A polyurethane foam for oil-water separation and its preparation method

By hydrophobic modification of chitosan and preparing nanofibers using electrospinning technology, the problems of high water absorption and insufficient hydrophobicity of polyurethane foam in oil-water separation are solved, and efficient oil-water separation and multiple cycle stability are achieved.

CN118063834BActive Publication Date: 2024-11-05HAINAN NORMAL UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410221674.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-02-28
Publication Date
2024-11-05
Estimated Expiration
2044-02-28

AI Technical Summary

Technical Problem

The existing polyurethane foam has high water absorption rate during oil-water separation, which leads to difficulty in handling oil-water mixtures and insufficient hydrophobicity, affecting recycling efficiency.

Method used

Nanostructural fibers on hydrophobic surfaces are prepared by hydrophobic modification of chitosan and electrospinning technology, combined with polyurethane foam for composite, increasing its surface roughness and hydrophobicity.

Benefits of technology

It significantly improves the hydrophobicity of polyurethane foam, enhances its oil absorption rate and reduces its water absorption rate, so that it exhibits extremely high oil-water separation performance and multiple cycle stability during the oil-water separation process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118063834B_ABST
    Figure CN118063834B_ABST
Patent Text Reader

Abstract

The present invention belongs to the technical field of oil-water separation, and particularly relates to a polyurethane foam used for oil-water separation and a preparation method thereof. The present invention hydrophobically modifies chitosan, prepares nanostructured fibers with a hydrophobic surface by using electrostatic spinning technology, and composites the nanostructured fibers with polyurethane foam to load them in the pores of the polyurethane foam, thereby increasing the surface roughness of the polyurethane foam. Furthermore, since the nanostructured fibers have a very high specific surface area and a hydrophobic surface, these characteristics together greatly increase the hydrophobicity of the polyurethane foam, and the polyurethane foam has an extremely high oil absorption rate and an extremely low water absorption rate.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of oil-water separation, and particularly relates to a polyurethane foam used for oil-water separation and a preparation method thereof. Background Art

[0002] With the rapid development of the global economy and the continuous development of industrialization, offshore oil transportation and petrochemical industries are also developing rapidly. However, many accidents have occurred in the process, resulting in a large amount of oil spills. A large amount of oily wastewater has a huge impact on the survival of animals and plants and the ecosystem. Therefore, it is increasingly important to effectively separate oil from water and recover floating oil on the water surface. Therefore, it is urgent to develop an efficient super-hydrophobic oil-water separation material.

[0003] There are currently widely used adsorbent materials that can potentially be used for oil-water separation, but these adsorbents have poor selectivity and can be recycled only a few times. In some scenarios, they cannot achieve effective oil-water separation and may even cause additional pollution to the water body. In recent years, porous materials have been frequently used due to their low cost, good oil-water separation effect and simple operation. Therefore, it is possible to use commercial polyurethane foam for effective oil-water separation. Compared with other adsorbents, polyurethane foam oil has a better three-dimensional porous structure, and it has a better specific surface area, porosity and better mechanical properties. It can achieve multiple cycles of oil absorption and desorption of foam, and oil can be recovered by physical extrusion.

[0004] Since the interior of polyurethane foam is a grid-like or film-like porous structure, it not only has a large specific surface area, but also contains abundant capillary channels. Therefore, when it comes into contact with an oil-water mixture, it will not only produce adsorption on the surface of the material, but also absorb oil and water along with the filling space. Since the polymer polyol used to prepare general polyurethane foam has low lipophilicity, the contact angle between the prepared polyurethane foam and water is small, so water and oil are more likely to gather in the micropores of such polyurethane foam and form a certain thickness. While absorbing oil in the oil-water mixture, it also absorbs water. The water absorption rate is generally 2-4 times its own weight, which makes it difficult to process the oil-water mixture after adsorption after secondary separation.

[0005] Therefore, it is necessary to modify the surface of the polyurethane foam structure and increase its surface hydrophobicity to make it more suitable for oil-water separation. Summary of the invention

[0006] In order to solve the above problems, the present invention provides a method for preparing polyurethane foam for oil-water separation, which comprises the following steps:

[0007] (1) dissolving chitosan in a 1:1 mixture of triethylamine and chloroform, adding an amino protecting agent to protect the amino group, then slowly adding octadecanoyl chloride dropwise, continuing the reaction for 3-6 hours, heating to reflux for 8-10 hours, cooling the reaction solution to room temperature, repeatedly performing solid-liquid separation, then adding an amino deprotecting agent to deprotect, and vacuum drying to obtain hydrophobically modified chitosan,

[0008] (2) mixing hydrophobically modified chitosan and polylactic acid dissolved in the same solvent at the same concentration in a volume ratio of 1:2, and electrospinning the mixed solution using a high-voltage electrospinning technique to obtain hydrophobically modified chitosan-based nanofibers,

[0009] (3) stirring a mixture containing hydrophobically modified chitosan-based nanofibers, polyols, foam stabilizers, catalysts and foaming agents, and then rapidly adding isocyanate and vigorously mechanically stirring until small bubbles appear, and then aging the mixture at 60-100° C. for 3-6 hours to obtain a polyurethane foam of composite hydrophobically modified chitosan-based nanofibers.

[0010] (4) The polyurethane foam obtained in step (3) is immersed in a glutaraldehyde solution, reacted at room temperature for 4 hours, and then heat treated for 10-14 hours. Finally, it is repeatedly rinsed with distilled water to make the foam neutral, and dried at 75° C. overnight.

[0011] Furthermore, the chitosan described in step (1) has a deacetylation degree of 70 to 90% and a weight average molecular weight M w It ranges from 100,000 to 800,000.

[0012] Furthermore, the molar ratio of chitosan to acylating agent is 1:1-9.

[0013] Furthermore, the amino protecting agent is methanesulfonic acid or phthalic anhydride.

[0014] Furthermore, the amino deprotecting agent is ammonia water or hydrazine hydrate.

[0015] Furthermore, the solvent for preparing the solution in step (2) is one or more of cyclohexane, chloroform, n-hexane or ethyl acetate, and the prepared concentration is 5 to 15 wt%.

[0016] Furthermore, the parameters of the high-voltage electrospinning technology described in step (2) are: a propulsion rate of 0.1 to 2 ml / h, a collection distance of 5 to 25 cm, and a high voltage of 10 to 50 kV.

[0017] Further, the polyol is a polyol.

[0018] Furthermore, the foam stabilizer is silicone oil.

[0019] Furthermore, the catalyst is n-butyltin dilaurate.

[0020] Furthermore, the foaming agent is sodium bicarbonate.

[0021] Furthermore, the isocyanate is isophordine diisocyanate.

[0022] Furthermore, in step (3), the added amounts of the components are as follows by weight: 5-10 parts of hydrophobically modified chitosan-based nanofibers, 20-50 parts of polyols, 1-5 parts of catalysts, 1-5 parts of foam stabilizers, 1-5 parts of blowing agents, and 20-40 parts of isocyanates.

[0023] Furthermore, in step (4), the concentration of the glutaraldehyde solution is 0.25 wt %.

[0024] Furthermore, in step (4), the heat treatment is carried out at 1 to 3 K·min -1 The temperature is raised to 105-120°C at a rate of 1.

[0025] The present invention also provides a polyurethane foam prepared by the method described herein and used for oil-water separation.

[0026] Beneficial Effects of the Invention

[0027] The present invention hydrophobically modifies chitosan and prepares nanostructured fibers with hydrophobic surfaces by using electrostatic spinning technology, and composites the nanostructured fibers with polyurethane foam to be loaded in the pores of the polyurethane foam, thereby increasing the surface roughness of the polyurethane foam. Furthermore, since the nanostructured fibers have a very high specific surface area and a hydrophobic surface, these characteristics together greatly increase the hydrophobicity of the polyurethane foam, and the polyurethane foam has an extremely high oil absorption rate and an extremely low water absorption rate. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 The water contact angle test graph of the polyurethane foam prepared in Example 1 is shown.

[0029] Figure 2 A graph showing the oil absorption capacity test results of the polyurethane foam prepared in Example 1 at room temperature. DETAILED DESCRIPTION

[0030] The present invention is further described below with reference to specific examples, but the examples do not limit the present invention in any form. Unless otherwise specified, the reagents, methods and equipment used in the present invention are conventional reagents, methods and equipment in the art.

[0031] Example 1

[0032] This embodiment provides a polyurethane foam for oil-water separation, which is prepared as follows:

[0033] (1) Under ice bath conditions, 3.5 g of chitosan with a deacetylation degree of 80% and a weight average molecular weight of 200,000 was dissolved in a mixture of 50 ml of triethylamine and 50 ml of chloroform, and methanesulfonic acid was added to protect the amino group. Then, 25.0 g of octadecanoyl chloride dissolved in 40 ml of chloroform was slowly added dropwise, and the reaction was continued for 6 hours. The temperature was raised to reflux for 10 hours, and the reaction solution was cooled to room temperature, and solid-liquid separation was repeated. Then, ammonia water was added to deprotect the chitosan, and the chitosan was obtained after vacuum drying.

[0034] (2) dissolving the hydrophobically modified chitosan in chloroform to prepare a solution with a concentration of 10 wt %, and dissolving the polylactic acid in chloroform to prepare a solution with a concentration of 10 wt %, then mixing the two solutions in a volume ratio of 1:2, and electrospinning the mixed solution using a high-voltage electrospinning technique (propulsion rate of 1 ml / h, collection distance of 15 cm, high voltage voltage of 30 kV) to obtain hydrophobically modified chitosan-based nanofibers,

[0035] (3) A mixture of 2 g of hydrophobically modified chitosan-based nanofibers, 10 g of polyol, 0.6 g of silicone oil, 0.6 g of n-butyltin dilaurate and 1 g of sodium bicarbonate was stirred uniformly, and then 5 g of isophordione diisocyanate was quickly added and mechanically stirred vigorously until small bubbles appeared, and then the mixture was aged at 100° C. for 6 h to obtain a polyurethane foam of composite hydrophobically modified chitosan-based nanofibers.

[0036] (4) The polyurethane foam obtained in step (3) was immersed in a 0.25 wt% glutaraldehyde solution, reacted at room temperature for 4 h, and heated at 2 K·min -1 The temperature was raised to 110°C at a rate of 100 °C and maintained for 12 hours. Finally, the foam was repeatedly rinsed with distilled water to make it neutral and dried at 75°C overnight.

[0037] Comparative Example 1

[0038] This comparative example provides a polyurethane foam for oil-water separation, which is prepared as follows:

[0039] (1) dissolving chitosan in chloroform to prepare a solution with a concentration of 10 wt %, and dissolving polylactic acid in chloroform to prepare a solution with a concentration of 10 wt %, then mixing the two solutions in a volume ratio of 1:2, and electrospinning the mixed solution using a high-voltage electrospinning technique (propulsion rate of 1 ml / h, collection distance of 15 cm, high voltage voltage of 30 kV) to obtain chitosan-based nanofibers.

[0040] (2) A mixture of 2 g of chitosan-based nanofibers, 10 g of polyol, 0.6 g of silicone oil, 0.6 g of n-butyltin dilaurate and 1 g of sodium bicarbonate was stirred uniformly, and then 5 g of isophordine diisocyanate was quickly added and mechanically stirred vigorously until small bubbles appeared, and then the mixture was aged at 100° C. for 6 h to obtain a polyurethane foam composited with chitosan-based nanofibers.

[0041] (3) The polyurethane foam obtained in step (2) was immersed in a 0.25 wt% glutaraldehyde solution, reacted at room temperature for 4 h, and heated at 2 K·min -1 The temperature was raised to 110°C at a rate of 100 °C and maintained for 12 hours. Finally, the foam was repeatedly rinsed with distilled water to make it neutral and dried at 75°C overnight.

[0042] Comparative Example 2

[0043] This comparative example provides a polyurethane foam for oil-water separation, which is prepared as follows:

[0044] (1) Under ice bath conditions, 3.5 g of chitosan with a deacetylation degree of 80% and a weight average molecular weight of 200,000 was dissolved in a mixture of 50 ml of triethylamine and 50 ml of chloroform, and methanesulfonic acid was added to protect the amino group. Then, 25.0 g of octadecanoyl chloride dissolved in 40 ml of chloroform was slowly added dropwise, and the reaction was continued for 6 hours. The temperature was raised to reflux for 10 hours, and the reaction solution was cooled to room temperature, and solid-liquid separation was repeated. Then, ammonia water was added to deprotect the chitosan, and the chitosan was obtained after vacuum drying.

[0045] (2) A mixture of 2 g of hydrophobically modified chitosan, 10 g of polyol, 0.6 g of silicone oil, 0.6 g of n-butyltin dilaurate and 1 g of sodium bicarbonate was stirred uniformly, and then 5 g of isophordione diisocyanate was quickly added and mechanically stirred vigorously until small bubbles appeared, and then the mixture was aged at 100° C. for 6 h to obtain a polyurethane foam of a composite hydrophobically modified chitosan.

[0046] (3) The polyurethane foam obtained in step (2) was immersed in a 0.25 wt% glutaraldehyde solution, reacted at room temperature for 4 h, and heated at 2 K·min -1 The temperature was raised to 110°C at a rate of 100 °C and maintained for 12 hours. Finally, the foam was repeatedly rinsed with distilled water to make it neutral and dried at 75°C overnight.

[0047] Comparative Example 3

[0048] This comparative example provides a polyurethane foam for oil-water separation, which is prepared as follows:

[0049] (1) Under ice bath conditions, 3.5 g of chitosan with a deacetylation degree of 80% and a weight average molecular weight of 200,000 was dissolved in a mixture of 50 ml of triethylamine and 50 ml of chloroform, and methanesulfonic acid was added to protect the amino group. Then, 25.0 g of octadecanoyl chloride dissolved in 40 ml of chloroform was slowly added dropwise, and the reaction was continued for 6 hours. The temperature was raised to reflux for 10 hours, and the reaction solution was cooled to room temperature, and solid-liquid separation was repeated. Then, ammonia water was added to deprotect the chitosan, and the chitosan was obtained after vacuum drying.

[0050] (2) dissolving polylactic acid in chloroform to prepare a solution with a concentration of 10 wt%, and electrospinning the solution using a high-voltage electrospinning technique (propulsion rate of 1 ml / h, collection distance of 15 cm, high voltage of 30 kV) to obtain polylactic acid nanofibers, dissolving hydrophobically modified chitosan in a citric acid solution, adding sodium hypophosphite and a penetrant JFC to prepare a chitosan finishing solution, and performing a finishing process of impregnating, baking, washing and drying the polylactic acid nanofibers to obtain hydrophobically modified chitosan-finished nanofibers,

[0051] (3) A mixture of 2 g of hydrophobically modified chitosan-finished nanofibers, 10 g of polyol, 0.6 g of silicone oil, 0.6 g of n-butyltin dilaurate and 1 g of sodium bicarbonate was stirred uniformly, and then 5 g of isophordione diisocyanate was quickly added and mechanically stirred vigorously until small bubbles appeared, and then the mixture was aged at 100° C. for 6 h to obtain a polyurethane foam of composite hydrophobically modified chitosan-finished nanofibers.

[0052] (4) The polyurethane foam obtained in step (3) was immersed in a 0.25 wt% glutaraldehyde solution, reacted at room temperature for 4 h, and heated at 2 K·min -1 The temperature was raised to 110°C at a rate of 100 °C and maintained for 12 hours. Finally, the foam was repeatedly rinsed with distilled water to make it neutral and dried at 75°C overnight.

[0053] Comparative Example 4

[0054] This comparative example provides a polyurethane foam for oil-water separation, which is prepared as follows:

[0055] (1) Under ice bath conditions, 3.5 g of chitosan with a deacetylation degree of 80% and a weight average molecular weight of 200,000 was dissolved in a mixture of 50 ml of triethylamine and 50 ml of chloroform, and methanesulfonic acid was added to protect the amino group. Then, 25.0 g of octadecanoyl chloride dissolved in 40 ml of chloroform was slowly added dropwise, and the reaction was continued for 6 hours. The temperature was raised to reflux for 10 hours, and the reaction solution was cooled to room temperature, and solid-liquid separation was repeated. Then, ammonia water was added to deprotect the chitosan, and the chitosan was obtained after vacuum drying.

[0056] (2) dissolving the hydrophobically modified chitosan in chloroform to prepare a solution with a concentration of 10 wt %, and dissolving the polylactic acid in chloroform to prepare a solution with a concentration of 10 wt %, then mixing the two solutions in a volume ratio of 1:2, and electrospinning the mixed solution using a high-voltage electrospinning technique (propulsion rate of 1 ml / h, collection distance of 15 cm, high voltage voltage of 30 kV) to obtain hydrophobically modified chitosan-based nanofibers,

[0057] (3) A mixture of 2 g of hydrophobically modified chitosan-based nanofibers, 10 g of polyol, 0.6 g of silicone oil, 0.6 g of n-butyltin dilaurate and 1 g of sodium bicarbonate was stirred evenly, and then 5 g of isophordine diisocyanate was quickly added and vigorously mechanically stirred until small bubbles appeared. The mixture was then aged at 100 °C for 6 h to obtain a polyurethane foam of composite hydrophobically modified chitosan-based nanofibers.

[0058] Comparative Example 5

[0059] This comparative example provides a polyurethane foam for oil-water separation, which is prepared as follows:

[0060] (1) Under ice bath conditions, 3.5 g of chitosan with a deacetylation degree of 80% and a weight average molecular weight of 200,000 was dissolved in a mixture of 50 ml of triethylamine and 50 ml of chloroform, and methanesulfonic acid was added to protect the amino group. Then, 25.0 g of octadecanoyl chloride dissolved in 40 ml of chloroform was slowly added dropwise, and the reaction was continued for 6 hours. The temperature was raised to reflux for 10 hours, and the reaction solution was cooled to room temperature, and solid-liquid separation was repeated. Then, ammonia water was added to deprotect the chitosan, and the chitosan was obtained after vacuum drying.

[0061] (2) dissolving the hydrophobically modified chitosan in chloroform to prepare a solution with a concentration of 10 wt %, and dissolving the polylactic acid in chloroform to prepare a solution with a concentration of 10 wt %, then mixing the two solutions in a volume ratio of 1:1, and electrospinning the mixed solution using a high-voltage electrospinning technique (propulsion rate of 1 ml / h, collection distance of 15 cm, high voltage voltage of 30 kV) to obtain hydrophobically modified chitosan-based nanofibers,

[0062] (3) A mixture of 2 g of hydrophobically modified chitosan-based nanofibers, 10 g of polyol, 0.6 g of silicone oil, 0.6 g of n-butyltin dilaurate and 1 g of sodium bicarbonate was stirred uniformly, and then 5 g of isophordione diisocyanate was quickly added and mechanically stirred vigorously until small bubbles appeared, and then the mixture was aged at 100° C. for 6 h to obtain a polyurethane foam of composite hydrophobically modified chitosan-based nanofibers.

[0063] (4) The polyurethane foam obtained in step (3) was immersed in a 0.25 wt% glutaraldehyde solution, reacted at room temperature for 4 h, and heated at 2 K·min -1 The temperature was raised to 110°C at a rate of 100 °C and maintained for 12 hours. Finally, the foam was repeatedly rinsed with distilled water to make it neutral and dried at 75°C overnight.

[0064] Test Example 1

[0065] The water contact angle (WCA) test was performed on the polyurethane foams obtained in Example 1 and Comparative Examples 1-5. The results are shown in Table 1.

[0066] Table 1

[0067]

[0068] As can be seen from the results of Table 1, the polyurethane foam prepared by Example 1 of the present invention has super-hydrophobicity, and when using unmodified chitosan (Comparative Example 1), not using polylactic acid nanofiber (Comparative Example 2), chitosan and polylactic acid nanofiber composite (Comparative Example 3) by the mode of post-finishing, and not using glutaraldehyde to carry out the last cross-linking step (Comparative Example 4), the water contact angle is relatively small, and hydrophobicity is not strong enough. When electrostatic spinning, when the ratio of chitosan is too high (Comparative Example 5), it is not suitable for forming stable nanofibers, resulting in weakening of the hydrophobic modification effect of polyurethane foam.

[0069] Test Example 2

[0070] Figure 2 The oil absorption capacity of the polyurethane foam of Example 1 was tested at room temperature. Diesel and crude oil were subjected to 10 oil absorption-desorption tests. The absorption capacity of diesel was up to 39.8 times of its own weight, and there was no significant change in the oil absorption capacity after 20 cycles. The initial absorption capacity of crude oil was 30.9 times of its own weight, and after 5 cycles, the oil absorption capacity dropped to 16.4 times of its own weight, and stabilized within 10 cycles, always maintaining at about 16.4 times.

[0071] It should be noted that the preferred embodiments of the present invention are given in the specification and drawings of the present invention. However, the present invention can be implemented in many different forms and is not limited to the embodiments described in this specification. These embodiments are not used as additional limitations on the content of the present invention. The purpose of providing these embodiments is to make the understanding of the disclosure of the present invention more thorough and comprehensive. In addition, the above-mentioned technical features continue to be combined with each other to form various embodiments not listed above, which are all regarded as the scope of the present invention; further, for ordinary technicians in this field, they can be improved or transformed according to the above description, and all these improvements and transformations should belong to the protection scope of the claims attached to the present invention.

Claims

1. A method for preparing a polyurethane foam for separating diesel or crude oil from water, wherein the polyurethane foam can effectively absorb diesel or crude oil. It is characterized in that The preparation method comprises the following steps: (1) dissolving chitosan in a 1:1 mixture of triethylamine and chloroform, adding an amino protecting agent to protect the amino group, then slowly adding octadecanoyl chloride dropwise, continuing the reaction for 3-6 hours, raising the temperature to reflux for 8-10 hours, cooling the reaction solution to room temperature, repeatedly performing solid-liquid separation, then adding an amino deprotecting agent to deprotect, and vacuum drying to obtain hydrophobically modified chitosan; (2) mixing hydrophobically modified chitosan and polylactic acid dissolved in the same solvent at the same concentration in a volume ratio of 1:2, and electrospinning the mixed solution using a high-voltage electrospinning technique to obtain hydrophobically modified chitosan-based nanofibers; (3) stirring a mixture containing hydrophobically modified chitosan-based nanofibers, polyols, foam stabilizers, catalysts and blowing agents, and then rapidly adding isocyanate and vigorously mechanically stirring until small bubbles appear, and then aging the mixture at 60-100° C. for 3-6 hours to obtain a polyurethane foam of composite hydrophobically modified chitosan-based nanofibers; (4) immersing the polyurethane foam obtained in step (3) into a glutaraldehyde solution, reacting at room temperature for 4 hours, and then heat treating for 10-14 hours. Finally, repeatedly rinsing with distilled water to make the foam neutral, and drying at 75° C. overnight. The foam stabilizer is silicone oil, the catalyst is n-butyltin dilaurate, the blowing agent is sodium bicarbonate, and the isocyanate is isophorone diisocyanate; In step (3), the added amounts of the components are as follows by weight: 5-10 parts of hydrophobically modified chitosan-based nanofibers, 20-50 parts of polyols, 1-5 parts of catalysts, 1-5 parts of foam stabilizers, 1-5 parts of foaming agents, and 20-40 parts of isocyanates; In step (4), the concentration of the glutaraldehyde solution is 0.25 wt %.

2. The preparation method according to claim 1, It is characterized in that The chitosan described in step (1) has a deacetylation degree of 70-90% and a weight average molecular weight Mw of 100,000-800,000; and the molar ratio of chitosan to octadecanoyl chloride is 1:1-9.

3. The preparation method according to claim 1, It is characterized in that The amino protecting agent is methanesulfonic acid or phthalic anhydride, and the amino deprotecting agent is ammonia water or hydrazine hydrate.

4. The preparation method according to claim 1, It is characterized in that The solvent of the solution described in step (2) is one or more of cyclohexane, chloroform, n-hexane or ethyl acetate, and the prepared concentration is 5 to 15 wt%. The parameters of the high-voltage electrospinning technology described in step (2) are: a propulsion rate of 0.1 to 2 ml / h, a collection distance of 5 to 25 cm, and a high voltage of 10 to 50 kV.

5. The preparation method according to claim 1, It is characterized in that In step (4), the heat treatment is carried out at 1 to 3 K·min -1 The temperature is raised to 105-120°C at a rate of 1.

6. A polyurethane foam prepared by the method according to any one of claims 1 to 5 and used for separation of diesel or crude oil from water.