A high temperature oxidation resistant composite coating on the surface of a nuclear zirconium alloy and a preparation method thereof
By first preparing a Cr-N transition layer on the surface of the zirconium alloy and then depositing the FeCrAl coating to form a Cr-N/FeCrAl composite coating, the problem of hydrogen and heat generated by the reaction of the zirconium alloy surface with water vapor at high temperatures is solved, and the resistance is improved. Oxidizing properties and reducing the columnar crystal structure, enhancing accident tolerance.
Patent Information
- Application Number
- CN202410259671.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-03-07
- Publication Date
- 2024-10-08
- Estimated Expiration
- 2044-03-07
AI Technical Summary
The surface of zirconium alloy reacts with water vapor at high temperatures to produce hydrogen and heat, which increases the risk of nuclear leakage. The performance of the existing FeCrAl coating attenuates at high temperatures and the columnar crystal structure is not ideal, affecting the oxidation resistance.
A Cr-N transition layer is first prepared on the zirconium alloy substrate, and then the FeCrAl coating is deposited. The Fe-Zr eutectic reaction is prevented through the AlN diffusion barrier layer and the Zr2N twin layer, and the columnar crystal structure of the FeCrAl layer is reduced to form Cr-N/ FeCrAl composite coating to improve oxidation resistance.
It effectively prevents the Fe-Zr eutectic reaction, reduces the columnar crystal structure of the FeCrAl coating, improves the high-temperature oxidation resistance of the zirconium alloy surface, reduces the oxidation weight gain by 56.9%, and enhances the accident tolerance rate.
Smart Images

Figure CN118086848B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of nuclear power metal coatings, and in particular to a high-temperature oxidation resistant composite coating on the surface of a nuclear zirconium alloy and a preparation method thereof. Background Art
[0002] Zirconium alloy is the preferred material for nuclear fuel cladding due to its good nuclear performance. However, in the event of a Loss of Coolant Accident (LOCA), the temperature of the zirconium alloy cladding material will quickly rise to over 1000°C and react with high-temperature water vapor to produce a large amount of hydrogen and heat. When the temperature is greater than 1200°C, the core will melt and the risk of hydrogen explosion will increase, leading to nuclear leakage.
[0003] Depositing high-temperature anti-oxidation coating on the surface of zirconium alloy has the advantages of short R&D cycle and good adaptability to the production process of zirconium alloy cladding tubes, and has become an important means to improve the accident tolerance of zirconium alloy in the short term. At present, the research on zirconium alloy surface coatings mainly focuses on pure metal coatings, ceramic coatings, alloy coatings and composite coatings. The metal FeCrAl coating shows excellent performance in resistance to high-temperature and high-pressure water corrosion, thermal shock resistance and reduction of hydrogen release, and is a potential candidate material. While improving the accident tolerance of the cladding tube, it does not significantly reduce the neutron economy of the fuel cladding tube, and maintains the existing thermal environment in the reactor to the maximum extent; and takes into account the compatibility of zirconium alloy and fuel fission products.
[0004] Magnetron sputtering is the most widely used chromium coating preparation technology, and the DC magnetron sputtering technology is currently widely used. Although the FeCrAl coating prepared by magnetron sputtering has the characteristics of good coating uniformity and stable process, when the FeCrAl coating is prepared on the surface of Zr alloy, a serious Fe-Zr eutectic reaction will occur when the temperature reaches 928°C, resulting in serious degradation of the coating performance and affecting the coating's antioxidant properties. In addition, the coating columnar crystals and porosity need to be improved to meet the use requirements. Summary of the invention
[0005] Based on the above technical problems, the purpose of the present invention is to provide a method for preparing a high-temperature oxidation resistant composite coating on the surface of a nuclear zirconium alloy. By introducing a Cr-N transition layer between the zirconium alloy substrate and the FeCrAl coating, the oxidation resistance of the FeCrAl coating is improved, and the columnar crystal structure of the FeCrAl coating is reduced, thereby improving the accident tolerance rate of the coating.
[0006] Another object of the present invention is to provide a high temperature oxidation resistant composite coating on the surface of the nuclear zirconium alloy.
[0007] The purpose of the present invention is achieved through the following technical solutions:
[0008] A method for preparing a high-temperature oxidation resistant composite coating on the surface of a nuclear zirconium alloy is characterized in that a Cr-N transition layer is first prepared on the surface of a zirconium alloy substrate by magnetron sputtering, and then a FeCrAl coating is prepared on the surface of the transition layer to form a CN / FeCrAl composite coating.
[0009] Furthermore, the deposition temperature for preparing the Cr-N transition layer is 250-350°C, the Cr target power is 240-260W, the deposition pressure is 0.3-0.5Pa, the N2 flow rate is 2-10sccm, the bias voltage is 8-12V, the rotating frame speed is 6-10rpm, the time is 6-8h, and the N content in the Cr-N transition layer is controlled to be 15-18at.%.
[0010] Furthermore, the deposition temperature for preparing the FeCrAl coating is 450-550°C, the CrAl alloy target power is 120-180W, the Fe target power is 280-320W, the deposition pressure is 0.3-0.5Pa, the bias voltage is 60-80V, the rotating frame speed is 6-10rpm, and the time is 2-3h.
[0011] Furthermore, the zirconium alloy substrate is pretreated before preparing the coating. Specifically, the surface of the zirconium alloy is polished with 100#, 400#, 1000#, and 2000# sandpaper in sequence. The polished zirconium alloy substrate is polished with a diamond polishing liquid with a particle size of 1.5μm and a silica suspension with a particle size of 0.06μm in sequence, and then ultrasonically cleaned with acetone and anhydrous ethanol for 10 minutes and then blown dry for use.
[0012] Furthermore, the pretreated zirconium alloy substrate needs to be ion cleaned, specifically, the zirconium alloy substrate is placed in a magnetron sputtering coating furnace, and when the vacuum degree reaches 8×10 -4 When 400 Pa was used, Ar was introduced, the bias voltage was adjusted to 420-480 V, the power was 280-320 W, and the treatment time was 8-15 min.
[0013] In the present invention, N element is introduced, and an AlN diffusion barrier layer is formed in situ at the Cr-N / FeCrAl interface in a high temperature environment, which can block the diffusion of Fe element to the inside; and the Zr2N twin layer is formed in situ at the Zr / Cr-N interface, which can greatly slow down the external diffusion of Zr element. Through the independent cooperation of the two interfaces, the Fe-Zr eutectic reaction is effectively prevented. In addition, by preparing an amorphous Cr-N coating on the surface of the substrate, the template effect can be suppressed, the growth effect of the columnar crystals of the FeCrAl layer can be reduced, and the fast channel for O2 to enter the zirconium alloy substrate can be blocked. By regulating the FeCrAl coating with a specific element ratio, a continuous and dense Al2O3 oxide layer can be quickly formed in a high temperature environment, which hinders the continuous invasion of O2, and further improves the high temperature oxidation resistance of the FeCrAl coating.
[0014] Most specifically, a method for preparing a high temperature oxidation resistant coating on the surface of a nuclear zirconium alloy is characterized by comprising the following steps:
[0015] (1) Matrix pretreatment: Specifically, the surface of the zirconium alloy was polished with 100#, 400#, 1000#, and 2000# sandpaper in sequence, and the polished zirconium alloy matrix was polished with a diamond polishing liquid with a particle size of 1.5μm and a silica suspension with a particle size of 0.06μm in sequence, and then ultrasonically cleaned with acetone and anhydrous ethanol for 10 minutes and then blown dry for use;
[0016] (2) Sample loading and cleaning: Place the zirconium alloy substrate into the magnetron sputtering coating furnace chamber. When the vacuum degree in the furnace reaches 8×10 - 4 When the pressure is 0.04 Pa, Ar is introduced, the bias voltage is adjusted to 420-480 V, the power is 280-320 W, and the treatment time is 8-15 min;
[0017] (3) Deposition of Cr-N transition layer: Cr target was used as the sputtering target, the deposition temperature was 250-350°C, the Cr target power was 240-260W, the deposition pressure was 0.3-0.5Pa, the N2 flow rate was 2-10sccm, the bias voltage was 8-12V, the rotating frame speed was 6-10rpm, the time was 6-8h, and the N content in the Cr-N transition layer was controlled to be 15-18at.%;
[0018] (4) Deposition of FeCrAl coating: high purity Fe target and CrAl alloy target were used as sputtering targets, the deposition temperature was 450~550℃, the CrAl alloy target power was 120~180W, the Fe target power was 280~320W, the deposition pressure was 0.3~0.5Pa, the bias voltage was 60~80V, the rotating frame speed was 6~10rpm, and the time was 2~3h.
[0019] A high temperature oxidation resistant composite coating on the surface of a nuclear zirconium alloy, characterized in that the composite coating comprises a Cr-N transition layer and a FeCrAl coating, wherein the N content in the Cr-N transition layer is 15-18 at.%, and the Al content in the FeCrAl coating is 15-22 at.%.
[0020] Furthermore, the Cr-N transition layer is prepared by magnetron sputtering, with a deposition temperature of 250~350°C, a Cr target power of 240~260W, a deposition pressure of 0.3~0.5Pa, a N2 flow rate of 2~10sccm, a bias voltage of 8~12V, a rotating frame speed of 6~10rpm, and a time of 6~8h.
[0021] Furthermore, the FeCrAl coating is prepared by magnetron sputtering with Fe target and CrAl alloy target as sputtering target, with a specific deposition temperature of 450-550°C, a CrAl alloy target power of 120-180W, a Fe target power of 280-320W, a deposition pressure of 0.3-0.5Pa, a bias voltage of 60-80V, a rotating frame speed of 6-10rpm, and a time of 2-3h.
[0022] The present invention has the following technical effects:
[0023] In the present invention, when preparing the FeCrAl oxidation resistant coating on the surface of the zirconium alloy substrate, Cr-N is first prepared as a transition layer, and a continuous AlN diffusion barrier layer is formed in situ at the Cr-N / FeCrAl interface under a high temperature environment to block the diffusion of Fe elements to the inside, and a Zr2N twin layer is formed in situ at the Zr / Cr-N interface, which can greatly slow down the external diffusion of Zr elements, effectively prevent the Fe-Zr eutectic reaction, and reduce the columnar crystal structure of the FeCrAl coating, thereby improving the oxidation resistance of the coating. The oxidation weight gain of the zirconium alloy prepared with the Cr-N / FeCrAl composite coating under 1200°C steam is reduced by 56.9% compared with the zirconium alloy. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 : Surface cross-sectional morphology of the magnetron sputtering deposited Cr-N / FeCrAl composite coating of the present invention.
[0025] Figure 2 : Surface cross-sectional morphology and EDS spectrum of Cr-N / FeCrAl composite coating after oxidation in 1200℃ high temperature steam environment for 30min.
[0026] Figure 3 : TEM microscopic characterization of Cr-N / FeCrAl coating after oxidation in high temperature steam environment at 1200℃ for 30min.
[0027] Figure 4 : Oxidation weight gain and XRD patterns of Cr-N / FeCrAl composite coating in high temperature steam environment. DETAILED DESCRIPTION
[0028] The present invention is described in detail below through examples. It is necessary to point out that the following examples are only used to further illustrate the present invention and cannot be understood as limiting the scope of protection of the present invention. Those skilled in the art can make some non-essential improvements and adjustments to the present invention based on the above-mentioned contents of the present invention.
[0029] Example 1
[0030] A method for preparing a high temperature oxidation resistant coating on the surface of a nuclear zirconium alloy comprises the following steps:
[0031] (1) Matrix pretreatment: Specifically, the surface of the zirconium alloy was polished with 100#, 400#, 1000#, and 2000# sandpaper in sequence, and the polished zirconium alloy matrix was polished with a diamond polishing liquid with a particle size of 1.5μm and a silica suspension with a particle size of 0.06μm in sequence, and then ultrasonically cleaned with acetone and anhydrous ethanol for 10 minutes and then blown dry for use;
[0032] (2) Sample loading and cleaning: Place the zirconium alloy substrate into the magnetron sputtering coating furnace chamber. When the vacuum degree in the furnace reaches 8×10 - 4 When Pa, Ar was introduced, the bias voltage was adjusted to 450 V, the power was 300 W, and the treatment time was 10 min;
[0033] (3) Deposition of Cr-N transition layer: Cr target was used as the sputtering target, the deposition temperature was 300°C, the Cr target power was 250 W, the deposition pressure was 0.4 Pa, the N2 flow rate was 2 sccm, the bias voltage was 10 V, the rotating frame speed was 8 rpm, the time was 7 h, and the N content in the prepared Cr-N transition layer was 15.48 at.%, and the thickness of the Cr-N transition layer was 5.42 μm;
[0034] (4) Deposition of FeCrAl coating: High-purity Fe target and CrAl alloy target were used as sputtering targets, the deposition temperature was 500°C, the CrAl target power was 150 W, the Fe target power was 300 W, the deposition pressure was 0.4 Pa, the bias voltage was 70 V, the spindle speed was 8 rpm, the time was 2.5 h, and the Al content in the prepared FeCrAl coating was 16.31%, and the thickness of the FeCrAl coating was 7.12 μm.
[0035] Figure 1 This is a cross-sectional morphology of the magnetron sputtering deposited Cr-N / FeCrAl composite coating of this embodiment. The figure shows the cross-sectional morphology and EDS spectrum of the deposited Cr-N / FeCrAl composite coating on the surface of zirconium alloy. Figure 1 (a) Surface morphology of the composite coating. As shown in the figure, the grains on the surface of the FeCrAl layer are typical "triangular prisms", but the intergranular spacing of the columnar crystals is significantly reduced, the structure is uniform and dense, and the Fe-Cr-Al element composition is Fe-13.48Cr-16.31Al (at.%). Figure 1As shown in (b) and (c), the cross-sectional morphology of the Cr-N / FeCrAl coating is shown. The interfaces of Cr-N / FeCrAl and Zr / Cr-N are flat and well bonded. The element composition of the Cr-N layer is Cr-15.48Al (at.%). The average thickness of the Cr-N / FeCrAl composite coating is about 12.5 ± 0.2 μm, the thickness of the Cr-N layer is about 5.4 ± 0.2 μm, and the thickness of the FeCrAl layer is about 7.1 ± 0.2 μm. The cross-sectional morphology shows that the Cr-N layer is amorphous. Under the influence of its template effect, the surface density of the FeCrAl layer is high, and the intergranular gap of the FeCrAl columnar crystals is reduced, which has a mitigating effect on the negative impact of the FeCrAl columnar crystals.
[0036] The substrate prepared with the Cr-N / FeCrAl composite coating in Example 1 was placed in a high-temperature steam environment at 1200°C for oxidation resistance test. The cross-sectional morphology and EDS spectrum after oxidation for 30 minutes were as follows: Figure 2 shown. Figure 2 The results show that after steam oxidation at 1200 ℃, a continuous and dense Al2O3 oxide layer is formed on the surface of the Cr-N / FeCrAl composite coating on the zirconium alloy surface, and its thickness is about 549 ± 50 nm. The cross-sectional morphology shows that there is a thin Zr-Cr-N diffusion layer at the Zr / Cr-N interface, which is about 670 ± 20nm, but the point scanning at P2-5 shows that the oxygen content inside the composite coating is low. After oxidation, the coating structure is very complete, and there is no sign of inward diffusion of Fe elements, and the rate of outward diffusion of Zr elements is slow, indicating that the Cr-N barrier layer can effectively prevent the Fe-Zr eutectic reaction and can effectively improve the high-temperature oxidation resistance of zirconium alloy.
[0037] The TEM spectrum of the oxidized Cr-N / FeCrAl composite coating is shown in Figure 3 As shown. After oxidation in a steam environment at 1200 °C for 30 min, a continuous Al-N-rich coating with a thickness of about 70 ± 20 nm was formed in situ at the Cr-N / FeCrAl interface of the composite coating. Combined with the SAED results, it was confirmed that its phase was AlN. During the oxidation process, a Zr-N diffusion layer crystalline layer was formed in situ at the Zr / Cr-N interface with a thickness of about 264 ± 25 nm. SAED confirmed that the Zr-N diffusion layer crystalline layer was composed of Zr2N phase, and Zr-4 matrix was still Zr, and no oxidation reaction occurred, indicating that the preparation of Cr-N / FeCrAl composite coating on the surface of zirconium alloy can greatly protect the zirconium matrix in a high-temperature steam environment.
[0038] When preparing the coating, as the thickness of the composite coating increases, the high temperature oxidation resistance of the composite coating will gradually increase.
[0039] Comparative Example 1
[0040] According to the preparation process of Example 1, a Cr / FeCrAl composite coating was prepared on the surface of the zirconium alloy substrate, except that N2 was not introduced when the Cr coating was prepared.
[0041] A Cr coating was prepared as a transition layer on the surface of the FeCrAl coating and the substrate. It was found that Fe and Cr would dissolve each other, and Cr could not prevent Zr from diffusing outward. Therefore, it could not effectively prevent the Fe in the FeCrAl coating and the substrate from undergoing the Fe-Zr eutectic reaction, resulting in unsatisfactory antioxidant properties of the coating.
[0042] The composite coatings prepared in Example 1, Comparative Example 1 and Comparative Example 2 were subjected to oxidation weight gain tests in a high-temperature steam environment. The test results are as follows: Figure 4 As shown in (a), after steam oxidation at different temperatures (1000, 1100, 1200 °C) for 30 min, the weight gain per unit area (ΔW / A) of the samples on the surface of the zirconium alloy Cr-N / FeCrAl coating, Cr / FeCrAl coating and Zry-4 alloy is 1.96 mg / cm 2 , 3.02 mg / cm 2 and 11.34 mg / cm 2 (Cr-N / FeCrAl coating); 3.79 mg / cm 2 , 8.81 mg / cm 2 and 19.93 mg / cm 2 (Cr / FeCrAl coating), while the oxidation weight gain of Zry-4 alloy sample is 5.88 mg / cm 2 , 14.67 mg / cm 2 and 26.31 mg / cm 2 The weight gain curve shows that the Cr-N / FeCrAl coating prepared on the surface of zirconium alloy has the strongest protective ability for the Zr-4 substrate under high-temperature steam environment. The composite coating prepared in Example 1 was subjected to high-temperature steam oxidation test at different temperatures. The XRD patterns after the test are as follows: Figure 4 As shown in (b), at 1000°C, the coating showed diffraction peaks of Cr2O3, Fe2O3, and Al2O3 phases, among which the Al2O3 peak intensity was higher. As the oxidation temperature increased to 1100°C, the diffraction peaks of the Al2O3 phase increased, but the Cr2O3 phases at 36.3° and 76.8° disappeared. At 1200°C, the XRD results of the coating surface showed that the diffraction peak intensity of the Al2O3 phase increased significantly, and the diffraction peak intensity of other oxidations was extremely weak, indicating that the surface was basically an Al2O3 oxide film.
[0043] Comparative Example 2
[0044] According to the preparation process of Example 1, a FeCrAl coating is prepared on the surface of the zirconium alloy substrate, and then the same Cr-N coating is prepared on the surface of the coating. The difference from Example 1 is that the order of preparing the coatings is exchanged.
[0045] The FeCrAl coating is in direct contact with the Zr alloy substrate without any barrier effect. An obvious Fe-Zr eutectic reaction occurs. Cr-N only plays a weak antioxidant role in the composite coating. However, due to the performance attenuation of the FeCrAl coating, the overall high-temperature oxidation resistance is not ideal. The oxidation weight gain in a 1200℃ steam environment reaches 19.26 mg / cm 2 .
[0046] On the basis of Example 1, the sputtering power of the Cr target, the flow rate of N2 and the preparation time were adjusted to adjust the N content in the prepared Cr-N transition layer, and a Cr-N transition layer of the same thickness was prepared. The sputtering power of the high-purity Fe target and the CrAl alloy target was adjusted to adjust the Al content in the FeCrAl coating to prepare a FeCrAl coating of the same thickness. The coating was oxidized in a steam environment at 1200°C for 30 minutes, and the influence of the N and Al contents in the composite coating on the high-temperature oxidation resistance of the composite coating was statistically analyzed. The results are shown in Table 1.
[0047] Table 1: Effect of N and Al content on high temperature oxidation resistance of composite coating
[0048]
[0049] It can be seen from the table that in a 1200℃ high-temperature steam environment, when the N content in the Cr-N transition layer and the Al content in the FeCrAl coating are within a certain range, the Al-N diffusion barrier layer generated at the interface of the Cr-N transition layer and the FeCrAl coating has good continuity, and the barrier effect for element diffusion is significantly improved. However, as the N content gradually increases to a certain range, when the coating is in a high-temperature steam environment for a long time, N2 will be generated, resulting in the attenuation of the coating's antioxidant properties, and as the N doping amount increases, the attenuation is aggravated. In addition, too low or too high an Al content will also reduce the continuity of the AlN barrier layer, resulting in a certain degree of attenuation of the barrier effect.
[0050] Example 2
[0051] A method for preparing a high temperature oxidation resistant coating on the surface of a nuclear zirconium alloy comprises the following steps:
[0052] (1) Matrix pretreatment: Specifically, the surface of the zirconium alloy was polished with 100#, 400#, 1000#, and 2000# sandpaper in sequence, and the polished zirconium alloy matrix was polished with a diamond polishing liquid with a particle size of 1.5μm and a silica suspension with a particle size of 0.06μm in sequence, and then ultrasonically cleaned with acetone and anhydrous ethanol for 10 minutes and then blown dry for use;
[0053] (2) Sample loading and cleaning: Place the zirconium alloy substrate into the magnetron sputtering coating furnace chamber. When the vacuum degree in the furnace reaches 8×10 - 4 When Pa, Ar was introduced, the bias voltage was adjusted to 420 V, the power was 280 W, and the treatment time was 15 min;
[0054] (3) Deposition of Cr-N transition layer: Cr target was used as the sputtering target, the deposition temperature was 250°C, the Cr target power was 260 W, the deposition pressure was 0.3 Pa, the N2 flow rate was 10 sccm, the bias voltage was 12 V, the rotating frame speed was 6 rpm, the time was 8 h, and the N content in the Cr-N transition layer was controlled to be 17.8 at.%;
[0055] (4) Deposition of FeCrAl coating: High-purity Fe target and CrAl alloy target were used as sputtering targets, the deposition temperature was 450°C, the CrAl alloy target power was 180 W, the Fe target power was 280 W, the deposition pressure was 0.3 Pa, the bias voltage was 60 V, the rotating frame speed was 10 rpm, the time was 2 h, and the Al content in the FeCrAl coating was 21.94 at.%.
[0056] Example 3
[0057] A method for preparing a high temperature oxidation resistant coating on the surface of a nuclear zirconium alloy comprises the following steps:
[0058] (1) Matrix pretreatment: Specifically, the surface of the zirconium alloy was polished with 100#, 400#, 1000#, and 2000# sandpaper in sequence, and the polished zirconium alloy matrix was polished with a diamond polishing liquid with a particle size of 1.5μm and a silica suspension with a particle size of 0.06μm in sequence, and then ultrasonically cleaned with acetone and anhydrous ethanol for 10 minutes and then blown dry for use;
[0059] (2) Sample loading and cleaning: Place the zirconium alloy substrate into the magnetron sputtering coating furnace chamber. When the vacuum degree in the furnace reaches 8×10 - 4 When Pa, Ar was introduced, the bias voltage was adjusted to 480 V, the power was 320 W, and the treatment time was 8 min;
[0060] (3) Deposition of Cr-N transition layer: Cr target was used as the sputtering target, the deposition temperature was 350°C, the Cr target power was 240 W, the deposition pressure was 0.5 Pa, the N2 flow rate was 5 sccm, the bias voltage was 8 V, the rotating frame speed was 10 rpm, the time was 6 h, and the N content in the Cr-N transition layer was controlled to be 16.2 at.%;
[0061] (4) Deposition of FeCrAl coating: High-purity Fe target and CrAl alloy target were used as sputtering targets, the deposition temperature was 550°C, the CrAl alloy target power was 120 W, the Fe target power was 320 W, the deposition pressure was 0.5 Pa, the bias voltage was 80 V, the rotating frame speed was 6 rpm, the time was 3 h, and the Al content in the FeCrAl coating was 15.16 at.%.
Claims
1. A method for preparing a high temperature oxidation resistant composite coating on the surface of a nuclear zirconium alloy, characterized in that: A Cr-N transition layer is first prepared on the surface of a zirconium alloy substrate by magnetron sputtering, wherein the N content in the transition layer is 15-18 at.%, and then a FeCrAl coating is prepared on the surface of the transition layer to form a Cr-N / FeCrAl composite coating, wherein the Al content in the FeCrAl coating is 15-22 at.%. The deposition temperature for preparing the Cr-N transition layer is 250-350°C, the Cr target power is 240-260W, the deposition pressure is 0.3-0.5Pa, the N2 flow rate is 2-10sccm, the bias voltage is 8-12V, the rotating frame speed is 6-10rpm, and the time is 6-8h.
2. The method for preparing a high temperature oxidation resistant composite coating on the surface of a nuclear zirconium alloy according to claim 1, characterized in that: The deposition temperature for preparing the FeCrAl coating is 450-550° C., the CrAl alloy target power is 120-180 W, the Fe target power is 280-320 W, the deposition pressure is 0.3-0.5 Pa, the bias voltage is 60-80 V, the rotating frame speed is 6-10 rpm, and the time is 2-3 h.
3. The method for preparing a high temperature oxidation resistant composite coating on the surface of a nuclear zirconium alloy as claimed in claim 1 or 2, characterized in that: The zirconium alloy substrate is pretreated before preparing the coating. Specifically, the surface of the zirconium alloy is polished with 100#, 400#, 1000#, and 2000# sandpaper in sequence. The polished zirconium alloy substrate is polished with a diamond polishing liquid with a particle size of 1.5μm and a silicon dioxide suspension with a particle size of 0.06μm in sequence, and then ultrasonically cleaned with acetone and anhydrous ethanol for 10 minutes and then blown dry for use.
4. The method for preparing a high temperature oxidation resistant composite coating on the surface of a nuclear zirconium alloy as claimed in claim 3, characterized in that: The pretreated zirconium alloy substrate needs to be ion cleaned. Specifically, the zirconium alloy substrate is placed in a magnetron sputtering coating furnace. When the vacuum degree reaches 8×10 -4 When 400 Pa was used, Ar was introduced, the bias voltage was adjusted to 420-480 V, the power was 280-320 W, and the treatment time was 8-15 min.
5. A high temperature oxidation resistant composite coating on the surface of a nuclear zirconium alloy prepared by the method according to any one of claims 1 to 4, characterized in that: The composite coating comprises a Cr-N transition layer and a FeCrAl coating, wherein the N content in the Cr-N transition layer is 15-18 at.%, and the Al content in the FeCrAl coating is 15-22 at.%.
Citation Information
Patent Citations
Electroless deposition process for zirconium and zirconium alloys
CA1128376A
Preparation method for CrN coating on surface of nuclear zirconium alloy and product
CN109852943A
Laminated protective coating with high-temperature water vapor oxidization resistance and strong toughness as well as preparation method thereof and application thereof
CN110616400A
Multilayer composite coating of zirconium alloy cladding surface, and preparation method thereof
CN111172503A
High-temperature steam corrosion resistant coating for zirconium alloy cladding tube
CN112164479A