C. for 10 minutes to obtain a premix.

[0044] Step 2: knead the blend, white oil, maleic anhydride grafted styrene elastomer, montmorillonite and nano-diatomaceous earth at 120° C. for 7 minutes, then add the remaining raw materials in the formula, continue kneading for 2 minutes, extrude and granulate to obtain a mixture.

[0045] Step 3: Injection molding the mixture for foaming, the injection temperature is 170℃, the injection pressure is 55MPa, and the injection rate is 0.58g / cm 3 , and then cooled to below 50°C within 50 seconds to obtain a low-density lightweight foamed TPE material.

[0046] Example 2

[0047] A low-density lightweight foamed TPE material, which is different from Example 1 in that it includes 80kg of styrene-butadiene thermoplastic elastomer, 10kg of polystyrene, 25kg of white oil, 8kg of maleic anhydride grafted styrene elastomer, 10kg of nano diatomaceous earth, 3kg of montmorillonite, 2kg of foaming agent, 0.2kg of triphenylphosphine oxide, 0.2kg of zinc stearate, and 0.2kg of tartaric acid.

[0048] The method for preparing the low-density lightweight foamed TPE material comprises the following steps:

[0049] Step 1: Premix butadiene styrene thermoplastic elastomer and polystyrene at 120° C. for 8 minutes to obtain a premix.

[0050] Step 2: knead the blend, white oil, maleic anhydride grafted styrene elastomer, montmorillonite and nano-diatomaceous earth at 120° C. for 5 minutes, then add the remaining raw materials in the formula, continue kneading for 1 minute, extrude and granulate to obtain a mixture.

[0051] Step 3: Injection molding the mixture for foaming, the injection temperature is 180℃, the injection pressure is 60MPa, and the injection rate is 0.57g / cm 3 , and then cooled to below 50°C within 70 seconds to obtain a low-density lightweight foamed TPE material.

[0052] Example 3

[0053] A low-density lightweight foamed TPE material, which is different from Example 1 in that it includes 65kg of styrene-butadiene thermoplastic elastomer, 15kg of polystyrene, 27kg of white oil, 7kg of maleic anhydride grafted styrene elastomer, 9kg of nano diatomaceous earth, 3.5kg of montmorillonite, 1.2kg of foaming agent, 0.27kg of triphenylphosphine oxide, 0.18kg of zinc stearate, and 0.13kg of tartaric acid.

[0054] The method for preparing the low-density lightweight foamed TPE material comprises the following steps:

[0055] Step 1: Premix butadiene styrene thermoplastic elastomer and polystyrene at 110° C. for 9 minutes to obtain a premix.

[0056] Step 2: knead the blend, white oil, maleic anhydride grafted styrene elastomer, montmorillonite and nano-diatomaceous earth at 115° C. for 6 minutes, then add the remaining raw materials in the formula, continue kneading for 1.5 minutes, extrude and granulate to obtain a mixture.

[0057] Step 3: Injection molding the mixture for foaming, the injection temperature is 175℃, the injection pressure is 58MPa, and the injection rate is 0.58g / cm 3 , and then cooled to below 50°C within 60 seconds to obtain a low-density lightweight foamed TPE material.

[0058] Example 4

[0059] A low-density lightweight foamed TPE material, which is different from Example 1 in that it includes 70kg of styrene-butadiene thermoplastic elastomer, 12kg of polystyrene, 28kg of white oil, 6kg of maleic anhydride grafted styrene elastomer, 8kg of nano diatomaceous earth, 4kg of montmorillonite, 1.6kg of foaming agent, 0.25kg of triphenylphosphine oxide, 0.2kg of zinc stearate, and 0.14kg of tartaric acid.

[0060] Example 5

[0061] A low-density lightweight foamed TPE material, which is different from Example 1 in that it includes 70kg of styrene-butadiene thermoplastic elastomer, 12kg of polystyrene, 28kg of white oil, 6kg of maleic anhydride grafted styrene elastomer, 8kg of nano diatomaceous earth, 4kg of montmorillonite, 1.6kg of foaming agent, 0.26kg of triphenylphosphine oxide, 0.19kg of zinc stearate, and 0.13kg of tartaric acid.

[0062] Example 6

[0063] A low-density, lightweight foamed TPE material, which is different from Example 1 in that the particle size of the nano-diatomaceous earth is 15-25 nm.

[0064] Example 7

[0065] A low-density, lightweight foamed TPE material, which is different from Example 1 in that the particle size of the montmorillonite is 25 to 30 mm.

[0066] Comparative Example 1

[0067] A foaming TPE material, which is different from Example 1 in that triphenylphosphine oxide is replaced by triphenyl methyl phosphate in equal amounts.

[0068] Comparative Example 2

[0069] A foaming TPE material, which is different from Example 1 in that zinc stearate is replaced by zinc oxide in equal amounts.

[0070] Comparative Example 3

[0071] A foaming TPE material, which is different from Example 1 in that tartaric acid is replaced by sebacic acid in equal amounts.

[0072] Performance Testing

[0073] Sample: the foamed TPE material of the above embodiments and comparative examples.

[0074] Apparent density: Tested in accordance with GB / T6343-2009, the apparent density of the sample is detected at 23°C.

[0075] Tensile properties: The tensile test was carried out using a universal testing machine in accordance with GB / T6344-2008, with a tensile rate of 500 mm / min.

[0076] Shore C hardness: tested in accordance with GB / T531-1999.

[0077] Rebound rate: tested in accordance with GB / T6670-2008.

[0078] Permanent compression set: Tested in accordance with GB / T6669-2001, using 7.1 Method A to detect the permanent compression set of the sample, with a compression of 75%.

[0079] The above test results are shown in Table 1.

[0080] Table 1:

[0081]

[0082] Combined with the analysis of Examples 1-7, Comparative Examples 1-3 and Table 1, the foamed TPE material prepared in the present application has good foaming performance, mechanical properties, resilience and resistance to permanent compression deformation.

[0083] Specifically combined with Example 1 and Comparative Examples 1-3, comparative examples 1-3 respectively replaced the three foaming aids of triphenylphosphine oxide, zinc stearate and tartaric acid, and Example 1 had better foaming performance, mechanical properties, resilience and permanent compression deformation. It can be seen that only the cooperation of the three foaming aids of triphenylphosphine oxide, zinc stearate and tartaric acid can further improve the foaming performance of the foaming TPE material, significantly reduce the density of the foaming TPE material, make the foaming process more uniform, and make the pores more delicate, so that the foaming TPE material has higher resilience and better resistance to permanent compression deformation.

[0084] Specifically combined with the analysis of Example 1 and Example 6-7, the particle size range of the nano-diatomite used in Example 6 is not 30-35nm, and the particle size range of the montmorillonite used in Example 7 is not 10-20mm, while Example 1 has good resilience and resistance to permanent compression deformation. It can be seen that only by limiting the particle size of nano-diatomite to 30-35nm and the particle size of montmorillonite to 10-20mm, can the nano-diatomite and montmorillonite better cooperate with each other, and better interact with other raw materials of the foaming TPE material, so that the foaming process is more uniform, the pores are more delicate, and the resilience and resistance to permanent compression deformation of the foaming TPE material are further improved.

[0085] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.

Claims

1. A low-density, lightweight foamed TPE material, characterized in that: The low-density lightweight foamed TPE material comprises 60-80 parts of styrene-butadiene thermoplastic elastomer, 10-20 parts of polystyrene, 25-30 parts of white oil, 6-8 parts of maleic anhydride grafted styrene elastomer, 7-10 parts of nano-diatomite, 3-5 parts of montmorillonite, 1-2 parts of azodimethylamine foaming agent, 0.2-0.4 parts of triphenylphosphine oxide, 0.1-0.2 parts of zinc stearate and 0.1-0.2 parts of tartaric acid, wherein the particle size of the nano-diatomite is 30-35 nm, and the particle size of the montmorillonite is 10-20 mm.

2. A low-density lightweight foamed TPE material according to claim 1, characterized in that: It includes 65-70 parts of styrene-butadiene thermoplastic elastomer, 12-15 parts of polystyrene, 27-28 parts of white oil, 6-7 parts of maleic anhydride grafted styrene elastomer, 8-9 parts of nano diatomaceous earth, 3.5-4 parts of montmorillonite, 1.2-1.6 parts of azodimethylamine foaming agent, 0.25-0.27 parts of triphenylphosphine oxide, 0.18-0.2 parts of zinc stearate and 0.13-0.14 parts of tartaric acid.

3. A low-density, lightweight foamed TPE material according to claim 1, characterized in that: The mass ratio of triphenylphosphine oxide, zinc stearate and tartaric acid is 0.26:0.19:0.

13.

4. A method for preparing a low-density, lightweight foamed TPE material as claimed in any one of claims 1 to 3, characterized in that: The following steps are involved: Step 1: premixing butadiene styrene thermoplastic elastomer and polystyrene at 100-120° C. for 8-10 minutes to obtain a premix; Step 2: knead the blend, white oil, maleic anhydride grafted styrene elastomer, montmorillonite, and nano-diatomaceous earth at 110-120° C. for 5-7 minutes, then add the remaining raw materials in the formula, continue kneading for 1-2 minutes, and extrude and granulate to obtain a mixture; Step 3: Injection mold the mixture for foaming and cool it to below 50°C to obtain a low-density, lightweight foamed TPE material.

5. The method for preparing a low-density lightweight foamed TPE material according to claim 4, characterized in that: The injection molding temperature in step 3 is 170-180°C, the injection molding pressure is 55-60MPa, and the injection molding rate is 0.57-0.58g / cm 3 , the cooling time is 50~70s.

6. An application of a low-density lightweight foamed TPE material as claimed in any one of claims 1 to 3, characterized in that: It is used to prepare shoe materials.