Environmentally friendly antibacterial sponge and preparation method thereof
By preparing an environmentally friendly antibacterial sponge containing carboxymethyl chitosan, sodium alginate, and a potent antibacterial agent, the problem of bacteria growth in traditional sponges has been solved, resulting in a highly effective antibacterial and environmentally friendly sponge material suitable for wound dressings.
Patent Information
- Application Number
- CN202410273740.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-03-11
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2044-03-11
AI Technical Summary
Traditional sponge materials are prone to bacterial growth, affecting their performance and posing a potential threat to human health. Furthermore, they are difficult to degrade, leading to environmental pollution.
An environmentally friendly antibacterial sponge is prepared by mixing and freeze-drying materials such as carboxymethyl chitosan, sodium alginate, polyethylene oxide, a potent antibacterial agent, and silver nitrate. The biomedical properties of carboxymethyl chitosan and sodium alginate, along with the antibacterial properties of the potent antibacterial agent and nano-silver, are utilized to form a highly efficient antibacterial sponge.
The prepared environmentally friendly antibacterial sponge has excellent antibacterial and environmental performance, is harmless to the human body, can degrade on its own, does not pollute the environment, is suitable for wound dressings, and improves the mechanical strength and antibacterial effect of the sponge.
Smart Images

Figure CN118085389B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of antibacterial sponges, and in particular to an environmentally friendly antibacterial sponge and a preparation method thereof. Background Art
[0002] Sponge is a material widely used in household, industrial and medical fields. It has strong water absorption and good elasticity. However, traditional sponge materials are prone to bacteria, which not only affects the use effect, but also poses a potential threat to human health. Although there are antibacterial sponges on the market, most antibacterial agents are toxic and harmful to the human body and the environment. Therefore, it is of great significance to develop an environmentally friendly antibacterial sponge and its preparation method. Summary of the invention
[0003] In order to overcome the above-mentioned technical problems, the object of the present invention is to provide an environmentally friendly antibacterial sponge and a preparation method thereof: carboxymethyl chitosan, deionized water and polyethylene oxide are mixed evenly to obtain a reaction solution one, sodium alginate and deionized water are mixed evenly to obtain a reaction solution two, a potent antibacterial agent, silver nitrate, 1-ethyl-(3-dimethylaminopropyl)carbodiimide hydrochloride, N-hydroxysuccinimide and deionized water are mixed evenly to obtain a reaction solution three, reaction solution one, reaction solution two and reaction solution three are mixed, then poured into a mold and allowed to stand, and then freeze-dried to obtain an environmentally friendly antibacterial sponge, which solves the problem that the existing traditional sponge materials are prone to breed bacteria, which not only affects the use effect, but also poses a potential threat to human health, and is difficult to degrade, resulting in easy pollution to the environment.
[0004] The purpose of the present invention can be achieved by the following technical solutions:
[0005] A method for preparing an environmentally friendly antibacterial sponge comprises the following steps:
[0006] Step 1: weigh 4-6 parts of carboxymethyl chitosan, 2-2.5 parts of sodium alginate, 0.5-1.5 parts of polyethylene oxide, 0.05-0.25 parts of a potent antibacterial agent, 0.01-0.03 parts of silver nitrate, 0.2-0.25 parts of 1-ethyl-(3-dimethylaminopropyl)carbodiimide hydrochloride, 0.12-0.16 parts of N-hydroxysuccinimide and 100-120 parts of deionized water according to weight parts, and set aside;
[0007] Step 2: adding carboxymethyl chitosan to 40-50% of the total weight of deionized water, and then stirring the mixture for 40-50 minutes at a temperature of 25-30° C. and a stirring rate of 300-400 r / min, adding polyethylene oxide and continuing to stir the mixture for 25-30 minutes, and then ultrasonically treating the mixture for 20-30 minutes at an ultrasonic power of 200-300 W to obtain a reaction solution 1;
[0008] Step 3: adding sodium alginate to 25-30% of the total weight of deionized water, stirring the mixture for 30-35 minutes at a temperature of 25-30° C. and a stirring rate of 300-400 r / min, and then ultrasonically treating the mixture for 10-15 minutes at an ultrasonic power of 200-300 W to obtain a reaction solution 2;
[0009] Step 4: adding a potent antibacterial agent, silver nitrate, 1-ethyl-(3-dimethylaminopropyl)carbodiimide hydrochloride and N-hydroxysuccinimide to the remaining deionized water, and then stirring the mixture for 1-2 hours at a temperature of 25-30° C. and a stirring rate of 300-400 r / min to obtain a reaction solution 3;
[0010] Step 5: Mix reaction solution 1, reaction solution 2 and reaction solution 3, and then stir the reaction at a temperature of 60-70°C and a stirring rate of 300-400r / min for 2-3 hours, then pour it into a mold and let it stand for 2-3 hours, then place it in a vacuum freeze dryer and freeze-dry it at a temperature of -60°C to obtain the environmentally friendly antibacterial sponge.
[0011] As a further solution of the present invention: the molecular weight of the carboxymethyl chitosan is 9000Da, the viscosity of the sodium alginate is 200±20mPa·s, and the molecular weight of the polyethylene oxide is 2 million.
[0012] As a further solution of the present invention: the potent antibacterial agent is prepared by the following steps:
[0013] Step A1: 3-bromopyridine, ethyl 4-piperidinate, anhydrous potassium carbonate and N-methylpyrrolidone are added to a three-necked flask equipped with a stirrer and a thermometer, and stirred for 40-50 hours at a pressure of 0.50-0.55 MPa, a temperature of 180-185° C. and a stirring rate of 300-400 r / min. After the reaction is completed, the reaction product is cooled to room temperature and then centrifuged. The precipitate is recrystallized with anhydrous methanol and then placed in a vacuum drying oven and dried at a temperature of 50-55° C. for 2-3 hours to obtain intermediate 1;
[0014] Step A2: Add intermediate 1, thionyl chloride and pyridine to a three-necked flask equipped with a stirrer and a thermometer, stir and react for 20-30 minutes at a temperature of 25-30° C. and a stirring rate of 300-400 r / min, then heat to 70-75° C. and continue stirring and reacting for 1.5-2 hours. After the reaction is completed, the reaction product is cooled to room temperature, and then the solvent is removed by rotary evaporation to obtain intermediate 2;
[0015] Step A3: Add intermediate 2, hydroquinone and dichloromethane to a three-necked flask equipped with a stirrer, a thermometer and a reflux condenser, stir and react for 20-30 minutes at a temperature of 25-30°C and a stirring rate of 300-400r / min, then heat to reflux and continue stirring and reacting for 3-5 hours. After the reaction is completed, the reaction product is cooled to room temperature, and then the solvent is removed by rotary evaporation, and then recrystallized with petroleum ether, and then placed in a vacuum drying oven and dried at a temperature of 60-65°C for 1-1.5 hours to obtain intermediate 3;
[0016] Step A4: Add intermediate 3, benzyl bromide and anhydrous acetone to a three-necked flask equipped with a stirrer, a thermometer and a reflux condenser, and stir the reaction at a temperature of 25-30°C and a stirring rate of 300-400r / min for 20-30h. After the reaction, the reaction product is rotary evaporated to remove the solvent, and then recrystallized with anhydrous methanol, and then placed in a vacuum drying oven and dried at a temperature of 50-55°C for 3-5h to obtain a potent antibacterial agent.
[0017] As a further scheme of the present invention: the usage ratio of the 3-bromopyridine, ethyl 4-piperidinate, anhydrous potassium carbonate and N-methylpyrrolidone in step A1 is 10 mmol: 10 mmol: 3-3.5 g: 30-35 mL.
[0018] As a further solution of the present invention: the usage ratio of the intermediate 1, thionyl chloride and pyridine in step A2 is 10 mmol: 5-7 mL: 0.1-0.3 mL.
[0019] As a further solution of the present invention: the usage ratio of the intermediate 2, hydroquinone and dichloromethane in step A3 is 20mmol:10mmol:50-60mL.
[0020] As a further solution of the present invention: the usage ratio of the intermediate 3, benzyl bromide and anhydrous acetone in step A4 is 10 mmol: 45-55 mmol: 80-90 mL.
[0021] As a further solution of the present invention: an environmentally friendly antibacterial sponge comprises the following components in parts by weight:
[0022] 4-6 parts of carboxymethyl chitosan, 2-2.5 parts of sodium alginate, 0.5-1.5 parts of polyethylene oxide, 0.05-0.25 parts of a potent antibacterial agent, 0.01-0.03 parts of silver nitrate, 0.2-0.25 parts of 1-ethyl-(3-dimethylaminopropyl)carbodiimide hydrochloride, 0.12-0.16 parts of N-hydroxysuccinimide and 100-120 parts of deionized water.
[0023] Beneficial effects of the present invention:
[0024] The invention discloses an environment-friendly antibacterial sponge and a preparation method thereof. The method comprises the following steps: uniformly mixing carboxymethyl chitosan, deionized water and polyethylene oxide to obtain a first reaction solution; uniformly mixing sodium alginate and deionized water to obtain a second reaction solution; uniformly mixing a potent antibacterial agent, silver nitrate, 1-ethyl-(3-dimethylaminopropyl) carbodiimide hydrochloride, N-hydroxysuccinimide and deionized water to obtain a third reaction solution; mixing the first reaction solution, the second reaction solution and the third reaction solution, and then pouring the mixture into a mold and letting it stand, and then freeze-drying the mixture to obtain the environment-friendly antibacterial sponge. The environment-friendly antibacterial sponge uses carboxymethyl chitosan and sodium alginate as main raw materials, and both of them have good water absorption and biodegradability. Medical properties, including tissue regeneration, hemostatic properties, antibacterial, antioxidant, cell adhesion, etc., make it a good choice for wound dressings. Adding polyethylene oxide can improve the mechanical strength of both. 1-ethyl-(3-dimethylaminopropyl) carbodiimide hydrochloride and N-hydroxysuccinimide can promote the cross-linking of carboxymethyl chitosan and sodium alginate, thereby further improving its mechanical strength. Carboxymethyl chitosan also has excellent antibacterial properties, and carboxymethyl chitosan and sodium alginate have reducing properties, which can reduce the silver ions provided by silver nitrate into nano-silver particles, further improving its antibacterial properties. After adding a strong antibacterial agent, the environmentally friendly antibacterial sponge obtained has excellent antibacterial effect.
[0025] In the process of preparing the environmentally friendly antibacterial sponge, a strong antibacterial agent is first prepared. First, 3-bromopyridine and ethyl 4-piperidinic acid are reacted to make the bromine atom on the 3-bromopyridine react with the NH on the piperidine ring of ethyl 4-piperidinic acid to undergo a nucleophilic substitution reaction, and the ester group is hydrolyzed under high pressure alkaline conditions to form a carboxyl group to obtain an intermediate 1. Then, the intermediate 1 is reacted with thionyl chloride. The thionyl chloride converts the carboxyl group on the intermediate 1 into an acyl chloride group to enhance its reactivity to obtain an intermediate 2. Then, the intermediate 2 is reacted with terephthalate. Phenol reaction, the acyl chloride group on the intermediate 2 and the phenolic hydroxyl group on the hydroquinone undergo nucleophilic substitution reaction to obtain the intermediate 3, and finally the intermediate 3 and benzyl bromide react, the benzyl bromide uses the bromine atom to react with the tertiary amine groups on the pyridine ring and the piperidine ring on the intermediate 3 to form a quaternary ammonium group, and a potent antibacterial agent is obtained; the molecular structure of the potent antibacterial agent contains a large number of quaternary ammonium groups, and the quaternary ammonium groups are positively charged and can be adsorbed onto the negatively charged cell membrane, thereby destroying the bacterial cell membrane, achieving the purpose of eliminating bacteria, and achieving a highly effective antibacterial effect.
[0026] The basic raw materials of the sponge of the present invention are carboxymethyl chitosan and sodium alginate, which have good elasticity and water absorption, and also have excellent biodegradability. The sponge degrades by itself after use and does not cause pollution to the environment. The antibacterial factors are potent antibacterial agents and nano-silver, which have broad-spectrum antibacterial properties under the synergistic effect and are non-toxic and harmless to the human body. The method can obtain an environmentally friendly antibacterial sponge with excellent antibacterial properties and environmental protection properties, while ensuring human health and environmental safety, and is of great significance for promoting the development of the antibacterial sponge industry. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] The present invention will be further described below in conjunction with the accompanying drawings.
[0028] Figure 1 It is a process flow chart of a method for preparing an environmentally friendly antibacterial sponge in the present invention;
[0029] Figure 2 It is a bar chart of antibacterial performance detection of the environmentally friendly antibacterial sponge in Examples 4-6 of the present invention and Comparative Examples 1-3. DETAILED DESCRIPTION
[0030] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0031] Embodiment 1:
[0032] See also Figure 1 As shown, this embodiment is a method for preparing a potent antibacterial agent, comprising the following steps:
[0033] Step A1: 10 mmol 3-bromopyridine, 10 mmol ethyl 4-piperidinic acid ester, 3 g anhydrous potassium carbonate and 30 mL N-methylpyrrolidone were added to a three-necked flask equipped with a stirrer and a thermometer, and stirred for 40 hours at a pressure of 0.50 MPa, a temperature of 180° C. and a stirring rate of 300 r / min. After the reaction, the reaction product was cooled to room temperature and then centrifuged. The precipitate was recrystallized with anhydrous methanol and then placed in a vacuum drying oven and dried at 50° C. for 2 hours to obtain intermediate 1;
[0034] Step A2: 10 mmol of intermediate 1, 5 mL of thionyl chloride and 0.1 mL of pyridine were added to a three-necked flask equipped with a stirrer and a thermometer, and the mixture was stirred at 25° C. and a stirring rate of 300 r / min for 20 min, and then the mixture was heated to 70° C. and stirred for 1.5 h. After the reaction was completed, the reaction product was cooled to room temperature, and then the solvent was removed by rotary evaporation to obtain intermediate 2;
[0035] Step A3: 20 mmol of intermediate 2, 10 mmol of hydroquinone and 50 mL of dichloromethane were added to a three-necked flask equipped with a stirrer, a thermometer and a reflux condenser, and the mixture was stirred at 25°C and a stirring rate of 300 r / min for 20 min, and then the mixture was heated to reflux and continued to stir for 3 h. After the reaction was completed, the reaction product was cooled to room temperature, and then the solvent was removed by rotary evaporation, and then the mixture was recrystallized with petroleum ether, and then placed in a vacuum drying oven and dried at 60°C for 1 h to obtain intermediate 3;
[0036] Step A4: Add 10 mmol of intermediate 3, 45 mmol of benzyl bromide and 80 mL of anhydrous acetone into a three-necked flask equipped with a stirrer, a thermometer and a reflux condenser, and stir the reaction at a temperature of 25°C and a stirring rate of 300 r / min for 20 hours. After the reaction is completed, the reaction product is rotary evaporated to remove the solvent, and then recrystallized with anhydrous methanol, and then placed in a vacuum drying oven and dried at a temperature of 50°C for 3 hours to obtain a potent antibacterial agent.
[0037] Embodiment 2:
[0038] See also Figure 1 As shown, this embodiment is a method for preparing a potent antibacterial agent, comprising the following steps:
[0039] Step A1: 10 mmol 3-bromopyridine, 10 mmol ethyl 4-piperidinic acid ester, 3.2 g anhydrous potassium carbonate and 32 mL N-methylpyrrolidone were added to a three-necked flask equipped with a stirrer and a thermometer, and stirred for 45 h at a pressure of 0.52 MPa, a temperature of 182° C. and a stirring rate of 350 r / min. After the reaction was completed, the reaction product was cooled to room temperature and then centrifuged. The precipitate was recrystallized with anhydrous methanol and then placed in a vacuum drying oven and dried at 52° C. for 2.5 h to obtain intermediate 1;
[0040] Step A2: 10 mmol of intermediate 1, 6 mL of thionyl chloride and 0.2 mL of pyridine were added to a three-necked flask equipped with a stirrer and a thermometer, and stirred for reaction at 28°C and a stirring rate of 350 r / min for 25 min, then heated to 72°C and continued to stir for 1.8 h. After the reaction was completed, the reaction product was cooled to room temperature, and then the solvent was removed by rotary evaporation to obtain intermediate 2;
[0041] Step A3: 20 mmol of intermediate 2, 10 mmol of hydroquinone and 55 mL of dichloromethane were added to a three-necked flask equipped with a stirrer, a thermometer and a reflux condenser, and stirred for reaction at a temperature of 28° C. and a stirring rate of 350 r / min for 25 min, then the temperature was raised to reflux and the stirring reaction was continued for 4 h. After the reaction was completed, the reaction product was cooled to room temperature, and then the solvent was removed by rotary evaporation, and then recrystallized with petroleum ether, and then placed in a vacuum drying oven and dried at a temperature of 62° C. for 1.2 h to obtain intermediate 3;
[0042] Step A4: Add 10 mmol of intermediate 3, 50 mmol of benzyl bromide and 85 mL of anhydrous acetone into a three-necked flask equipped with a stirrer, a thermometer and a reflux condenser, and stir the reaction at a temperature of 28°C and a stirring rate of 350 r / min for 25 hours. After the reaction is completed, the reaction product is rotary evaporated to remove the solvent, and then recrystallized with anhydrous methanol, and then placed in a vacuum drying oven and dried at a temperature of 52°C for 4 hours to obtain a potent antibacterial agent.
[0043] Embodiment 3:
[0044] See also Figure 1 As shown, this embodiment is a method for preparing a potent antibacterial agent, comprising the following steps:
[0045] Step A1: 10 mmol 3-bromopyridine, 10 mmol ethyl 4-piperidinic acid ester, 3.5 g anhydrous potassium carbonate and 35 mL N-methylpyrrolidone were added to a three-necked flask equipped with a stirrer and a thermometer, and stirred for 50 hours at a pressure of 0.55 MPa, a temperature of 185° C. and a stirring rate of 400 r / min. After the reaction, the reaction product was cooled to room temperature and then centrifuged. The precipitate was recrystallized with anhydrous methanol and then placed in a vacuum drying oven and dried at 55° C. for 3 hours to obtain intermediate 1;
[0046] Step A2: 10 mmol of intermediate 1, 7 mL of thionyl chloride and 0.3 mL of pyridine were added to a three-necked flask equipped with a stirrer and a thermometer, and the mixture was stirred at 30° C. and 400 r / min for 30 min, then the mixture was heated to 75° C. and stirred for 2 h. After the reaction was completed, the reaction product was cooled to room temperature, and then the solvent was removed by rotary evaporation to obtain intermediate 2;
[0047] Step A3: 20 mmol of intermediate 2, 10 mmol of hydroquinone and 60 mL of dichloromethane were added to a three-necked flask equipped with a stirrer, a thermometer and a reflux condenser, and the mixture was stirred at 30°C and a stirring rate of 400 r / min for 30 min, and then the mixture was heated to reflux and continued to stir for 5 h. After the reaction was completed, the reaction product was cooled to room temperature, and then the solvent was removed by rotary evaporation, and then the mixture was recrystallized with petroleum ether, and then placed in a vacuum drying oven and dried at 65°C for 1.5 h to obtain intermediate 3;
[0048] Step A4: Add 10 mmol of intermediate 3, 55 mmol of benzyl bromide and 90 mL of anhydrous acetone into a three-necked flask equipped with a stirrer, a thermometer and a reflux condenser, and stir the reaction at a temperature of 30°C and a stirring rate of 400 r / min for 30 hours. After the reaction is completed, the reaction product is rotary evaporated to remove the solvent, and then recrystallized with anhydrous methanol, and then placed in a vacuum drying oven and dried at a temperature of 55°C for 5 hours to obtain a potent antibacterial agent.
[0049] Embodiment 4:
[0050] See also Figure 1 As shown, this embodiment is a method for preparing an environmentally friendly antibacterial sponge, comprising the following steps:
[0051] Step 1: Weigh 4 parts of carboxymethyl chitosan, 2 parts of sodium alginate, 0.5 parts of polyethylene oxide, 0.05 parts of the potent antibacterial agent from Example 1, 0.01 parts of silver nitrate, 0.2 parts of 1-ethyl-(3-dimethylaminopropyl) carbodiimide hydrochloride, 0.12 parts of N-hydroxysuccinimide and 100 parts of deionized water according to weight parts for use; the molecular weight of the carboxymethyl chitosan is 9000Da, the viscosity of the sodium alginate is 200±20mPa·s, and the molecular weight of the polyethylene oxide is 2 million;
[0052] Step 2: adding carboxymethyl chitosan to 40% of the total weight of deionized water, and then stirring the mixture at a temperature of 25° C. and a stirring rate of 300 r / min for 40 minutes, then adding polyethylene oxide and continuing to stir the mixture for 25 minutes, and then ultrasonically treating the mixture at an ultrasonic power of 200 W for 20 minutes to obtain a reaction solution 1;
[0053] Step 3: adding sodium alginate to 25% of the total weight of deionized water, stirring the mixture for 30 minutes at a temperature of 25° C. and a stirring rate of 300 r / min, and then ultrasonically treating the mixture for 10 minutes at an ultrasonic power of 200 W to obtain a reaction solution 2;
[0054] Step 4: adding a potent antibacterial agent, silver nitrate, 1-ethyl-(3-dimethylaminopropyl)carbodiimide hydrochloride and N-hydroxysuccinimide to the remaining deionized water, and then stirring the mixture for 1 hour at a temperature of 25° C. and a stirring rate of 300 r / min to obtain a reaction solution 3;
[0055] Step 5: Mix reaction solution 1, reaction solution 2 and reaction solution 3, and then stir the reaction at a temperature of 60°C and a stirring rate of 300r / min for 2 hours, then pour it into a mold and let it stand for 2 hours, then place it in a vacuum freeze dryer and freeze-dry it at a temperature of -60°C to obtain the environmentally friendly antibacterial sponge.
[0056] Embodiment 5:
[0057] See also Figure 1 As shown, this embodiment is a method for preparing an environmentally friendly antibacterial sponge, comprising the following steps:
[0058] Step 1: Weigh 5 parts of carboxymethyl chitosan, 2.2 parts of sodium alginate, 1.0 parts of polyethylene oxide, 0.15 parts of the potent antibacterial agent from Example 2, 0.02 parts of silver nitrate, 0.22 parts of 1-ethyl-(3-dimethylaminopropyl) carbodiimide hydrochloride, 0.14 parts of N-hydroxysuccinimide and 110 parts of deionized water according to weight parts for use; the molecular weight of the carboxymethyl chitosan is 9000Da, the viscosity of the sodium alginate is 200±20mPa·s, and the molecular weight of the polyethylene oxide is 2 million;
[0059] Step 2: adding carboxymethyl chitosan to 45% of the total weight of deionized water, and then stirring the reaction for 45 minutes at a temperature of 28° C. and a stirring rate of 350 r / min, and then adding polyethylene oxide and continuing to stir the reaction for 28 minutes, and then ultrasonically treating for 25 minutes at an ultrasonic power of 250 W to obtain a reaction solution 1;
[0060] Step 3: adding sodium alginate to 28% of deionized water by total weight, stirring the mixture for 32 min at 28° C. and 350 r / min, and then ultrasonically treating the mixture for 12 min at 250 W to obtain a reaction solution 2;
[0061] Step 4: adding a potent antibacterial agent, silver nitrate, 1-ethyl-(3-dimethylaminopropyl)carbodiimide hydrochloride and N-hydroxysuccinimide to the remaining deionized water, and then stirring the mixture at a temperature of 28° C. and a stirring rate of 350 r / min for 1.5 h to obtain a reaction solution 3;
[0062] Step 5: Mix reaction solution 1, reaction solution 2 and reaction solution 3, and then stir the reaction at a temperature of 65°C and a stirring rate of 350r / min for 2.5 hours, then pour it into a mold and let it stand for 2.5 hours, then place it in a vacuum freeze dryer and freeze-dry it at a temperature of -60°C to obtain the environmentally friendly antibacterial sponge.
[0063] Embodiment 6:
[0064] See also Figure 1 As shown, this embodiment is a method for preparing an environmentally friendly antibacterial sponge, comprising the following steps:
[0065] Step 1: Weigh 6 parts of carboxymethyl chitosan, 2.5 parts of sodium alginate, 1.5 parts of polyethylene oxide, 0.25 parts of the potent antibacterial agent from Example 3, 0.03 parts of silver nitrate, 0.25 parts of 1-ethyl-(3-dimethylaminopropyl) carbodiimide hydrochloride, 0.16 parts of N-hydroxysuccinimide and 120 parts of deionized water according to weight parts for use; the molecular weight of the carboxymethyl chitosan is 9000Da, the viscosity of the sodium alginate is 200±20mPa·s, and the molecular weight of the polyethylene oxide is 2 million;
[0066] Step 2: adding carboxymethyl chitosan to 50% of the total weight of deionized water, and then stirring the mixture for 50 minutes at a temperature of 30° C. and a stirring rate of 400 r / min, adding polyethylene oxide and continuing to stir the mixture for 30 minutes, and then ultrasonically treating the mixture for 30 minutes at an ultrasonic power of 300 W to obtain a reaction solution 1;
[0067] Step 3: adding sodium alginate to 30% of the total weight of deionized water, stirring the mixture for 35 minutes at a temperature of 30° C. and a stirring rate of 400 r / min, and then ultrasonically treating the mixture for 15 minutes at an ultrasonic power of 300 W to obtain a reaction solution 2;
[0068] Step 4: adding a potent antibacterial agent, silver nitrate, 1-ethyl-(3-dimethylaminopropyl)carbodiimide hydrochloride and N-hydroxysuccinimide to the remaining deionized water, and then stirring the mixture at a temperature of 30° C. and a stirring rate of 400 r / min for 2 h to obtain a reaction solution 3;
[0069] Step 5: Mix reaction solution 1, reaction solution 2 and reaction solution 3, and then stir the reaction at a temperature of 70°C and a stirring rate of 400r / min for 3 hours, then pour it into a mold and let it stand for 3 hours, then place it in a vacuum freeze dryer and freeze-dry it at a temperature of -60°C to obtain the environmentally friendly antibacterial sponge.
[0070] Comparative Example 1:
[0071] This comparative example is a method for preparing an environmentally friendly antibacterial sponge, comprising the following steps:
[0072] Step 1: weigh 6 parts of carboxymethyl chitosan, 2.5 parts of sodium alginate, 1.5 parts of polyethylene oxide, 0.25 parts of 1-ethyl-(3-dimethylaminopropyl) carbodiimide hydrochloride, 0.16 parts of N-hydroxysuccinimide and 120 parts of deionized water according to weight parts for use; the molecular weight of the carboxymethyl chitosan is 9000Da, the viscosity of the sodium alginate is 200±20mPa·s, and the molecular weight of the polyethylene oxide is 2 million;
[0073] Step 2: adding carboxymethyl chitosan to 50% of the total weight of deionized water, and then stirring the mixture for 50 minutes at a temperature of 30° C. and a stirring rate of 400 r / min, adding polyethylene oxide and continuing to stir the mixture for 30 minutes, and then ultrasonically treating the mixture for 30 minutes at an ultrasonic power of 300 W to obtain a reaction solution 1;
[0074] Step 3: adding sodium alginate to 30% of the total weight of deionized water, stirring the mixture for 35 minutes at a temperature of 30° C. and a stirring rate of 400 r / min, and then ultrasonically treating the mixture for 15 minutes at an ultrasonic power of 300 W to obtain a reaction solution 2;
[0075] Step 4: adding 1-ethyl-(3-dimethylaminopropyl)carbodiimide hydrochloride and N-hydroxysuccinimide to the remaining deionized water, and then stirring the mixture at a temperature of 30° C. and a stirring rate of 400 r / min for 2 h to obtain a reaction solution 3;
[0076] Step 5: Mix reaction solution 1, reaction solution 2 and reaction solution 3, and then stir the reaction at a temperature of 70°C and a stirring rate of 400r / min for 3 hours, then pour it into a mold and let it stand for 3 hours, then place it in a vacuum freeze dryer and freeze-dry it at a temperature of -60°C to obtain the environmentally friendly antibacterial sponge.
[0077] Comparative Example 2:
[0078] This comparative example is a method for preparing an environmentally friendly antibacterial sponge, comprising the following steps:
[0079] Step 1: Weigh 6 parts of carboxymethyl chitosan, 2.5 parts of sodium alginate, 1.5 parts of polyethylene oxide, 0.03 parts of silver nitrate, 0.25 parts of 1-ethyl-(3-dimethylaminopropyl) carbodiimide hydrochloride, 0.16 parts of N-hydroxysuccinimide and 120 parts of deionized water according to weight parts for use; the molecular weight of the carboxymethyl chitosan is 9000Da, the viscosity of the sodium alginate is 200±20mPa·s, and the molecular weight of the polyethylene oxide is 2 million;
[0080] Step 2: adding carboxymethyl chitosan to 50% of the total weight of deionized water, and then stirring the mixture for 50 minutes at a temperature of 30° C. and a stirring rate of 400 r / min, adding polyethylene oxide and continuing to stir the mixture for 30 minutes, and then ultrasonically treating the mixture for 30 minutes at an ultrasonic power of 300 W to obtain a reaction solution 1;
[0081] Step 3: adding sodium alginate to 30% of the total weight of deionized water, stirring the mixture for 35 minutes at a temperature of 30° C. and a stirring rate of 400 r / min, and then ultrasonically treating the mixture for 15 minutes at an ultrasonic power of 300 W to obtain a reaction solution 2;
[0082] Step 4: Add silver nitrate, 1-ethyl-(3-dimethylaminopropyl)carbodiimide hydrochloride and N-hydroxysuccinimide to the remaining deionized water, and then stir the mixture at a temperature of 30° C. and a stirring rate of 400 r / min for 2 h to obtain a reaction solution 3;
[0083] Step 5: Mix reaction solution 1, reaction solution 2 and reaction solution 3, and then stir the reaction at a temperature of 70°C and a stirring rate of 400r / min for 3 hours, then pour it into a mold and let it stand for 3 hours, then place it in a vacuum freeze dryer and freeze-dry it at a temperature of -60°C to obtain the environmentally friendly antibacterial sponge.
[0084] Comparative Example 3:
[0085] This comparative example is a method for preparing an environmentally friendly antibacterial sponge, comprising the following steps:
[0086] Step 1: Weigh 6 parts of carboxymethyl chitosan, 2.5 parts of sodium alginate, 1.5 parts of polyethylene oxide, 0.25 parts of the potent antibacterial agent from Example 3, 0.25 parts of 1-ethyl-(3-dimethylaminopropyl) carbodiimide hydrochloride, 0.16 parts of N-hydroxysuccinimide and 120 parts of deionized water according to weight parts for use; the molecular weight of the carboxymethyl chitosan is 9000Da, the viscosity of the sodium alginate is 200±20mPa·s, and the molecular weight of the polyethylene oxide is 2 million;
[0087] Step 2: adding carboxymethyl chitosan to 50% of the total weight of deionized water, and then stirring the mixture for 50 minutes at a temperature of 30° C. and a stirring rate of 400 r / min, adding polyethylene oxide and continuing to stir the mixture for 30 minutes, and then ultrasonically treating the mixture for 30 minutes at an ultrasonic power of 300 W to obtain a reaction solution 1;
[0088] Step 3: adding sodium alginate to 30% of the total weight of deionized water, stirring the mixture for 35 minutes at a temperature of 30° C. and a stirring rate of 400 r / min, and then ultrasonically treating the mixture for 15 minutes at an ultrasonic power of 300 W to obtain a reaction solution 2;
[0089] Step 4: adding a potent antibacterial agent, 1-ethyl-(3-dimethylaminopropyl)carbodiimide hydrochloride and N-hydroxysuccinimide to the remaining deionized water, and then stirring the mixture at a temperature of 30° C. and a stirring rate of 400 r / min for 2 h to obtain a reaction solution 3;
[0090] Step 5: Mix reaction solution 1, reaction solution 2 and reaction solution 3, and then stir the reaction at a temperature of 70°C and a stirring rate of 400r / min for 3 hours, then pour it into a mold and let it stand for 3 hours, then place it in a vacuum freeze dryer and freeze-dry it at a temperature of -60°C to obtain the environmentally friendly antibacterial sponge.
[0091] The performance of the environmentally friendly antibacterial sponges of Examples 4-6 and Comparative Examples 1-3 was tested, and the test results are shown in the following table:
[0092]
[0093] See the table above and Figure 2It can be seen from the comparison between Examples 4-6 and Comparative Examples 1-3 that the addition of a strong antibacterial agent and silver nitrate can significantly improve the antibacterial properties of the environmentally friendly antibacterial sponge, among which the strong antibacterial agent has a better improvement effect, and when the two work synergistically, the environmentally friendly antibacterial sponge has excellent antibacterial properties, and the antibacterial rate can reach more than 99%.
[0094] In the description of this specification, the description with reference to the terms "one embodiment", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.
[0095] The above contents are merely examples and explanations of the present invention. Those skilled in the art may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the invention or exceed the scope defined by the claims, they shall all fall within the protection scope of the present invention.
Claims
1. A method for preparing an environmentally friendly antibacterial sponge, characterized in that: The following steps are involved: Step 1: weigh 4-6 parts of carboxymethyl chitosan, 2-2.5 parts of sodium alginate, 0.5-1.5 parts of polyethylene oxide, 0.05-0.25 parts of a potent antibacterial agent, 0.01-0.03 parts of silver nitrate, 0.2-0.25 parts of 1-ethyl-(3-dimethylaminopropyl)carbodiimide hydrochloride, 0.12-0.16 parts of N-hydroxysuccinimide and 100-120 parts of deionized water according to weight parts, and set aside; Step 2: adding carboxymethyl chitosan to 40-50% of the total weight of deionized water, and then stirring the mixture for 40-50 minutes at a temperature of 25-30° C. and a stirring rate of 300-400 r / min, adding polyethylene oxide and continuing to stir the mixture for 25-30 minutes, and then ultrasonically treating the mixture for 20-30 minutes at an ultrasonic power of 200-300 W to obtain a reaction solution 1; Step 3: adding sodium alginate to 25-30% of the total weight of deionized water, stirring the mixture for 30-35 minutes at a temperature of 25-30° C. and a stirring rate of 300-400 r / min, and then ultrasonically treating the mixture for 10-15 minutes at an ultrasonic power of 200-300 W to obtain a reaction solution 2; Step 4: adding a strong antibacterial agent, silver nitrate, 1-ethyl-(3-dimethylaminopropyl)carbodiimide hydrochloride and N-hydroxysuccinimide to the remaining deionized water, and then stirring the mixture for 1-2 hours at a temperature of 25-30° C. and a stirring rate of 300-400 r / min to obtain a reaction solution 3; Wherein, the potent antibacterial agent is prepared by the following steps: Step A1: 3-bromopyridine, ethyl 4-piperidinic acid ester, anhydrous potassium carbonate and N-methylpyrrolidone are added to a three-necked flask equipped with a stirrer and a thermometer, and stirred for 40-50 hours at a pressure of 0.50-0.55 MPa, a temperature of 180-185° C. and a stirring rate of 300-400 r / min. After the reaction is completed, the reaction product is cooled to room temperature, then centrifuged, and the precipitate is recrystallized with anhydrous methanol, and then placed in a vacuum drying oven and dried at a temperature of 50-55° C. for 2-3 hours to obtain intermediate 1; the amount ratio of 3-bromopyridine, ethyl 4-piperidinic acid ester, anhydrous potassium carbonate and N-methylpyrrolidone is 10 mmol: 10 mmol: 3-3.5 g: 30-35 mL; Step A2: Add intermediate 1, thionyl chloride and pyridine to a three-necked flask equipped with a stirrer and a thermometer, stir and react for 20-30 minutes at a temperature of 25-30° C. and a stirring rate of 300-400 r / min, then heat to 70-75° C. and continue stirring and reacting for 1.5-2 hours. After the reaction is completed, the reaction product is cooled to room temperature, and then the solvent is removed by rotary evaporation to obtain intermediate 2; the amount ratio of intermediate 1, thionyl chloride and pyridine is 10 mmol: 5-7 mL: 0.1-0.3 mL; Step A3: Add intermediate 2, hydroquinone and dichloromethane to a three-necked flask equipped with a stirrer, a thermometer and a reflux condenser, stir and react for 20-30 minutes at a temperature of 25-30°C and a stirring rate of 300-400r / min, then heat to reflux and continue stirring and reacting for 3-5 hours. After the reaction is completed, cool the reaction product to room temperature, then rotary evaporate to remove the solvent, then recrystallize with petroleum ether, and then place in a vacuum drying oven and dry for 1-1.5 hours at a temperature of 60-65°C to obtain intermediate 3; the amount ratio of intermediate 2, hydroquinone and dichloromethane is 20mmol:10mmol:50-60mL; Step A4: Add intermediate 3, benzyl bromide and anhydrous acetone to a three-necked flask equipped with a stirrer, a thermometer and a reflux condenser, stir and react for 20-30 hours at a temperature of 25-30° C. and a stirring rate of 300-400 r / min. After the reaction is completed, the reaction product is rotary evaporated to remove the solvent, and then recrystallized with anhydrous methanol, and then placed in a vacuum drying oven and dried at a temperature of 50-55° C. for 3-5 hours to obtain a potent antibacterial agent; the amount ratio of the intermediate 3, benzyl bromide and anhydrous acetone is 10mmol:45-55mmol:80-90mL; Step 5: Mix reaction solution 1, reaction solution 2 and reaction solution 3, and then stir the reaction at a temperature of 60-70°C and a stirring rate of 300-400r / min for 2-3 hours, then pour it into a mold and let it stand for 2-3 hours, then place it in a vacuum freeze dryer and freeze-dry it at a temperature of -60°C to obtain the environmentally friendly antibacterial sponge.
2. The method for preparing an environmentally friendly antibacterial sponge according to claim 1, characterized in that: The molecular weight of the carboxymethyl chitosan is 9000Da, the viscosity of the sodium alginate is 200±20mPa•s, and the molecular weight of the polyethylene oxide is 2 million.
3. An environmentally friendly antibacterial sponge, characterized in that: The environmentally friendly antibacterial sponge is prepared according to the method for preparing the environmentally friendly antibacterial sponge according to any one of claims 1-2.