A viscosity-reducing adhesive reducing agent for concrete and preparation method thereof
By using organic alcohol amine, polycarboxylic acid mother liquor and water-retaining agent as a viscosity-reducing glue reducer in concrete, combined with unsaturated alkoxysilane monomer and graphene oxide modified polyether, the problem of concrete glue reducer and The problem of poor compatibility of raw materials achieves low water-binder ratio and high fluidity, reduces the bleeding rate, and improves the durability and construction performance of concrete.
Patent Information
- Application Number
- CN202410136118.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-01-31
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2044-01-31
AI Technical Summary
Existing concrete glue reducers have poor compatibility with concrete raw materials, resulting in rapid slump loss, prone to bleeding and segregation, and affecting the normal progress of construction.
A viscosity-reducing glue reducer including organic alcohol amine, polycarboxylic acid mother liquor and water-retaining agent is used, and modified by the compound addition of unsaturated alkoxysilane monomers and functional monomers in the polycarboxylic acid mother liquor. Polycarboxylic acid molecules are used to improve dispersion performance and fluidity, and side chains are added through carboxylated graphene oxide modified polyether to form a water film to improve water enrichment and durability of concrete.
While maintaining the strength of the concrete, reduce the amount of cementitious materials by 10%-15%, improve the slurry fullness and fluidity of the concrete, delay the hydration reaction of the cement, significantly reduce the bleeding rate, and improve the crack resistance. and durability properties, improving the workability and long-term performance of concrete.
Smart Images

Figure BDA0004691314360000081 
Figure BDA0004691314360000091
Abstract
Description
Technical Field
[0001] The invention relates to the field of concrete admixtures, in particular to a viscosity-reducing gel reducer for concrete and a preparation method thereof. Background Art
[0002] Concrete admixtures refer to substances added to improve and adjust the performance of concrete. They are added before or during the mixing of concrete. The amount of concrete admixtures is generally not more than 5% of the mass of cement. Concrete admixtures can be divided into water reducing agents, air entraining agents, early strength agents, colorants, rust inhibitors, and adhesive reducers according to their functions.
[0003] Gel reducer is a concrete additive. Its main function is to significantly reduce the amount of gel material, especially cement and mineral powder, while maintaining the concrete strength grade unchanged, and improve the working performance and volume stability of concrete. The mechanism of action of the gel reducer is that the cement material particles are very fine, and there will be some fine particle aggregates. The gel reducer can effectively disperse these aggregates, so that the cement particles are more fully in contact with water, maximizing the potential activity of cement, and promoting the hydration reaction of cement to be more complete; it can improve the bonding performance of the cement-based material slurry and the aggregate interface, and improve the strength of concrete.
[0004] During the use of existing concrete reducers, when reducing the amount of cementitious materials, it is found that the compatibility of the reducer with concrete raw materials is poor, the slump of concrete is lost quickly, and water seepage and segregation are prone to occur, affecting the normal pumping construction of concrete. Summary of the invention
[0005] In order to solve the problems that the existing concrete reducers have poor compatibility with concrete raw materials, the concrete slump loss is fast, and water seepage and segregation are prone to occur, the present application provides a viscosity-reducing reducer for concrete and a preparation method thereof.
[0006] The present application provides a viscosity reducing adhesive for concrete and a preparation method thereof, which adopts the following technical scheme:
[0007] In a first aspect, the present application provides a viscosity reducing adhesive for concrete, which is prepared by the following raw materials in parts by weight: 8-12 parts of organic alcohol amine; 5-10 parts of polycarboxylic acid mother liquid; 1-2 parts of water retaining agent; 75-85 parts of water;
[0008] The polycarboxylic acid mother solution comprises the following raw materials in parts by weight: 30-40 parts of polyether macromonomer; 5-8 parts of unsaturated carboxylic acid; 9-13 parts of functional monomer; 2-4 parts of unsaturated alkoxysilane monomer; 0.15-0.25 parts of initiator; 0.3-0.5 parts of chain transfer agent; and 65-75 parts of deionized water.
[0009] By adopting the above technical scheme, organic alcohol amine can promote the dispersion of cement particles in concrete, making the concrete paste more uniform, and the water retaining agent can reduce the cracking and leakage of concrete. The polycarboxylic acid mother liquor is selected to be mixed with the organic alcohol amine, the water retaining agent and water. The amount of cementitious material can be reduced by 10%-15% while keeping the strength grade of concrete unchanged, achieving a low water-cement ratio, and forming a water film at the same time, increasing the enrichment of water, significantly improving the paste fullness of the concrete, and improving the durability.
[0010] In the polycarboxylic acid mother liquor, unsaturated alkoxysilane monomers are used to modify the polycarboxylic acid, and siloxane functional groups are introduced into the main chain, which can chemically bond with the silanol groups of cement particles, thereby improving the dispersion performance of the glue reducer in cement and improving the viscosity reduction performance. By adding unsaturated alkoxysilane monomers and functional monomers in combination, the main chain of the polycarboxylic acid polymer is extended, so that the main chain has more anchor points with cement particles, which is beneficial to improve the fluidity of cement and improve the compatibility with concrete raw materials. By increasing the delay of the later cement hydration reaction, the durability of concrete can be improved and the slump of concrete can be maintained.
[0011] Optionally, the polyether macromonomer is selected from one or more of isopentanol polyoxyethylene ether, methyl allyl polyoxyethylene ether, and 4-hydroxybutyl vinyl polyethylene glycol ether.
[0012] By adopting the above technical solution, a polyether macromonomer is selected as the side chain of the polycarboxylic acid, and water solubility is achieved through the hydrophilic group at the end of the side chain. At the same time, the polyether side chain provides steric hindrance to promote the dispersion of cement and improve fluidity.
[0013] Optionally, the polyether macromonomer is graphene oxide modified methyl allyl polyoxyethylene ether, and the graphene oxide modified methyl allyl polyoxyethylene ether is prepared from the following raw materials in parts by weight:
[0014] Graphene oxide 0.18-0.22 parts;
[0015] 20-25 parts of methyl allyl polyoxyethylene ether;
[0016] Chloroacetic acid 4-10 parts;
[0017] 75-85 parts of solvent;
[0018] 30-45 parts of 20% alkali solution by mass.
[0019] By adopting the above technical scheme, the polyether is modified by carboxylated graphene oxide, and carboxyl groups and graphene oxide segments are introduced into the side chains of the formed polycarboxylic acid molecules. The formed side chains can solve the water bleeding and segregation phenomena of concrete, and at the same time, the steric hindrance is further increased. The introduced carboxyl groups have an adsorption effect on cement particles, thereby further improving the fluidity and dispersibility of cement. The later hydration of cement is promoted by graphene oxide, which is beneficial to improving the crack resistance and durability of concrete.
[0020] Optionally, the unsaturated carboxylic acid is selected from one or more of acrylic acid and methacrylic acid; the unsaturated alkoxysilane monomer is selected from one or more of vinyltriethoxysilane, γ-methacryloxypropyltrimethoxysilane and 3-(methacryloxy)propyltrimethoxysilane; and the functional monomer is selected from one or more of sodium methyl allyl sulfonate and 2-acrylamide-2-methylpropane sulfonic acid.
[0021] By adopting the above technical scheme, unsaturated monomers with carbon-carbon double bonds are selected for copolymerization to achieve the synthesis of polycarboxylic acid, and functional monomers containing sulfonic acid groups are selected to introduce sulfonic acid groups into the polycarboxylic acid molecules. The sulfonic acid groups can also be affinity with calcium ions of cement and serve as anchor points for the gel reducer.
[0022] Optionally, the unsaturated carboxylic acid is acrylic acid, the unsaturated alkoxysilane monomer is vinyltriethoxysilane, and the functional monomer is 2-acrylamide-2-methylpropanesulfonic acid.
[0023] By adopting the above technical scheme, when acrylic acid, vinyl triethoxysilane and 2-acrylamide-2-methylpropane sulfonic acid are selected in combination, the concrete adhesive reducer has higher stability, is more conducive to improving the comprehensive performance of concrete, and has better synergistic effect with other admixtures.
[0024] Optionally, the organic alcohol amine is one or more of triethanolamine, triisopropanolamine, diethanol monoisopropanolamine and N,N-dimethylisopropanolamine.
[0025] By adopting the above technical solution, the organic alcohol amine has the effect of promoting the hydration rate of cement particles, thereby improving the strength of concrete, and has a significant dispersing effect on cement, making the concrete paste more uniform.
[0026] Optionally, the water-retaining agent is one or more of hydroxypropyl methylcellulose, carboxymethyl cellulose, hydroxyethyl cellulose, and polyvinyl alcohol.
[0027] Optionally, the initiator is selected from one or more of hydrogen peroxide, ammonium persulfate, and ascorbic acid; the chain transfer agent is selected from one or more of mercaptoethanol, thioglycolic acid, and sodium hypophosphite.
[0028] In a second aspect, the present application provides a method for preparing a viscosity-reducing adhesive reducer for concrete.
[0029] In summary, this application has the following beneficial effects:
[0030] 1. Organic alcohol amines can promote the dispersion of cement particles in concrete, making the concrete paste more uniform. Water retaining agents can reduce cracking and leakage of concrete. The use of polycarboxylic acid mother liquor mixed with organic alcohol amines, water retaining agents and water can reduce the amount of cementitious materials by 10%-15% while keeping the strength grade of concrete unchanged, achieve a low water-cement ratio, form a water film, increase the degree of water enrichment, significantly improve the fullness of concrete paste, and improve durability.
[0031] In the polycarboxylic acid mother liquor, unsaturated alkoxysilane monomers are used to modify the polycarboxylic acid, and siloxane functional groups are introduced into the main chain, which can chemically bond with the silanol groups of cement particles, thereby improving the dispersion performance of the glue reducer in cement and improving the viscosity reduction performance. By adding unsaturated alkoxysilane monomers and functional monomers in combination, the main chain of the polycarboxylic acid polymer is extended, so that the main chain has more anchor points with cement particles, which is beneficial to improve the fluidity of cement and improve the compatibility with concrete raw materials. By increasing the delay of the later cement hydration reaction, the durability of concrete can be improved and the slump of concrete can be maintained.
[0032] 2. The polyether is modified by carboxylated graphene oxide, and carboxyl groups and graphene oxide segments are introduced into the side chains of the formed polycarboxylic acid molecules. The formed side chains can solve the water bleeding and segregation phenomena of concrete, and at the same time, the steric hindrance is further increased. The introduced carboxyl groups have an adsorption effect on cement particles, thereby further improving the fluidity and dispersibility of cement. Graphene oxide promotes the later hydration of cement, which is beneficial to improve the crack resistance and durability of concrete. DETAILED DESCRIPTION
[0033] The present application is further described in detail below in conjunction with Examples 1-8 and Comparative Examples 1-3.
[0034] Preparation Example
[0035] It should be noted that the graphene oxide mentioned below is selected from Nanjing Jicang Nanotechnology Co., Ltd., with a single layer ratio of >95% and a diameter of <5μm.
[0036] Preparation Example 1
[0037] Preparation of graphene oxide modified methyl allyl polyoxyethylene ether
[0038] Add 30 g of 20% alkali solution (sodium hydroxide solution) into a beaker, add 0.18 g of graphene oxide into the beaker, ultrasonically disperse into a colloidal solution, add 4 g of chloroacetic acid to the colloidal solution, ultrasonically react for 2 h, filter the reaction solution hot to remove impurities, evaporate excess water, and vacuum dry at 60 ° C to obtain carboxylated graphene oxide;
[0039] The carboxylated graphene oxide was dissolved in 75 g of solvent water, 20 g of methyl allyl polyoxyethylene ether with an average molecular weight of 2400 was added, and the mixture was reacted at 40° C. for 2 h, washed three times with anhydrous ethanol and deionized water respectively, recrystallized with 100 ml of anhydrous ethanol, and vacuum dried at 40° C. for 6 h to obtain graphene oxide modified methyl allyl polyoxyethylene ether.
[0040] Preparation Example 2
[0041] Preparation of graphene oxide modified methyl allyl polyoxyethylene ether
[0042] Add 45 g of 20% alkali solution (sodium hydroxide solution) into a beaker, add 0.22 g of graphene oxide into the beaker, ultrasonically disperse into a colloidal solution, add 10 g of chloroacetic acid to the colloidal solution, ultrasonically react for 3 h, filter the reaction solution hot to remove impurities, evaporate excess water, and vacuum dry at 70 ° C to obtain carboxylated graphene oxide;
[0043] The carboxylated graphene oxide was dissolved in 85 g of solvent water, 25 g of methyl allyl polyoxyethylene ether with an average molecular weight of 2400 was added, and the mixture was reacted at 45° C. for 4 h, washed three times with anhydrous ethanol and deionized water respectively, recrystallized with 100 ml of anhydrous ethanol, and vacuum dried at 45° C. for 8 h to obtain graphene oxide modified methyl allyl polyoxyethylene ether.
[0044] Preparation Example 3
[0045] Preparation of graphene oxide modified methyl allyl polyoxyethylene ether
[0046] Add 40 g of 20% alkali solution (sodium hydroxide solution) into a beaker, add 0.20 g of graphene oxide into the beaker, ultrasonically disperse into a colloidal solution, add 7 g of chloroacetic acid into the colloidal solution, ultrasonically react for 2.5 h, filter the reaction solution hot to remove impurities, evaporate excess water, and vacuum dry at 65 ° C to obtain carboxylated graphene oxide;
[0047] The carboxylated graphene oxide was dissolved in 80 g of solvent water, 23 g of methyl allyl polyoxyethylene ether with an average molecular weight of 2400 was added, and the mixture was reacted at 42° C. for 3 h, washed three times with anhydrous ethanol and deionized water respectively, recrystallized with 100 ml of anhydrous ethanol, and vacuum dried at 42° C. for 7 h to obtain graphene oxide modified methyl allyl polyoxyethylene ether.
[0048] Example
[0049] Example 1
[0050] Preparation of a viscosity-reducing adhesive for concrete
[0051] (1) Weigh 30 g of deionized water, 30 g of isopentanol polyoxyethylene ether with an average molecular weight of 2400, and 0.1 g of hydrogen peroxide into a reactor, stir and heat until the isopentanol polyoxyethylene ether is completely dissolved to obtain a base solution;
[0052] (2) Dissolve 5 g of acrylic acid, 9 g of sodium methyl allyl sulfonate and 2 g of vinyl triethoxysilane in 30 g of deionized water, and mix to obtain liquid a; dissolve 0.05 g of ascorbic acid and 0.3 g of mercaptoethanol in 5 g of deionized water, and mix to obtain liquid b;
[0053] (3) Add liquid a to the base liquid dropwise for 2 h, and add liquid b dropwise for 2.5 h;
[0054] (4) After the addition is completed, the reaction is kept at 45°C for 1 hour, cooled to room temperature, and a certain amount of liquid alkali neutralizer is added to adjust the pH to 6 to obtain a polycarboxylic acid mother solution;
[0055] (5) Add 8 g of triethanolamine, 1 g of hydroxypropyl methylcellulose and 75 g of water to the polycarboxylic acid mother liquor and stir evenly to obtain a viscosity-reducing type gel reducer.
[0056] Example 2
[0057] Preparation of a viscosity-reducing adhesive for concrete
[0058] (1) Weigh 35 g of deionized water, 40 g of methyl allyl polyoxyethylene ether with an average molecular weight of 2400, and 0.15 g of ammonium persulfate into a reactor, stir and heat until the methyl allyl polyoxyethylene ether is completely dissolved to obtain a base solution;
[0059] (2) Dissolve 8 g of methacrylic acid, 13 g of 2-acrylamide-2-methylpropanesulfonic acid and 4 g of γ-methacryloxypropyltrimethoxysilane in 35 g of deionized water, and mix to obtain liquid a; dissolve 0.1 g of ascorbic acid and 0.5 g of thioglycolic acid in 5 g of deionized water, and mix to obtain liquid b;
[0060] (3) Add liquid a to the base liquid dropwise for 2.5 hours, and add liquid b dropwise for 3 hours;
[0061] (4) After the addition is completed, the reaction is kept at 60°C for 2 hours, then cooled to room temperature, a certain amount of liquid alkali neutralizer is added, and the pH is adjusted to 7 to obtain a polycarboxylic acid mother solution;
[0062] (5) Add 12 g of triisopropanolamine, 2 g of carboxymethyl cellulose and 85 g of water to the polycarboxylic acid mother liquor and stir evenly to obtain a viscosity-reducing type glue reducer.
[0063] Example 3
[0064] Preparation of a viscosity-reducing adhesive for concrete
[0065] (1) 30 g of deionized water, 35 g of 4-hydroxybutyl vinyl polyethylene glycol ether with an average molecular weight of 3000, and 0.1 g of ammonium persulfate were weighed into a reactor, and the mixture was stirred and heated until the 4-hydroxybutyl vinyl polyethylene glycol ether was completely dissolved to obtain a base liquid;
[0066] (2) Dissolve 7 g of methacrylic acid, 11 g of sodium methallyl sulfonate and 3 g of 3-(methacryloyloxy)propyltrimethoxysilane in 30 g of deionized water, and mix to obtain liquid a; dissolve 0.1 g of ascorbic acid and 0.4 g of sodium hypophosphite in 10 g of deionized water, and mix to obtain liquid b;
[0067] (3) Add liquid a to the base liquid dropwise for 2 hours, and add liquid b dropwise for 3 hours;
[0068] (4) After the addition is completed, the reaction is kept at 55°C for 1.5 hours, then cooled to room temperature, a certain amount of liquid alkali neutralizer is added, and the pH is adjusted to 7 to obtain a polycarboxylic acid mother solution;
[0069] (5) Add 10 g of diethanol monoisopropanolamine, 1.5 g of polyvinyl alcohol and 80 g of water to the polycarboxylic acid mother liquor and stir evenly to obtain a viscosity-reducing type glue reducer.
[0070] Example 4
[0071] Preparation of a viscosity-reducing adhesive for concrete
[0072] The difference between the present application and Example 1 is that in step (1), the polyether macromonomer is the graphene oxide modified methyl allyl polyoxyethylene ether prepared in Preparation Example 1.
[0073] The preparation method of the viscosity reducing agent is the same as that of Example 1.
[0074] Example 5
[0075] Preparation of a viscosity-reducing adhesive for concrete
[0076] The difference between the present application and Example 1 is that in step (1), the polyether macromonomer is the graphene oxide modified methyl allyl polyoxyethylene ether obtained in Preparation Example 2.
[0077] The preparation method of the viscosity reducing agent is the same as that of Example 1.
[0078] Example 6
[0079] Preparation of a viscosity-reducing adhesive for concrete
[0080] The difference between the present application and Example 1 is that in step (1), the polyether macromonomer is the graphene oxide modified methyl allyl polyoxyethylene ether prepared in Preparation Example 3.
[0081] The preparation method of the viscosity reducing agent is the same as that of Example 1.
[0082] Example 7
[0083] Preparation of a viscosity-reducing adhesive for concrete
[0084] The difference between the present application and Example 1 is that in step (2), the unsaturated carboxylic acid is acrylic acid, the unsaturated alkoxysilane monomer is vinyltriethoxysilane, and the functional monomer is 2-acrylamide-2-methylpropanesulfonic acid.
[0085] The preparation method of the viscosity reducing agent is the same as that of Example 1.
[0086] Example 8
[0087] Preparation of a viscosity-reducing adhesive for concrete
[0088] The difference between the present application and Example 1 is that: in step (1), the polyether macromonomer is the graphene oxide modified methyl allyl polyoxyethylene ether prepared in Preparation Example 1;
[0089] In step (2), the unsaturated carboxylic acid is acrylic acid, the unsaturated alkoxysilane monomer is vinyltriethoxysilane, and the functional monomer is 2-acrylamide-2-methylpropanesulfonic acid.
[0090] The preparation method of the viscosity reducing agent is the same as that of Example 1.
[0091] Comparative Example
[0092] Comparative Example 1
[0093] Preparation of a viscosity-reducing adhesive for concrete
[0094] The difference between the present application and Example 1 is that in step (2), no functional monomer is added to liquid a.
[0095] The preparation method of the viscosity reducing agent is the same as that of Example 1.
[0096] Comparative Example 2
[0097] Preparation of a viscosity-reducing adhesive for concrete
[0098] The difference between the present application and Example 1 is that in step (2), no unsaturated alkoxysilane monomer is added to liquid a.
[0099] The preparation method of the viscosity reducing agent is the same as that of Example 1.
[0100] Comparative Example 3
[0101] The difference between the present application and Example 1 is that in step (5), no organic alcohol amine is added.
[0102] The preparation method of the viscosity reducing agent is the same as that of Example 1.
[0103] Performance Testing
[0104] 1. The raw material selection of concrete is designed to have a strength of C30, using China Resources P·Ⅱ42.5 cement with a specific surface area of 358m 2 / kg; river sand, fineness modulus 2.6, particle size 0-5mm; stone, particle size 5-20mm; fly ash, fineness 15%, specific surface area 460m 2 / kg; mineral powder, specific surface area of 483m 2 / kg; the water reducer is the high-performance polycarboxylate water reducer produced by Hunan Zhongyan Building Materials Technology Co., Ltd.
[0105] 2. Blank example: 180 kg cement, 90 kg mineral powder, 60 kg fly ash, 850 g sand, 1010 kg stone, 160 kg water and 8.58 kg polycarboxylate water reducer were mixed to obtain a reference concrete.
[0106] Test example: 160 kg of cement, 90 kg of mineral powder, 60 kg of fly ash, 860 g of sand, 1020 kg of stone, 160 kg of water, 8.58 kg of polycarboxylic acid water reducer and 1.98 kg of the gel reducer of Examples 1-8 and Comparative Examples 1-3 were stirred and mixed to obtain concrete of each test example.
[0107] Extended test example: 180 kg of cement, 90 kg of mineral powder, 60 kg of fly ash, 850 g of sand, 1010 kg of stone, 160 kg of water, 8.58 kg of polycarboxylic acid water reducer and 1.98 kg of the gel reducer of Example 1, Example 4, Example 7 and Example 8 were stirred and mixed to obtain extended test example concrete.
[0108] 3. Test the initial slump / expansion, time-dependent slump / expansion, strength, water seepage rate and other indicators of the benchmark concrete, test case concrete and extended test case concrete respectively, refer to the GB / 8076-2008 "Concrete Admixture" test standard, and record the test results in Table 1.
[0109] Table 1
[0110]
[0111] Result analysis:
[0112] According to Table 1, by using the gel reducer of the embodiment of the present invention, the amount of cementitious material (cement) used in concrete can be reduced by 10%-15%. When the amount of cement is reduced, the performance of the concrete is slightly reduced compared with the benchmark concrete, but the overall difference is not large. There is not much effect on the fluidity, workability and time-slump retention capacity of the concrete, and the strength grade of the concrete remains basically unchanged.
[0113] By using the adhesive reducer of the embodiment of the present invention, without reducing the amount of cement, the initial slump and expansion of the concrete are greatly improved compared with the benchmark concrete. The slump and expansion are the determination methods and indicators of the workability of concrete. The larger the slump and expansion, the better the fluidity of the concrete, which shows that the adhesive reducer of the present application improves and enhances the uniformity and fluidity of the concrete. The compressive strength of the concrete is increased by more than 10%, which helps to improve the strength and mechanical properties of the concrete.
[0114] After the adhesive reducer of the present application is applied, the water bleeding rate of the concrete is greatly reduced, indicating that the adhesive reducer of the present application can solve the problems of stone leakage, sand leakage, and easy water separation of concrete by using the unique hydrophilic functional group, and does not affect the maintenance of slump. The adhesive reducer can effectively reduce the viscosity of concrete and improve the pumpability and durability.
[0115] Compared with Examples 1-3, Examples 4-7 of the present application use graphene oxide-modified methyl allyl polyoxyethylene ether instead of polyether macromonomer in the preparation of polycarboxylic acid mother liquor, so that carboxyl groups and graphene oxide segments are introduced into the side chains of polycarboxylic acid molecules, which further improves the fluidity of the concrete, helps solve the problem of water segregation in the concrete, and reduces the water bleeding rate.
[0116] Compared with Examples 1-3, Example 8 of the present application specifically selects a monomer combination of acrylic acid, vinyl triethoxysilane and 2-acrylamide-2-methylpropane sulfonic acid in the monomer selection, which makes the structure of the concrete more stable, is conducive to the full play of the effect of the gel reducer, and thus the comprehensive performance of the concrete is improved.
[0117] 1. The performance indexes of the concrete mixed with the adhesive reducing agent of Example 1 of the present application were measured, and the results were recorded in Table 2.
[0118] Table 2
[0119]
[0120] According to the data in Table 2, the glue reducing agent prepared in the present application meets the performance requirements of national standards, can improve the durability of concrete such as anti-shrinkage and anti-carbonation, play a role in reducing water and glue, improve the working performance of concrete, and has obvious economic, ecological and social benefits.
[0121] This specific implementation manner is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make non-creative modifications to the specific implementation manner as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.
Claims
1. A viscosity reducing adhesive for concrete, It is characterized in that The method is prepared by the following raw materials in parts by weight: 8-12 parts of organic alcohol amine; 5-10 parts of polycarboxylic acid mother solution; 1-2 parts of water retaining agent; 75-85 parts of water; The polycarboxylic acid mother solution is made of the following raw materials in parts by weight: 30-40 parts of polyether macromonomer; 5-8 parts of unsaturated carboxylic acid; 9-13 parts of functional monomer; 2-4 parts of unsaturated alkoxysilane monomer; 0.15-0.25 parts of initiator; 0.3-0.5 parts of chain transfer agent; and 65-75 parts of deionized water; The polyether macromonomer is graphene oxide modified methyl allyl polyoxyethylene ether, and the graphene oxide modified methyl allyl polyoxyethylene ether is prepared from the following raw materials in parts by weight: Graphene oxide 0.18-0.22 parts; 20-25 parts of methyl allyl polyoxyethylene ether; Chloroacetic acid 4-10 parts; 75-85 parts of solvent; 30-45 parts of 20% alkali solution; The preparation steps of the polyether macromonomer include: The graphene oxide is dispersed in an alkali solution with a mass fraction of 20%, and ultrasonically dispersed into a colloidal solution. Chloroacetic acid is added to the colloidal solution and ultrasonicated for 2-3 hours. Impurities are removed by hot filtration, excess water is evaporated, and vacuum drying is performed at 60-70° C. to obtain carboxylated graphene oxide. Dissolving carboxylated graphene oxide in a solvent, adding methyl allyl polyoxyethylene ether, reacting at 40-45° C. for 2-4 hours, washing with anhydrous ethanol and deionized water, recrystallizing with anhydrous ethanol, and vacuum drying at 40-45° C. for 6-8 hours to obtain graphene oxide modified methyl allyl polyoxyethylene ether; The unsaturated carboxylic acid is selected from one or more of acrylic acid and methacrylic acid; the unsaturated alkoxysilane monomer is selected from one or more of vinyl triethoxysilane and γ-methacryloxypropyl trimethoxysilane; the functional monomer is selected from one or more of sodium methyl allyl sulfonate and 2-acrylamide-2-methylpropane sulfonic acid.
2. A viscosity reducing adhesive for concrete according to claim 1, Features: The unsaturated carboxylic acid is acrylic acid, the unsaturated alkoxysilane monomer is vinyltriethoxysilane, and the functional monomer is 2-acrylamide-2-methylpropanesulfonic acid.
3. A viscosity reducing adhesive for concrete according to claim 1, Features: The organic alcohol amine is selected from one or more of triethanolamine, triisopropanolamine, diethanol monoisopropanolamine and N,N-dimethylisopropanolamine.
4. A viscosity-reducing adhesive for concrete according to claim 1, Features: The water retaining agent is selected from one or more of hydroxypropyl methylcellulose, carboxymethyl cellulose, hydroxyethyl cellulose and polyvinyl alcohol.
5. The viscosity-reducing adhesive for concrete according to claim 1, Features: The initiator is selected from one or more of hydrogen peroxide, ammonium persulfate, and ascorbic acid; the chain transfer agent is selected from one or more of mercaptoethanol, thioglycolic acid, and sodium hypophosphite.
6. A method for preparing a viscosity-reducing adhesive reducer for concrete according to any one of claims 1 to 5, It is characterized in that The following steps are involved: (1) Weigh a certain amount of deionized water, polyether macromonomer and initiator into a reactor, stir and heat until the polyether macromonomer is completely dissolved to obtain a base solution; (2) dissolving an unsaturated carboxylic acid, a functional monomer and an unsaturated alkoxysilane monomer in deionized water, mixing to obtain a liquid A, dissolving an initiator and a chain transfer agent in deionized water, mixing to obtain a liquid B; (3) Add liquid a to the base liquid dropwise for 2 h to 2.5 h, and add liquid b dropwise for 2.5 h to 3 h; (4) After the addition is completed, the reaction is carried out at 45-60°C for 1-2 hours, then cooled to room temperature, a certain amount of liquid alkali neutralizer is added, and the pH is adjusted to 6-7 to obtain a polycarboxylic acid mother solution; (5) Add organic alcohol amine, water retaining agent and water to the polycarboxylic acid mother liquor and stir evenly to obtain a viscosity reducing glue reducing agent.