Preparation and application of a liquid porous material

Fe-Si porous liquid materials were prepared by co-precipitation, which solved the safety and flowability issues of porous materials in CO2 capture process, and achieved efficient and low-cost CO2 capture and conversion, which is suitable for industrial applications.

CN118059641BActive Publication Date: 2026-11-17FUZHOU UNIV
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202410368071.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-03-28
Publication Date
2026-11-17
Estimated Expiration
2044-03-28

AI Technical Summary

Technical Problem

Existing porous materials suffer from low safety, high cost, and poor flowability in CO2 capture and conversion processes, making them difficult to apply on an industrial scale.

Method used

Amorphous iron-silicon powder materials were prepared by co-precipitation and mixed with titanate coupling agent. Fe-Si porous liquid materials were prepared by controlling the reaction conditions. Combined with cyclohexane treatment, the solid materials were liquefied and CO2 was captured efficiently.

Benefits of technology

The prepared liquid iron-silicon material exhibits high stability, significantly improved CO2 capture capacity, and is suitable for large-scale industrial production. It is also low in cost and highly safe.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118059641B_ABST
    Figure CN118059641B_ABST
Patent Text Reader

Abstract

This invention discloses the preparation and application of a liquid porous material. The material is a porous liquid material comprising Fe-Si material and titanate coupling agent, exhibiting strong gas adsorption capacity and excellent adsorption performance in carbon dioxide capture. It can be used for the adsorption of single-component carbon dioxide and the selective separation of multi-component gases. This material achieves a solid-to-liquid phase transition. Compared to commonly used solid porous materials, such as zeolite molecular sieves and porous framework materials, this material has fluidity. Compared to commonly used pure liquid adsorbents, this material has a permanent pore structure, resulting in a higher gas adsorption capacity than pure liquid adsorbents. The advantages of this invention are its simple preparation process, low cost, combination of the porosity of solid materials and the fluidity of liquid materials, and higher gas adsorption capacity than traditional solid and liquid materials, making it highly economical and practical.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of gas adsorption technology in petrochemicals, and relates to a method for preparing a novel liquid porous material. Background Technology

[0002] In recent years, the rapid development of global industry has accelerated the consumption of fossil fuels, leading to excessive emissions of the greenhouse gas CO2. Therefore, environmental problems caused by carbon emissions are becoming increasingly serious, and reducing CO2 emissions is an urgent issue to be addressed. Carbon capture, utilization, and storage (CCUS) technology is one of the important solutions to mitigate CO2 emissions. This technology is a new process that captures CO2 from the gas mixture produced by the combustion of fossil fuels and stores or reuses it to prevent large amounts of CO2 from being released into the atmosphere. Globally, China is the largest emitter of CO2, therefore CCUS technology has received increasing attention in China and is considered an important technological option for achieving emission reduction targets.

[0003] To alleviate the energy shortage and global warming crisis, my country has formulated and implemented a series of practical energy conservation and emission reduction measures: First, improving the utilization rate of existing energy sources. my country's energy reserves are characterized by "abundant coal, limited oil, and scarce natural gas," which determines that my country's energy supply structure is dominated by coal, and this structural change is unlikely to occur for a considerable period of time. Due to limitations in my country's technological level, the production and consumption methods for coal are relatively backward, resulting in low utilization rates of coal resources and the emission of large amounts of CO2 into the atmosphere. Second, vigorously developing renewable energy sources. As is well known, my country has a vast territory and abundant natural energy resources, but due to its large population, the per capita resource availability is low. Therefore, it is necessary to vigorously develop renewable energy sources (such as solar energy, wind energy, ocean energy, and hydrogen energy) to optimize and upgrade the existing energy supply structure, thereby reducing CO2 emissions and addressing the energy crisis. Third, reducing the CO2 content in the atmosphere through CO2 capture and storage (CCS) technology, CO2 capture and utilization (CCU) technology, and the combined CO2 capture, utilization, and storage (CCUS) technology. CCS (Carbon Capture and Sequestration) technology refers to the capture and storage of CO2 before it enters the atmosphere. CCUS (Carbon Capture and Sequestration System) technology utilizes CO2 as an abundant and inexpensive carbon-oxygen source. Under appropriate conditions, CO2 can be selectively captured from existing emission sources and then fixed using renewable energy sources, converting it into useful fuels or higher-value-added chemicals (e.g., carbon olefins, cyclic carbonates, etc.). CCUS is a technology capable of capturing industrially produced CO2 on a large scale, preventing its direct emission into the atmosphere, and enabling the effective utilization of CO2. CCUS technology mainly includes CO2 capture, transportation, safe storage, and conversion or utilization. Therefore, these technologies are particularly important for CO2 emission reduction, addressing the greenhouse effect, and alleviating the energy crisis.

[0004] Currently, CO2 sequestration primarily involves transporting captured CO2 to designated locations via pipelines, tanker trucks, and ships for long-term storage, achieving long-term isolation of CO2 from the atmosphere. The main sequestration technologies include: ecological sequestration, which utilizes the photosynthesis of plants to absorb, fix, and transform CO2, thereby sequestering it; mineral sequestration, which uses metal oxides in natural ores (such as olivine and serpentine) to react with CO2 through acidification to obtain stable carbonates, thus permanently solidifying CO2; and geological sequestration, which involves injecting the separated high-purity CO2 in gaseous or liquid phases into suitable geological structures such as saline aquifers, abandoned coalfields, and depleted oil and gas fields for permanent storage, which can also improve oil and gas recovery rates and coalbed methane recovery rates. In this type of storage process, CO2 dissolves in underground fluids and reacts chemically with minerals, ultimately fixing the CO2 through precipitation. Ocean storage, on the other hand, utilizes CO2's solubility in water and its high density to inject captured CO2 through pipelines into seawater at depths of 1000 meters or more, allowing it to dissolve naturally or forming solid CO2 at depths of 3000 meters or more. While CO2 storage methods are diverse, they harbor significant safety risks and could potentially cause catastrophic disasters at any time. If leaks occur at the storage site, or if natural disasters such as earthquakes occur, large amounts of CO2 will return to the atmosphere, potentially leading to dangers such as ocean acidification—a situation that is unpredictable. Therefore, it is imperative to accelerate the development of safer storage technologies or find better CO2 treatment technologies.

[0005] After a long period of development, CO2 capture, as the initial and most important stage of various emission reduction technologies, has been extensively studied by researchers. Meanwhile, the technology of converting captured CO2 into useful fuels or high-value-added chemicals is recognized as a very promising solution strategy due to its high safety and its contribution to the carbon cycle, and has been the subject of much scientific research. Currently, the main research direction focuses on improving the CO2 capture performance of materials and increasing their CO2 conversion efficiency while reducing capture costs.

[0006] CO2 capture is a technology for removing or separating CO2 from the exhaust gas of fossil fuel combustion. Based on the combustion method, capture process, and the amount of CO2 produced, it is further subdivided into three main categories: pre-combustion capture technology, oxy-fuel combustion technology, and post-combustion capture technology. To date, CO2 capture and separation methods mainly include solvent absorption, solid adsorption separation, and membrane separation. Since this patent primarily focuses on innovations in solid and liquid materials, it mainly introduces the commonly used industrial solvent absorption and solid adsorption separation methods; other methods will not be elaborated upon.

[0007] (1) Solvent absorption method Solvent absorption refers to the process where CO2 is absorbed by an absorbent solution when a mixed gas passes through it, thus separating CO2 from the mixed gas. Based on different absorption and separation principles, it is divided into two main categories: physical absorption and chemical absorption. Physical absorption involves dissolving CO2 in an absorbent solution that has good selectivity for CO2, high solubility, stable performance, and is non-corrosive. Physical absorption has many advantages, including low energy consumption for absorbent regeneration, small required absorbent dosage, and strong absorption capacity. However, it also suffers from poor CO2 absorption selectivity, high operating costs, and low absorbent recovery rates, making it only suitable for situations with high CO2 concentrations. Chemical absorption utilizes the neutralization reaction between CO2 and an alkaline absorbent solution, thereby absorbing and separating CO2 from the mixed gas. Alternatively, the rich solution can be heated to decompose it into CO2, ultimately successfully separating CO2 from the mixed gas. While this method has a high recovery rate, it suffers from high investment costs, high regeneration energy consumption, and severe equipment corrosion, making it suitable for situations with low or medium CO2 concentrations.

[0008] (2) Solid adsorption separation method Solid-state adsorption separation refers to the selective adsorption of CO2 from a gas mixture using a solid adsorbent. This adsorption must be reversible to effectively separate and capture CO2. The adsorption and desorption principles of solid-state adsorption separation are similar to those of physical absorption, both following Henry's Law. Generally, solid-state adsorption separation is divided into two main categories: physical adsorption and chemisorption.

[0009] Physical adsorption refers to the adsorption of CO2 onto the surface of a solid adsorbent through van der Waals forces, hence it is also called "van der Waals adsorption". Because the van der Waals forces between molecules are relatively weak, the binding force between CO2 and the solid adsorbent is weak. This is more conducive to the reversible adsorption and desorption of CO2 on the solid adsorbent, thus making it easier to regenerate the solid adsorbent. However, its adsorption capacity for CO2 is relatively low.

[0010] Chemisorption refers to the chemical reaction between CO2 and the surface of a solid adsorbent to form stable chemical bonds, thereby separating and capturing CO2. CO2 adsorbed onto the surface of a solid adsorbent via chemisorption is relatively stable. This process is generally irreversible, and the adsorption rate is relatively slow, but it exhibits high selectivity and adsorption capacity.

[0011] In summary, among numerous CO2 capture and separation methods, solid adsorption separation is considered the most promising due to the advantages of solid adsorbents, such as simple operation, recyclability, and low regeneration energy consumption. Porous materials, with their well-developed pore structure and high specific surface area, are widely used in many fields of human life and industrial production. Traditional porous materials include zeolite molecular sieves, porous framework materials, and covalent organic frameworks, which generally exist in solid form, possessing relatively stable cavity structures, high durability, and easy storage. However, their lack of fluidity makes them difficult to scale up for industrial production. Traditional liquid solvents have good fluidity, and liquid circulation systems are easier to integrate into existing industrial equipment, facilitating system recycling. However, they lack permanent pore structures. Therefore, designing and preparing novel porous liquid materials that combine the porosity of solid materials with the fluidity of liquid materials is of great significance and far-reaching impact on technological progress and the improvement of industrial production efficiency.

[0012] Several reports have been published regarding the preparation of porous liquids. CN114425181A discloses a method for preparing porous liquids, which involves reacting nano-silica with a eutectic solvent to obtain eutectic solvent-modified silica, and then reacting nonylphenol polyoxyethylene ether propyl sulfonate with the eutectic solvent-modified silica to obtain a porous liquid material. CN109745952A discloses another method for preparing porous liquids, in which the surface of MOFs material is modified with free radical polymerization initiating groups. The polysiloxane segments include a second connecting functional group that can be polymerized by the free radical polymerization initiating groups. The second connecting functional group and the free radical polymerization initiating groups form carbon-carbon covalent bonds through free radical polymerization. The polysiloxane segments are modified on the surface of the MOFs material by the free radical polymerization initiating groups. According to different needs, the pore structure of the MOFs material can be controlled to obtain the desired MOFs-based porous liquid. CN112934196A describes a hollow carbon sphere HCS porous liquid exhibiting flow behavior at room temperature. This liquid combines the characteristics of porous solids (such as zeolites and metal-organic frameworks, possessing permanent, rigid, and well-defined pores) and liquids (possessing fluidity, rapid heating, and mass transfer). Using hollow carbon spheres (HCS) as the core, polymeric ionic liquids (PILs) are modified onto their surface via electrostatic assistance. Then, through anion exchange, organic oligomers with opposite charges to the PILs (such as 4-nonylphenol-polyvinyl ether sulfonate potassium PEGS) are grafted onto the HCS surface to prepare the porous liquid, which exhibits a liquid state at room temperature. CN108905501A discloses a method for preparing porous liquid materials. This method uses iron(III) oxide (Fe3O4) as a hard template to prepare hollow SiO2 nanoparticles. Then, utilizing the electrostatic interaction between the hollow SiO2 nanoparticles and the polymeric ionic liquid, porous liquid intermediates (SiO2@PILs) are obtained. This method ensures the surface of the hollow SiO2 nanoparticles carries a positive charge while preventing the silica micropores from being sealed. Finally, sulfonated polyethylene glycol is used as the outer cap to form a stable porous liquid material (PLs). CN107140644A discloses a room-temperature fluid-behavior SiO2 porous liquid and its preparation method. Hollow SiO2 is prepared using a template method, employing co-precipitated iron(III) oxide as a template. Simultaneously, ethyl orthosilicate is hydrolyzed under the catalysis of ammonia water, depositing onto the iron(III) oxide template surface. Then, hydrochloric acid is used to remove the iron(III) oxide, forming a hollow structure. A porous liquid is formed by hydrolyzing siloxyethyl groups on the surface of porous nanoparticles and grafting them onto the hollow surface via covalent bonds to form a neck layer. Then, an organic oligomer with the opposite charge to the neck layer is selected as the crown layer.

[0013] The methods for preparing porous liquids listed above mainly involve grafting silica or MOF-based materials, followed by the addition of a flowable canopy through covalent or ionic bonds to liquefy the solid material. This mechanism is quite complex, and the grafted and canopy materials are typically expensive. Currently, there are no reports on the grafting and liquefaction of iron-based materials. Building upon previous work, this study combines iron oxide with a silica support to prepare amorphous iron-silicon materials with low density and small particle size. Utilizing the abundant hydroxyl groups on the surface of the silica material, the amorphous iron-silicon materials are grafted and liquefied. The resulting iron-silicon liquid material exhibits a significantly higher CO2 capture capacity than the solid porous material. Summary of the Invention

[0014] The purpose of this invention is to provide a novel method for preparing liquid materials to improve the CO2 capture capacity of solid porous materials.

[0015] A novel liquid material preparation method involves co-precipitation to obtain amorphous iron-silicon powder, which is then mixed with a titanate coupling agent. After heating and stirring for a certain time, cyclohexane is added. By controlling the type and amount of titanate coupling agent and changing the reaction temperature and time, Fe-Si porous liquid material is obtained. The preparation method includes the following steps: (1) Prepare an iron salt solution of a certain concentration and take a certain amount of ammonia water as the alkaline solution; (2) Add the iron salt solution and alkali solution obtained in step (1) dropwise into a beaker containing water while stirring and controlling the pH. (3) Stabilize the gel obtained in step (2) for 10-180 min, quickly add the silicon source, age for 20-150 min, dry at 100-200 ℃ for 12-24 h, and then heat it at 300-600 ℃. o Amorphous iron-silicon materials were obtained by calcining in air atmosphere at C for 2-12 h. (4) Add the titanate coupling agent and amorphous iron-silicon material into the sample bottle and pre-stir at room temperature for 10-60 min to form a suspension; (5) Stir the suspension obtained in step (4) at 30-80°C. o Stir thoroughly at temperature C for 0.5-12 hours; (6) Add cyclohexane to the solution obtained in step (5) at 30-90 °C. o The liquid porous material was obtained by stirring at C for several hours.

[0016] The concentration of the iron salt solution in step (1) is 0.5 mol / L-2 mol / L, and the mass fraction of ammonia water is 25%-28%.

[0017] The pH value of the suspension system formed in step (2) is maintained between 8 and 11.

[0018] The titanate coupling agent in step (4) is one of isopropyl tris(dioctyl pyrophosphoryl) titanate (KR-38S), isopropyl tris(dioctyl pyrophosphoryl) titanate (KR-12), and isopropyl tris(isostearoyl) titanate (KR-TTS); The mass ratio of the amorphous iron-silicon material to the titanate coupling agent in step (4) is 1:10-1:15; The hydrothermal temperature in step (5) is 30-80°C. o C, stirring time is 0.5-6 h.

[0019] The stirring temperature in step (6) is 60-90 ℃ and the reaction time is not less than 3 h.

[0020] The liquid porous material is an Fe-Si porous liquid material; the application of the Fe-Si porous liquid material in carbon dioxide capture: the Fe-Si porous liquid material is added as an adsorbent to a reaction vessel, and carbon dioxide at a certain pressure is added. The reaction conditions are: reaction temperature 20-40°C. o C, carbon dioxide pressure 0-2 MPa, adsorption time 1-12 h.

[0021] The present invention has the following advantages: 1) The liquid iron-silicon material prepared by the present invention liquefies solid powder through a simple process. After liquefaction, it is very stable and will not separate into layers over a long period of time.

[0022] 2) The liquid iron-silicon material prepared by this invention has a high carbon dioxide capture capacity. Compared with traditional porous solid materials, the carbon dioxide adsorption capacity of the liquid iron-silicon material prepared by this invention is increased by several times, and it has good utilization potential in carbon dioxide capture and conversion.

[0023] 3) The liquid iron-silicon material prepared by this invention uses a very green and simple material preparation process, and its raw materials are inexpensive, making it suitable for large-scale production and showing good application prospects in industry. Attached Figure Description

[0024] Figure 1 This is a sample image of the liquid iron-silicon material obtained in Example 1.

[0025] Figure 2 The image shows the XRD pattern of the iron-silicon material obtained in Example 1.

[0026] Figure 3 The Fourier transform infrared spectra of the liquid iron-silicon material, the iron-silicon material, and the titanate coupling agent KR-38S obtained in Example 1 are shown.

[0027] Figure 4This is a transmission electron microscope (TEM) image of the liquid iron-silicon material obtained in Example 1.

[0028] Figure 5 The graph shows the carbon dioxide adsorption curves of the liquid iron-silicon material and the iron-silicon powder solid obtained in Example 1.

[0029] Figure 6 The results show the CO2 gas adsorption of the silicon-based porous liquids in Examples 1, 2, and 3.

[0030] Figure 7 The porosity structure of the precursors corresponding to Comparative Example 1 and Comparative Examples 2-3 is shown. Detailed Implementation

[0031] To further understand the present invention, the following detailed description is provided with reference to the embodiments and the accompanying drawings to illustrate the liquid iron-silicon material of the present invention.

[0032] Comparative Example 1 25.25 g of ferric nitrate nonahydrate was dissolved in 50 g of water to obtain a Fe salt solution. 10 mL of 28 wt% ammonia solution was dissolved in 40 g of water to obtain an ammonia solution. The Fe salt solution and ammonia solution were added concurrently to 100 mL of deionized water. The mixture was stirred continuously at 60 °C until the pH reached 8.5, and then slowly titrated, with the acid-base neutralization reaction time controlled at 1.5–2.0 h. After the Fe salt solution titration was complete, the mixture was allowed to stabilize for 60 min. 8.77 g of 27.68% water glass was diluted with water to 20.32 g and rapidly added to the obtained sol within 5–10 min, maintaining the pH at 8.2–8.7, and aged for 20 min. The mixture was then filtered and washed until neutral, dried at 150 °C for 10 h, and calcined at 500 °C for 3 h to obtain an amorphous iron-silicon material with particles of 2–3 nm.

[0033] Example 1 The steps for preparing amorphous iron-silicon are the same as those for the comparative example.

[0034] 3 g of isopropyl tris(dioctylpyrophosphoryl)titanate (KR-38S) and 1 g of amorphous iron-silicon material were added to a sample vial and pre-stirred at room temperature for 1 h to form a suspension. The resulting suspension was then incubated at 80 °C. o Stir thoroughly at C for 1 h, add 3 g of cyclohexane, and heat at 80°C. o Liquid iron-silicon material was obtained by stirring at C for 3 hours. Sample attached. Figure 1 As shown.

[0035] Example 2 The steps for preparing amorphous iron-silicon are the same as those for the comparative example.

[0036] 3 g of isopropyl tris(dioctylphosphoyl)titanate (KR-12) and 1 g of amorphous iron-silicon material were added to a sample vial and pre-stirred at room temperature for 1 h to form a suspension. The resulting suspension was then incubated at 80 °C. o Stir thoroughly at C for 1 h, add 3 g of cyclohexane, and heat at 80°C. o Stirring at C for 3 h yields liquid iron-silicon material.

[0037] Comparative Example 2 Preparation of silica: A certain amount of hexadecyltrimethylammonium bromide (CTAB) was dissolved in deionized water to a concentration of 0.0056 mol / L. An appropriate amount of ethanol and sodium hydroxide with a final concentration of 2 mol / L were added. The volume ratio of ethanol to water was 1:9. The mixture was stirred vigorously at 60 °C until the solution became clear and transparent. 1.5 g of tetraethyl orthosilicate (TEOS) was quickly added while stirring to a concentration of 0.053 mol / L. The mixture was stirred vigorously for another 2 h. The reaction mixture was then filtered, washed three times with ethanol, vacuum dried at 60 °C for 12 h, and calcined at 550 °C for 5 h to obtain silica nanomaterials.

[0038] 0.75 g of silica and 3 g of isopropyltris(dioctylpyrophosphoryl)titanate (KR-38S) were added to a sample vial and pre-stirred at room temperature for 1 h to form a suspension. The resulting suspension was then incubated at 80 °C. o Stir thoroughly at C for 1 h, add 3 g of cyclohexane, and heat at 80°C. o Stirring at C for 3 h yielded a porous silica liquid.

[0039] Comparative Example 3 Al-Si material preparation: 50 mL of 0.1 mol / L aluminum nitrate solution and 10 mL of 28% ammonia solution were dissolved in 40 g of water to obtain an ammonia solution. This solution was then added dropwise to 100 mL of deionized water at 60 °C with continuous stirring to maintain the pH at 8.5. After aging the resulting suspension at 60 °C for 1 h, 9.44 g of water glass (containing 27.68 wt% SiO2) was added dropwise to the above solution with continuous stirring. The solution was then aged at 60 °C for another 1 h. The solid product was filtered, washed until neutral, dried at 120 °C for 12 h, and calcined at 550 °C for 4 h to obtain aluminum-silicon material with a particle size of 3-4 nm.

[0040] 1 g of Al-Si material and 3 g of isopropyl tris(dioctylpyrophosphoryl)titanate (KR-38S) were added to a sample vial and pre-stirred at room temperature for 1 h to form a suspension. The resulting suspension was then incubated at 80 °C. o Stir thoroughly at C for 1 h, add 3 g of cyclohexane, and heat at 80°C. oStirring at C for 3 h yielded Al-Si porous liquid.

[0041] Experimental procedure for carbon dioxide adsorption: The adsorption performance of carbon dioxide was evaluated in a batch reactor. Before each adsorption reaction, the reactor was sealed and filled with carbon dioxide to 5 MPa. After 1 hour, the pressure inside the device remained unchanged, indicating good sealing of the reactor. 5 g of liquid material was weighed and placed in a 50 mL reactor, sealed, and the constant temperature water bath was adjusted to 25℃. Carbon dioxide gas was then introduced at 2 MPa, and the gas inlet valve was closed. The pressure change inside the reactor was recorded by computer. If the pressure remained unchanged within 1 hour, the adsorption reaction was considered complete.

[0042] Under low-pressure conditions, carbon dioxide can be approximated as an ideal gas, but this will inevitably differ from reality. Therefore, a correction factor γ is introduced. γ is mainly related to pressure. The correction factor γ can be obtained by calculating the gas compression model using Matlab and inputting the gas composition and pressure. The amount of carbon dioxide adsorbed is calculated using the constant volume method. The data acquisition device records the pressure change inside the reactor. The difference between the pressure after the reaction and the initial pressure inside the reactor is the amount of carbon dioxide gas change. The temperature inside the reactor can be obtained using a constant temperature water bath. Therefore, the amount of carbon dioxide adsorbed per gram of porous material during the adsorption process is calculated as shown in Equations 2-1 and 2-2.

[0043] Examples 1, 2, and 3 belong to the same type: silicon-based porous liquids. The gas adsorption results at a reaction pressure of 2 MPa are as follows: Figure 6 And as shown in the table below: The pore structure of liquid materials cannot be measured directly; it can only be inferred from TEM results that the pore structure of the precursor is retained. Therefore, this proves that the liquid material contains a pore structure. The pore structure of the precursor material was determined using nitrogen-physical adsorption-desorption, and the results are as follows: The pore structures of the precursors in Comparative Example 1 and Comparative Examples 2-3 are shown in the table below. Figure 7 As shown: This invention prepares a liquid porous material, but since it is generated by coupling a precursor with a coupling agent, the pore structure of the liquid material cannot be characterized. TEM analysis reveals that the precursor retains a complete pore structure within the liquid porous material, indicating the presence of pores within the liquid porous material. In carbon dioxide adsorption applications, the adsorption capacity per unit mass of carbon dioxide from the precursor (solid porous material) and the liquid porous material is primarily compared. Figure 5This paper compares the carbon dioxide adsorption capacities of the precursor (Fe-Si), coupling agent, and Fe-Si liquid porous material under different pressures. It shows that the carbon dioxide adsorption capacity of all three increases with increasing pressure. The adsorption capacity of Fe-Si porous liquid per unit mass of carbon dioxide at pressures of 0.5, 1, 1.5, and 2 MPa are 0.27, 0.44, 0.59, and 0.99 mmol / g, respectively. The increase in carbon dioxide adsorption capacity of the porous liquid with increasing pressure is due to the fact that the adsorption of carbon dioxide by the porous liquid is a mixed process of physical dissolution and chemisorption. Specifically, during the physical dissolution process, the carbon dioxide adsorption capacity of the porous liquid increases with increasing pressure.

[0044] This invention patent can also be implemented in other types of instances. Those skilled in the art can make corresponding changes based on this invention, but all such changes should fall within the protection scope of this invention.

Claims

1. A method for preparing a liquid porous material, characterized in that: This material is a liquid phase used for the efficient capture of carbon dioxide, and its preparation process includes the following steps: (1) Prepare an iron salt solution of a certain concentration and take a certain amount of ammonia water as the alkaline solution; (2) Add the iron salt solution and alkali solution obtained in step (1) dropwise into a beaker containing water while stirring and controlling the pH. (3) Stabilize the gel obtained in step (2) for 10-180 min, quickly add silicon source, age for 20-150 min, dry at 100-200℃ for 12-24 h, and then calcine it in air atmosphere at 300-600℃ for 2-12 h to obtain amorphous iron-silicon material. (4) Add the titanate coupling agent and amorphous iron-silicon material into the sample bottle and pre-stir at room temperature for 10-60 min to form a suspension; (5) Stir the suspension obtained in step (4) at 30-80℃ for 0.5-12 h. (6) Add cyclohexane to the solution obtained in step (5) and stir at 30-90 °C for several hours to obtain a liquid porous material; The titanate coupling agent in step (4) is one of isopropyl tris(dioctyl pyrophosphoryloxy) titanate, isopropyl tris(dioctyl pyrophosphoryloxy) titanate, and isopropyl tris(isostearoyl) titanate.

2. The preparation method according to claim 1, characterized in that: The concentration of the iron salt solution in step (1) is 0.5 mol / L-2 mol / L, and the mass fraction of ammonia water is 25%-28%.

3. The preparation method according to claim 1, characterized in that: The pH value of the suspension system formed in step (2) is maintained between 8 and 11.

4. The preparation method according to claim 1, characterized in that: The silicon source in step (3) is water glass or sodium silicate.

5. The preparation method according to claim 1, characterized in that: In step (4), the mass ratio of amorphous iron-silicon material to titanate coupling agent is 1:10-1:

15.

6. The preparation method according to claim 1, characterized in that: The stirring time in step (5) is 0.5-6 h.

7. The preparation method according to claim 1, characterized in that: In step (6), the stirring temperature is 60-90 ℃ and the reaction time is not less than 3 h.

8. The liquid porous material prepared by the preparation method according to any one of claims 1-7, characterized in that: The liquid porous material is an Fe-Si porous liquid material.

9. An application of the liquid porous material as described in claim 8 in carbon dioxide capture, characterized in that: Fe-Si porous liquid material was added to the reactor as an adsorbent, and carbon dioxide was added at a certain pressure. The reaction conditions were: reaction temperature 20-40 ℃, carbon dioxide pressure 0-2 MPa, and adsorption time 1-12 h.

Citation Information

Patent Citations

  • SiO2 porous liquid with fluid behavior at room temperature and preparation method thereof

    CN107140644A

  • Porous liquid material and preparation method thereof

    CN108905501A

  • Porous liquid as well as preparation method and application thereof

    CN109745952A

  • Hollow carbon sphere HCS porous liquid with flowing behavior at room temperature and preparation method

    CN112934196A

  • MOF (Metal Organic Framework)-based porous liquid carbon capture absorbent as well as preparation method and application thereof

    CN114748984A