Epoxy resin mixture for prepreg and preparation method and application thereof
By using liquid multifunctional epoxy resin and solid o-cresol epoxy resin in the prepreg, the interlayer defect problem of thick part molding under the non-hot press tank curing process is solved, and high efficiency is achieved , low-cost thickness forming and good surface cutting effect.
Patent Information
- Application Number
- CN202410212063.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-02-27
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2044-02-27
AI Technical Summary
In the prior art, epoxy resin for prepreg is prone to interlayer defects when the thickness of the part exceeds 5 mm under the non-hot press tank curing process, resulting in an increase in cost and cannot meet the needs of thick-piece molding and manufacturing.
Using a mixture of epoxy resins for prepregs, including liquid multifunctional epoxy resins, solid o-cresol epoxy resins, tougheners, fillers and coupling agents, to form a dense crosslinking structure through interaction, which is suitable for In the non-heat press tank curing process, the thickness of the parts can reach 10-30mm, and the sectional effect is good, and there are no defects such as pore bubbles.
It realizes efficient molding of the thickness of the part exceeding 5mm under the non-heat press tank curing process, with good cross-sectional effect, avoids interlayer defects, reduces costs, and improves the strength, temperature resistance and impact resistance of the material.
Smart Images

Figure CN118085500B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of epoxy resins, in particular to an epoxy resin mixture for prepregs and a preparation method and application thereof. Background Art
[0002] At present, high-performance epoxy resin-based carbon fiber composite materials are developing rapidly, and many high-performance parts need to use prepreg. As China's aerospace industry equipment exports participate in international competition, the manufacturing cost needs to be reduced. In order to reduce the cost of molding and curing, the OOA (non-autoclave curing) process is developing day by day. It has been gradually applied from ordinary civilian fields to aerospace and national defense fields. At present, the thickness of OOA parts after prepreg plying cannot exceed 5mm, otherwise there will be many interlayer defects. In order to solve the molding and manufacturing problems of some thick parts, the expensive autoclave process has to be used, which increases the cost of mass production.
[0003] Chinese patent CN115975346B discloses an epoxy resin premix for OOA curing prepreg and a preparation method thereof. The invention adopts a non-autoclave process (OOA) and the thickness of the product does not exceed 5 mm.
[0004] The Chinese patent with publication number CN116063819B discloses a medium-temperature curing epoxy resin premix and preparation method for unmanned aerial vehicle structural parts. The epoxy resin premix is composed of the following materials by weight: 20-40 parts of multifunctional epoxy resin, 10-20 parts of solid phenolic epoxy resin, 10-20 parts of toughening agent, and 5-10 parts of curing agent. The multifunctional epoxy resin is selected from one of MF-2133, MF-4230 or S-610. The solid phenolic epoxy resin is selected from one or more of NPCN-703, NPCN-704 or ECN-1273. In the invention, the material after the interaction reaction between the multifunctional epoxy resin, the solid phenolic epoxy resin and the curing agent dicyandiamide has high temperature resistance, and the glass transition temperature of the cured material can reach above 200°C. The end groups of the toughening agent gradually react and graft with the epoxy resin, so that it is evenly distributed after combining with the epoxy resin, and there will be no problems such as toughening agent aggregation and sedimentation. The grafting process will produce more macromolecular structures, which will gradually increase the viscosity of the premix, which is conducive to achieving the optimal viscosity of prepreg production. However, this patent is applied to the OOA process after the prepreg is laid, and the thickness of the product cannot exceed 5mm. This patent uses an autoclave process, which has external air pressure. The formula of this patent is not suitable for non-autoclave processes. If non-autoclave processes are used, it may cause prepreg materials with interlayer defects. Summary of the invention
[0005] The technical problem to be solved by the present invention is to provide an epoxy resin mixture for prepreg and a preparation method and application thereof in view of the shortcomings of the prior art. The prepared epoxy resin mixture is then used to prepare prepreg, and a non-autoclave curing process can be adopted. The thickness of the product exceeds 5mm and can reach 10-30mm, and the cross-section effect is good without defects such as pores and bubbles.
[0006] In order to solve the above technical problems, the technical solution adopted by the present invention is: an epoxy resin mixture for prepreg, comprising the following raw materials in parts by weight:
[0007] 20-40 parts of liquid multifunctional epoxy resin, 10-20 parts of solid o-cresol epoxy resin, 10-20 parts of toughening agent, 5-10 parts of filler, 1-3 parts of coupling agent, 10-20 parts of curing agent;
[0008] The number of epoxy groups in the liquid multifunctional epoxy resin is 3-4;
[0009] Preferably, the epoxy resin mixture for prepreg comprises the following raw materials in parts by weight: 20-30 parts of liquid multifunctional epoxy resin, 10-15 parts of solid o-cresol epoxy resin, 15-20 parts of toughening agent, 7.5-10 parts of filler, 1-3 parts of coupling agent, and 15-20 parts of curing agent.
[0010] The liquid multifunctional epoxy resin in the present invention includes multiple epoxy groups, which interact with solid o-cresol epoxy resin, toughening agent, filler, coupling agent and curing agent to obtain an epoxy resin mixture for prepreg, which can be used to prepare carbon fiber resin-based composite materials by non-autoclave curing process. The carbon fiber resin-based composite materials are prepared from prepreg, the thickness of the prepreg exceeds 5mm, and the cross-section effect is good without defects such as pores and bubbles.
[0011] The o-cresol-formaldehyde epoxy resin in the present invention has a moderate modulus and is suitable for being mixed with a liquid multifunctional epoxy resin for use.
[0012] In a preferred embodiment of the present invention, the viscosity of the liquid multifunctional epoxy resin at 25° C. needs to be lower than 3000 cps.
[0013] In a preferred embodiment of the present invention, the filler includes one or more of silicon micropowder, alumina powder and asbestos powder.
[0014] In a preferred embodiment of the present invention, the coupling agent comprises a first group and a second group;
[0015] The first group reacts with chemical groups on the surface of inorganic molecules, and the second group chemically reacts with organic molecules;
[0016] Preferably, the coupling agent includes one or both of Momentive Silquest A-1110 and BYK-C8001.
[0017] In a preferred embodiment of the present invention, the toughening agent includes a terminal carboxyl component;
[0018] Preferably, the toughening agent includes one or more of carboxyl-terminated nitrile rubber, nylon 6 powder and polylactic acid.
[0019] In a preferred embodiment of the present invention, the curing agent includes an amine group;
[0020] Preferably, the curing agent includes one or both of 4,4-DDS and 3,3-DDS.
[0021] In a preferred embodiment of the present invention, the solid o-cresol epoxy resin is composed of one or two of Nanya Electronics NPCN-701, NPCN-703, and NPCN-704;
[0022] The liquid multifunctional epoxy resin is composed of one or more of Huntsman MY0510, Mitsubishi Chemical TETRAD-X, and Hubei Zhenzhengfeng MF-4230.
[0023] The present invention also discloses a method for preparing the epoxy resin mixture for prepreg, comprising the following steps:
[0024] S1. Weighing: prepare liquid multifunctional epoxy resin, solid o-cresol epoxy resin, toughening agent, filler, coupling agent, and curing agent according to mass parts;
[0025] S2, preparing a resin mixture: heating a liquid multifunctional epoxy resin, continuing to add a solid o-cresol epoxy resin, keeping the mixture warm, and fully mixing and dissolving the mixture to obtain an epoxy resin solution;
[0026] S3. Add and mix various auxiliary agents: add toughening agent to the epoxy resin solution in S2, heat and mix to completely dissolve the toughening agent, and after cooling, add filler, coupling agent and curing agent, mix thoroughly and discharge the material.
[0027] In a preferred embodiment of the present invention, the heating temperature in S2 is 90-120°C;
[0028] The holding time in S2 is 30-60min;
[0029] The heating temperature in S3 is 90-120°C, and the heating and mixing time in S3 is 30-60 minutes;
[0030] The temperature after cooling in S3 is 60-80°C;
[0031] The mixing time after cooling in S3 is 15-30 minutes.
[0032] The present invention also discloses the use of the epoxy resin mixture for prepreg or the epoxy resin mixture prepared according to the preparation method in a carbon fiber resin-based composite material. The carbon fiber resin-based composite material adopts a non-autoclave curing process. The carbon fiber resin-based composite material is prepared from a prepreg, and the thickness of the prepreg exceeds 5 mm.
[0033] The Chinese patent with publication number CN116063819B adopts the autoclave process. The biggest difference between the non-autoclave process and the non-autoclave process is that there is no external air pressure like the autoclave. The patent does not contain fillers and coupling agents to fill the interlayer defects that may exist in the OOA process. If the autoclave process in the patent is replaced by the OOA process, it will cause interlayer pores in the prepreg.
[0034] Generally, in the absence of external pressure, the more layers a multilayer laminate has during the curing process, the more likely it is that gas will be difficult to discharge during the curing process or that pores will appear due to the internal stress of the reaction process, leading to defects in the laminate.
[0035] The present invention achieves the effect of preparing thick parts under the OOA process by selecting high-functionality resins (multifunctional epoxy resins, o-cresol epoxy resins), reactive toughening agents, fillers, coupling agents and other materials to interact with each other through high cross-linking, uniform distribution of components, pore filling and the like during the board curing process.
[0036] Compared with the prior art, the present invention has the following beneficial effects:
[0037] In the present invention, the multifunctional epoxy resin contains multiple epoxy groups, which can react with the curing agent to form a denser cross-linked structure, thereby improving the strength, modulus and temperature resistance of the epoxy resin. At the same time, more epoxy groups can also react with other active groups of substances in the mixture (such as terminal carboxyl groups in the toughening agent, nucleophilic groups and amine groups in the coupling agent) to achieve more cross-linking density, form a stable and uniform chemical bonding structure with other effective ingredients, and give full play to the effects of various reactive auxiliary agents. The 3-4 functional epoxy resins selected in the present invention are all resins with a viscosity lower than 3000cps at room temperature of 25°C, which is beneficial to the viscosity adjustment of the entire system, and the viscosity is not too high. The viscosity adjusted with other resins is more conducive to prepreg production.
[0038] Ortho-cresol epoxy resin is beneficial to increase the cross-linking density of the system, improve the temperature resistance, strength and corrosion resistance. At the same time, the combination of solid phenolic and liquid multifunctional epoxy resin can adjust the viscosity of the overall mixture to achieve a viscosity suitable for prepreg production (such as dry prepregs usually have a coating temperature between 60-90°C and a coating viscosity between 20,000-50,000cps).
[0039] Fillers can diffuse with epoxy resin through intermolecular forces and their smaller surface tension during the curing process to fill the defects of internal bubbles that are difficult to expel during the curing process of thicker epoxy resin prepregs. At the same time, they will improve the wear resistance and thermal stability of the premix and further enhance the impact resistance. Coupling agents are a class of substances with amphiphilic structures. Some of the groups in their molecules can react with the chemical groups on the inorganic surface to form chemical bonds, while the other groups have the property of being organic-philic and can react chemically with organic molecules or produce strong intermolecular effects, thereby connecting two materials with completely different properties. Firmly combined, the inorganic filler is dispersed more evenly in the epoxy resin mixture matrix, giving full play to the basic properties of the filler; the amine group in the curing agent reacts with the epoxy group in the epoxy resin to form a stable structure of a three-dimensional network, so that the epoxy resin is cured into a hard solid. The DDS curing agent used in the present invention can improve the strength, rigidity and corrosion resistance of the epoxy resin cured material; the toughening agent can improve the impact resistance of the resin system. The toughening agent in the present invention contains a terminal carboxyl component, which can be chemically bonded with the epoxy resin to form a stable cross-linked structure, giving full play to the toughening effect. Toughening agents without active groups cannot combine well with epoxy groups, affecting the toughening effect, and may cause uneven dispersion during the mixing process. BRIEF DESCRIPTION OF THE DRAWINGS
[0040] Figure 1 This is a physical picture of the epoxy resin mixture in Example 1.
[0041] Figure 2 10 mm laminate section made from prepreg made from epoxy resin and HF20 grade 220 gsm carbon fiber twill fabric in Example 1.
[0042] Figure 3 30mm laminate section made from prepreg made of epoxy resin and HF20 grade 220gsm carbon fiber twill fabric in Example 1.
[0043] Figure 4 10 mm laminate section made from prepreg made of epoxy resin and HF20 grade 220 gsm carbon fiber twill fabric in Example 2.
[0044] Figure 5 10 mm laminate section made from prepreg made of epoxy resin and HF20 grade 220 gsm carbon fiber twill fabric in Example 3.
[0045] Figure 6 This is a 10 mm laminate section made from prepreg made of epoxy resin and HF20 grade 220 gsm carbon fiber twill fabric in comparative example 1.
[0046] Figure 7 This is a 10 mm laminate section made from prepreg made of epoxy resin and HF20 grade 220 gsm carbon fiber twill fabric in comparative example 2.
[0047] Figure 8 This is a 10 mm laminate section made from prepreg made of epoxy resin and HF20 grade 220 gsm carbon fiber twill fabric in comparative example 3.
[0048] Fig. 9 This is a 10 mm laminate section made from prepreg made of epoxy resin and HF20 grade 220 gsm carbon fiber twill fabric in comparative example 4.
[0049] Fig.10 This is a 10 mm laminate section made from prepreg made from epoxy resin and HF20 grade 220 gsm carbon fiber twill fabric in comparative example 5. DETAILED DESCRIPTION
[0050] Example 1
[0051] The present invention is an epoxy resin mixture for prepreg, which is composed of the following raw materials by weight:
[0052] Liquid multifunctional epoxy resin: MY0510: 20 parts
[0053] o-Cresol epoxy resin: NPCN-701: 10 parts
[0054] Toughening agent: carboxyl-terminated nitrile rubber: 10 parts
[0055] Filler: Silica powder: 5 parts
[0056] Coupling agent: Silquest A-1110: 1 part
[0057] Curing agent: 4,4-DDS: 10 parts
[0058] Add the weighed liquid multifunctional epoxy resin into a disperser, heat to 90°C, add solid o-cresol epoxy resin, keep warm for 30 minutes, add toughening agent after it is fully dissolved, keep warm and mix for 30 minutes, cool to 60°C, add filler, coupling agent, and curing agent, keep 60°C for dispersion and mixing for 15 minutes, and discharge.
[0059] The main performance tests of the resin system are as follows:
[0060] Table 1 Performance test of the resin obtained in Example 1
[0061] Test items Test conditions / reference method Test Results Viscosity (75℃) ASTM D4287 26800cps Gel time (150℃) ASTM D2471 48min Tg (DSC method) GB / T 19466.2 215℃
[0062] The resin was made into a prepreg with a resin content of 43% using Hengshen HF20 grade 220gsm carbon fiber twill fabric, and the main mechanical properties of the laminated board obtained by OOA curing process (keeping warm at 180°C for 3 hours) are shown in Table 2 (the plying method of the test laminated board in the embodiment and comparative example is shown in Appendix 15):
[0063] Table 2 Mechanical properties of the laminated board obtained in Example 1
[0064] Test items Test conditions / reference method OOA Process Test Results 0° tensile strength ASTM D3039 695Mpa 0° tensile modulus ASTM D3039 68Gpa 90° tensile strength ASTM D3039 669Mpa 90° tensile modulus ASTM D3039 66Gpa 0° compression strength ASTM D6641 769Mpa 0° compression modulus ASTM D6641 59Gpa Bending Strength ASTM D790 880Mpa Flexural modulus ASTM D790 54Gpa Short beam shear strength ASTM D2344 90Mpa In-plane shear strength ASTM D3518 117Mpa In-plane shear modulus ASTM D3518 90Gpa
[0065] The prepreg was cured by OOA process to make a 10mm thick laminate. Figure 2 It can be seen that the cross-section effect is good, without defects such as pores and bubbles. Then the prepreg is cured by OOA process to make a 30mm laminate. The cross-section effect is shown in Figure 3 , it can be seen that the effect is still very good.
[0066] Example 2
[0067] The present invention is an epoxy resin mixture for prepreg, which is composed of the following raw materials by weight:
[0068] Liquid multifunctional epoxy resin: TETRAD-X: 40 parts
[0069] o-Cresol epoxy resin: NPCN-703: 20 parts
[0070] Toughening agent: Nylon 6 powder: 20 parts
[0071] Filler: Alumina powder: 10 parts
[0072] Coupling agent: BYK-C8001: 3 parts
[0073] Curing agent: 3,3-DDS: 20 parts
[0074] Add the weighed liquid multifunctional epoxy resin into a disperser, heat to 120°C, add solid o-cresol epoxy resin, keep warm for 60 minutes, add toughening agent after it is fully dissolved, keep warm and mix for 60 minutes, cool to 80°C, add filler, coupling agent and curing agent, keep 80°C for dispersion and mixing for 30 minutes, and discharge.
[0075] The main performance tests of the resin system are as follows:
[0076] Table 3 Performance test of the resin obtained in Example 2
[0077] Test items Test conditions / reference method Test Results Viscosity (75℃) ASTM D4287 30800cps Gel time (150℃) ASTM D2471 46min Tg (DSC method) GB / T 19466.2 212℃
[0078] The resin was made into a prepreg with a resin content of 43% using Hengshen HF20 grade 220gsm carbon fiber twill fabric. The main mechanical properties of the laminate obtained by OOA curing process (heat preservation at 180°C for 3 hours) are as follows:
[0079] Table 4 Mechanical properties of the laminated board prepared in Example 2
[0080] Test items Test conditions / reference method OOA Process Test Results 0° tensile strength ASTM D3039 692Mpa 0° tensile modulus ASTM D3039 69Gpa 90° tensile strength ASTM D3039 674Mpa 90° tensile modulus ASTM D3039 68Gpa 0° compression strength ASTM D6641 760Mpa 0° compression modulus ASTM D6641 62Gpa Bending Strength ASTM D790 899Mpa Flexural modulus ASTM D790 57Gpa Short beam shear strength ASTM D2344 92Mpa In-plane shear strength ASTM D3518 110Mpa In-plane shear modulus ASTM D3518 88Gpa
[0081] The prepreg was cured by OOA process to make a 10mm thick laminate. Figure 4 It can be seen that the cross-section effect is good, without defects such as pores and bubbles.
[0082] Embodiment 3
[0083] The present invention is an epoxy resin mixture for prepreg, which is composed of the following raw materials by weight:
[0084] Liquid multifunctional epoxy resin: MY0510: 10 parts, MF-4230: 10 parts
[0085] o-Cresol epoxy resin: NPCN-701: 7.5 parts, NPCN-704: 7.5 parts
[0086] Toughening agent: carboxyl-terminated nitrile rubber: 5 parts, nylon 6 powder: 5 parts, polylactic acid: 5 parts
[0087] Filler: 2.5 parts of silica powder, 2.5 parts of alumina powder, 2.5 parts of asbestos powder
[0088] Coupling agent: Silquest A-1110: 1 part, BYK-C8001: 1 part
[0089] Curing agent: 4,4-DDS: 7.5 parts, 3,3-DDS: 7.5 parts
[0090] Add the weighed liquid multifunctional epoxy resin into a disperser, heat to 105°C, add solid o-cresol epoxy resin, keep warm for 45 minutes, add toughening agent after it is fully dissolved, keep warm and mix for 45 minutes, cool to 70°C, add filler, coupling agent and curing agent, keep 70°C for dispersion and mixing for 23 minutes, and discharge.
[0091] The main performance tests of the resin system are as follows:
[0092] Table 5 Performance test of the resin obtained in Example 3
[0093] Test items Test conditions / reference method Test Results Viscosity (75℃) ASTM D4287 29800cps Gel time (150℃) ASTM D2471 49min Tg (DSC method) GB / T 19466.2 210℃
[0094] The resin was made into a prepreg with a resin content of 43% using Hengshen HF20 grade 220gsm carbon fiber twill fabric. The main mechanical properties of the laminate obtained by OOA curing process (heat preservation at 180°C for 3 hours) are as follows:
[0095] Table 6 Mechanical properties of the laminated board obtained in Example 3
[0096] Test items Test conditions / reference method OOA Process Test Results 0° tensile strength ASTM D3039 688Mpa 0° tensile modulus ASTM D3039 64Gpa 90° tensile strength ASTM D3039 668Mpa 90° tensile modulus ASTM D3039 69Gpa 0° compression strength ASTM D6641 760Mpa 0° compression modulus ASTM D6641 63Gpa Bending Strength ASTM D790 892Mpa Flexural modulus ASTM D790 55Gpa Short beam shear strength ASTM D2344 93Mpa In-plane shear strength ASTM D3518 121Mpa In-plane shear modulus ASTM D3518 86Gpa
[0097] The prepreg was cured by OOA process to make a 10mm thick laminate. Figure 5 It can be seen that the cross-section effect is good, without defects such as pores and bubbles.
[0098] Comparative Example 1
[0099] The present invention is an epoxy resin mixture for prepreg, which is composed of the following raw materials by weight:
[0100] Liquid bisphenol A epoxy resin: NPEL-128: 20 parts (replaced with general bisphenol A epoxy resin)
[0101] o-Cresol epoxy resin: NPCN-701: 10 parts
[0102] Toughening agent: carboxyl-terminated nitrile rubber: 10 parts
[0103] Filler: Silica powder: 5 parts
[0104] Coupling agent: Silquest A-1110: 1 part
[0105] Curing agent: 4,4-DDS: 10 parts
[0106] Add the weighed liquid multifunctional epoxy resin into a disperser, heat to 90°C, add solid o-cresol epoxy resin, keep warm for 30 minutes, add toughening agent after it is fully dissolved, keep warm and mix for 30 minutes, cool to 60°C, add filler, coupling agent, and curing agent, keep 60°C for dispersion and mixing for 15 minutes, and discharge.
[0107] The main performance tests of the resin system are as follows:
[0108] Table 7 Performance test of the resin obtained in Comparative Example 1
[0109] Test items Test conditions / reference method Test Results Viscosity (75℃) ASTM D4287 28200cps Gel time (150℃) ASTM D2471 53min Tg (DSC method) GB / T 19466.2 170℃
[0110] The resin was made into a prepreg with a resin content of 43% using Hengshen HF20 grade 220gsm carbon fiber twill fabric. The main mechanical properties of the laminate obtained by OOA curing process (heat preservation at 180°C for 3 hours) are as follows:
[0111] Table 8 Mechanical properties of the laminated board prepared in Comparative Example 1
[0112]
[0113]
[0114] After the liquid epoxy resin was replaced with bisphenol A epoxy resin, the glass transition temperature (Tg) decreased significantly, and at the same time, the mechanical properties of the laminate also decreased significantly.
[0115] The prepreg was cured by OOA process to make a 10mm thick laminate. Figure 6 , it can be seen that there are some tiny pores on the cross-section, and the lossless effect of the board is poor.
[0116] Comparative Example 2
[0117] The present invention is an epoxy resin mixture for prepreg, which is composed of the following raw materials by weight:
[0118] Liquid multifunctional epoxy resin: MY0510: 20 parts
[0119] o-Cresol epoxy resin: NPCN-701: 10 parts
[0120] Toughening agent: carboxyl-terminated nitrile rubber: 10 parts
[0121] Filler: Calcium carbonate: 5 parts
[0122] Coupling agent: Silquest A-1110: 1 part
[0123] Curing agent: 4,4-DDS: 10 parts
[0124] Add the weighed liquid multifunctional epoxy resin into a disperser, heat to 90°C, add solid o-cresol epoxy resin, keep warm for 30 minutes, add toughening agent after it is fully dissolved, keep warm and mix for 30 minutes, cool to 60°C, add filler, coupling agent, and curing agent, keep 60°C for dispersion and mixing for 15 minutes, and discharge.
[0125] The main performance tests of the resin system are as follows:
[0126] Table 9 Performance test of the resin obtained in Comparative Example 2
[0127] Test items Test conditions / reference method Test Results Viscosity (75℃) ASTM D4287 25500cps Gel time (150℃) ASTM D2471 49min Tg (DSC method) GB / T 19466.2 209℃
[0128] The resin was made into a prepreg with a resin content of 43% using Hengshen HF20 grade 220gsm carbon fiber twill fabric. The main mechanical properties of the laminate obtained by OOA curing process (heat preservation at 180°C for 3 hours) are as follows:
[0129] Table 10 Mechanical properties of the laminated board prepared in Comparative Example 2
[0130]
[0131]
[0132] When calcium carbonate, another filler, is used, the compression and bending properties of the laminate are significantly reduced.
[0133] The prepreg was cured by OOA process to make a 10mm thick laminate. Figure 7 It can be seen that there are many continuous large pores on the cross-section, and the lossless effect of the board is poor.
[0134] Comparative Example 3
[0135] The present invention is an epoxy resin mixture for prepreg, which is composed of the following raw materials by weight:
[0136] Liquid multifunctional epoxy resin: MY0510: 20 parts
[0137] o-Cresol epoxy resin: NPCN-701: 10 parts
[0138] Toughening agent: carboxyl-terminated nitrile rubber: 10 parts
[0139] Filler: Silica powder: 5 parts
[0140] Coupling agent: KH-550: 1 part (replace general silane coupling agent)
[0141] Curing agent: 4,4-DDS: 10 parts
[0142] Add the weighed liquid multifunctional epoxy resin into a disperser, heat to 90°C, add solid o-cresol epoxy resin, keep warm for 30 minutes, add toughening agent after it is fully dissolved, keep warm and mix for 30 minutes, cool to 60°C, add filler, coupling agent, and curing agent, keep 60°C for dispersion and mixing for 15 minutes, and discharge.
[0143] The main performance tests of the resin system are as follows:
[0144] Table 11 Performance test of the resin obtained in Comparative Example 3
[0145] Test items Test conditions / reference method Test Results Viscosity (75℃) ASTM D4287 28000cps Gel time (150℃) ASTM D2471 47min Tg (DSC method) GB / T 19466.2 212℃
[0146] The resin was made into a prepreg with a resin content of 43% using Hengshen HF20 grade 220gsm carbon fiber twill fabric. The main mechanical properties of the laminate obtained by OOA curing process (heat preservation at 180°C for 3 hours) are as follows:
[0147] Table 12 Mechanical properties of the laminated board prepared in Comparative Example 3
[0148] Test items Test conditions / reference method OOA Process Test Results 0° tensile strength ASTM D3039 700Mpa 0° tensile modulus ASTM D3039 63Gpa 90° tensile strength ASTM D3039 680Mpa 90° tensile modulus ASTM D3039 65Gpa 0° compression strength ASTM D6641 690Mpa 0° compression modulus ASTM D6641 40Gpa Bending Strength ASTM D790 680Mpa Flexural modulus ASTM D790 59Gpa Short beam shear strength ASTM D2344 85Mpa In-plane shear strength ASTM D3518 60Mpa In-plane shear modulus ASTM D3518 70Gpa
[0149] After the coupling agent was replaced, the mechanical properties of the laminate part decreased significantly, especially the in-plane shear strength, which was only half of the previous level.
[0150] The coupling agent of the present application includes a first group and a second group; the first group reacts with a chemical group on the surface of an inorganic molecule, and the second group reacts chemically with an organic molecule. Compared with the silane coupling agent in the comparative example, the coupling agent selected in the present application has an unexpected effect.
[0151] The prepreg was cured by OOA process to make a 10mm thick laminate. Figure 8 It can be seen that there are many tiny pores on the cross-section, and the lossless effect of the board is poor.
[0152] Comparative Example 4
[0153] The present invention is an epoxy resin mixture for prepreg, which is composed of the following raw materials by weight:
[0154] Liquid multifunctional epoxy resin: MY0510: 20 parts
[0155] o-Cresol epoxy resin: NPCN-701: 10 parts
[0156] Toughening agent: carboxyl-terminated nitrile rubber: 10 parts
[0157] Filler: Silica powder: 5 parts
[0158] Coupling agent: Silquest A-1110: 1 part
[0159] Curing agent: dicyandiamide: 5 parts (change the type of curing agent)
[0160] Add the weighed liquid multifunctional epoxy resin into a disperser, heat to 90°C, add solid o-cresol epoxy resin, keep warm for 30 minutes, add toughening agent after it is fully dissolved, keep warm and mix for 30 minutes, cool to 60°C, add filler, coupling agent, and curing agent, keep 60°C for dispersion and mixing for 15 minutes, and discharge.
[0161] The main performance tests of the resin system are as follows:
[0162] Table 13 Performance test of the resin obtained in Comparative Example 4
[0163] Test items Test conditions / reference method Test Results Viscosity (75℃) ASTM D4287 27300cps Gel time (150℃) ASTM D2471 42min Tg (DSC method) GB / T 19466.2 190℃
[0164] The resin was made into a prepreg with a resin content of 43% using Hengshen HF20 grade 220gsm carbon fiber twill fabric. The main mechanical properties of the laminate obtained by OOA curing process (heat preservation at 180°C for 3 hours) are as follows:
[0165] Table 14 Mechanical properties of the laminated board prepared in Comparative Example 4
[0166] Test items Test conditions / reference method OOA Process Test Results 0° tensile strength ASTM D3039 685Mpa 0° tensile modulus ASTM D3039 59Gpa 90° tensile strength ASTM D3039 660Mpa 90° tensile modulus ASTM D3039 58Gpa 0° compression strength ASTM D6641 773Mpa 0° compression modulus ASTM D6641 48Gpa Bending Strength ASTM D790 888Mpa Flexural modulus ASTM D790 44Gpa Short beam shear strength ASTM D2344 88Mpa In-plane shear strength ASTM D3518 114Mpa In-plane shear modulus ASTM D3518 78Gpa
[0167] After the curing agent was replaced, the glass transition temperature (Tg) and the modulus of various mechanical properties of the laminate decreased.
[0168] The prepreg was cured by OOA process to make a 10mm thick laminate. Fig. 9 It can be seen that the cross-section effect is worse than that of comparative examples 1, 2, and 3, but there are still a small amount of pores, which is not as good as that of embodiments 1, 2, and 3.
[0169] Comparative Example 5
[0170] The present invention is an epoxy resin mixture for prepreg, which is composed of the following raw materials by weight:
[0171] Liquid multifunctional epoxy resin: MY0510: 20 parts
[0172] o-Cresol epoxy resin: NPCN-701: 10 parts
[0173] Toughener: High-density polyethylene HDPE: 10 parts (replace toughener)
[0174] Filler: Silica powder: 5 parts
[0175] Coupling agent: Silquest A-1110: 1 part
[0176] Curing agent: 4,4-DDS: 10 parts
[0177] Add the weighed liquid multifunctional epoxy resin into a disperser, heat to 90°C, add solid o-cresol epoxy resin, keep warm for 30 minutes, add toughening agent after it is fully dissolved, keep warm and mix for 30 minutes, cool to 60°C, add filler, coupling agent, and curing agent, keep 60°C for dispersion and mixing for 15 minutes, and discharge.
[0178] The main performance tests of the resin system are as follows:
[0179] Table 15 Performance test of the resin obtained in Comparative Example 5
[0180] Test items Test conditions / reference method Test Results Viscosity (75℃) ASTM D4287 32300cps Gel time (150℃) ASTM D2471 42min Tg (DSC method) GB / T 19466.2 182℃
[0181] The resin was made into a prepreg with a resin content of 43% using Hengshen HF20 grade 220gsm carbon fiber twill fabric. The main mechanical properties of the laminate obtained by OOA curing process (heat preservation at 180°C for 3 hours) are as follows:
[0182] Table 16 Mechanical properties of the laminated board prepared in Comparative Example 5
[0183]
[0184]
[0185] After replacing the toughening agent with one without active groups, the glass transition temperature (Tg) and the modulus of various mechanical properties of the laminate decreased significantly.
[0186] The prepreg was cured by OOA process to make a 10mm thick laminate. Fig.10 It can be seen that the cross-section effect not only has some pores, but also has a small amount of uneven aggregation of toughening agent powder, which is not as good as Examples 1, 2, and 3.
[0187] Table 17 Laying of HF20 grade 220gsm carbon fiber twill fabric prepreg molding test laminate
[0188] Test items Laying method Number of layers Warp stretch <![CDATA[[(0 / 90)] 5s ]]> 10 Weft stretch <![CDATA[[(0 / 90)] 5s ]]> 10 Warp Compression <![CDATA[[(0 / 90)] 4s ]]> 8 Warp bending <![CDATA[[(0 / 90)] 4s ]]> 8 Short beam shear <![CDATA[[(0 / 90)] 4s ]]> 8 In-plane shear <![CDATA[[(45 / -45)] 5s ]]> 10
Claims
1. An epoxy resin mixture for prepreg, characterized in that The invention comprises the following raw materials in parts by weight: 20-40 parts of liquid multifunctional epoxy resin, 10-20 parts of solid o-cresol epoxy resin, 10-20 parts of toughening agent, 5-10 parts of filler, 1-3 parts of coupling agent, 10-20 parts of curing agent; The number of epoxy groups in the liquid multifunctional epoxy resin is 3-4; The viscosity of the liquid multifunctional epoxy resin at 25°C must be lower than 3000cps; The liquid multifunctional epoxy resin is composed of one or two of Huntsman MY0510, Mitsubishi Chemical TETRAD-X, and Hubei Zhenzhengfeng MF-4230; The coupling agent includes a first group and a second group; The first group reacts with chemical groups on the surface of inorganic molecules, and the second group chemically reacts with organic molecules; The coupling agent includes one or two of Momentive Silquest A-1110 and BYK-C8001; The toughening agent includes a terminal carboxyl component; The filler includes one or more of silicon powder, alumina powder and asbestos powder; The curing agent includes one or both of 4,4-DDS and 3,3-DDS.
2. The epoxy resin mixture for prepreg according to claim 1, characterized in that: The toughening agent includes carboxyl-terminated nitrile rubber and one or more of nylon 6 powder and polylactic acid.
3. The epoxy resin mixture for prepreg according to any one of claims 1-2, characterized in that: The solid o-cresol epoxy resin is composed of one or two of Nanya Electronics NPCN-701, NPCN-703 and NPCN-704.
4. The epoxy resin mixture for prepreg according to any one of claims 1-2, characterized in that: The epoxy resin mixture for prepreg comprises the following raw materials in parts by weight: 20-30 parts of liquid multifunctional epoxy resin, 10-15 parts of solid o-cresol epoxy resin, 15-20 parts of toughening agent, 7.5-10 parts of filler, 1-3 parts of coupling agent and 15-20 parts of curing agent.
5. A method for preparing the epoxy resin mixture for prepreg according to any one of claims 1 to 4, characterized in that: The steps include: S1. Weighing: Prepare liquid multifunctional epoxy resin, solid o-cresol epoxy resin, toughening agent, filler, coupling agent, and curing agent according to mass parts; S2, preparing a resin mixture: heating a liquid multifunctional epoxy resin, continuing to add a solid o-cresol epoxy resin, keeping the mixture warm, and fully mixing and dissolving the mixture to obtain an epoxy resin solution; S3. Add and mix various auxiliary agents: add toughening agent to the epoxy resin solution in S2, heat and mix to completely dissolve the toughening agent, and after cooling, add filler, coupling agent and curing agent, mix thoroughly and discharge the material.
6. The method for preparing the epoxy resin mixture for prepreg according to claim 5, characterized in that: The heating temperature in S2 is 90-120°C; The holding time in S2 is 30-60min; The heating and mixing temperature in S3 is 90-120°C, and the heating and mixing time in S3 is 30-60 minutes; The temperature after cooling in S3 is 60-80°C; The mixing time after cooling in S3 is 15-30 minutes.
7. Use of the epoxy resin mixture for prepreg according to any one of claims 1 to 4 or the epoxy resin mixture prepared by the preparation method according to claim 5 or 6 in a carbon fiber resin-based composite material, characterized in that: The carbon fiber resin-based composite material adopts a non-autoclave curing process, and the carbon fiber resin-based composite material is made of prepreg, and the thickness of the prepreg exceeds 5 mm.
Citation Information
Patent Citations
An epoxy resin premix for OOA-cured prepreg and its preparation method
CN115975346B
A medium-temperature curing epoxy resin premix for UAV structural components and its preparation method
CN116063819B
High temperature-resistant epoxy resin for composite material prepreg, and synthesis technology thereof
CN110128785A
Halogen-free copper-clad plate for automotive electronic material, and preparation method and application of halogen-free copper-clad plate
CN113290981A
Epoxy resin composition for OOA process and preparation method of composite material of epoxy resin composition
CN114230973A