A precise control method for treating solid waste using a rotary kiln

CN118127320BActive Publication Date: 2024-11-08ZHONGYE-CHANGTIAN INT ENG CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410444319.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-04-12
Publication Date
2024-11-08
Estimated Expiration
2044-04-12

AI Technical Summary

Technical Problem

物料进入回转窑后首先经过干燥段,现有技术中干燥段采用统一的温度范围进行处理,由于物料来源不同,物料中的成分变化巨大,造成现有技术中还原装置的干燥段极易发生物料熔融或者结圈现象,熔融或者结圈的物料对还原装置内部耐火材料侵蚀,使得还原装置变薄甚至脱落

Benefits of technology

[0092] 1. The present invention controls the maximum temperature and maximum heating rate of the drying section of the reduction device according to the different sources of raw materials, the composition of the composite pellets and the specific properties of the materials, which can effectively avoid the explosion of the pellets after entering the kiln; at the same time, according to The pellet performance regulates the temperature field distribution in the kiln to achieve efficient reduction dezincification of zinc-containing dust mud pellets.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118127320B_ABST
    Figure CN118127320B_ABST
Patent Text Reader

Abstract

The present invention proposes a method for resource utilization of iron-containing solid waste. According to the specific situation of pre-treating the iron-containing solid waste to be treated to obtain composite pellets, a precise treatment method of treating the iron-containing solid waste using a reduction device is proposed. First, the iron-containing solid waste, the reducing agent, and the additive are mixed and pelletized to obtain composite pellets, and then the composite pellets are input into the reduction device, and sequentially pass through the drying section, preheating section, reduction roasting section, and preliminary cooling section of the reduction device to obtain high-temperature iron slag. The present invention controls the temperature field in the drying section of the reduction device to avoid the large-scale melting of the material in the reduction device under the conditions of local high temperature and high reduction atmosphere, resulting in kiln stagnation; at the same time, the ingredients are controlled according to the maximum temperature and maximum heating rate of the drying section to avoid the formation of a large amount of low-melting-point substances, thereby avoiding the ringing of the material in the reduction device.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a method for treating iron-containing solid waste, and in particular to a method for resource utilization of iron-containing solid waste by adopting a reduction device, and belongs to the technical field of metallurgy and mineral processing. Background Art

[0002] A large amount of iron-zinc-containing dust and mud will be generated in the process of iron and steel metallurgy and nonferrous metallurgy, mainly including blast furnace ash produced in the iron-making process, converter ash, converter dust and mud, electric furnace ash, etc. produced in the steel-making process, and dust and slag produced in the smelting process of zinc and copper. Due to the differences in smelting raw materials, equipment, and process conditions, the composition of each of the above iron-zinc-containing dust and mud varies greatly. In addition to a large amount of iron, blast furnace ash also contains a large amount of carbon and zinc elements. In particular, zinc is harmful to the blast furnace smelting process. Therefore, the blast furnace ash needs to be free of zinc before it can be returned to the iron-making process for recycling. Steelmaking ash also contains a large amount of iron and zinc elements, which cannot all be directly returned to the sintering-blast furnace process. The zinc element must be removed in advance before it can be recycled.

[0003] In the prior art, most of the metallurgical solid wastes generated in the process of iron and steel metallurgy and nonferrous metallurgy are disposed by pyrometallurgical disposal. The pyrometallurgical smelting process mostly uses carbon-based reduction or pyrolysis / combustion to recover metals. The carbon-based reduction or pyrolysis / combustion disposal methods are usually prone to secondary oxidation during the metal vapor condensation process, which reduces the purity of the recovered products and emits a large amount of CO2 during the reaction process, which does not meet the requirements of energy conservation and environmental protection. In addition, the prior art usually uses traditional rotary kiln processes and rotary hearth furnace processes for pyrolysis or combustion reduction of metallurgical solid wastes. The rotary kiln uses solid fuel as a reducing agent and uses the rotary kiln as a reaction device, which can process a wider range of raw materials. The material flow movement mode inside the rotary kiln is gas-solid reverse movement. The burner at the kiln head generates high-temperature gas. The flow from the head to the tail forms a countercurrent contact with the material added at the kiln tail. The high-temperature airflow contacts the material to exchange heat. The added material completes the smelting process under the high-temperature environment at the kiln head. The rotary kiln has the significant advantages of low investment and simple operation, but it is not suitable for handling low-zinc materials, and the metallization rate of iron materials is also low. Since the temperature of the drying, preheating, and reduction roasting sections in the kiln and the heating rate of each section are not accurately constrained, the system temperature is too high and uneven, causing the furnace body to form rings or harden. Ring formation will cause the cross-sectional area of ​​the rotary kiln to continuously reduce, causing material blocking, deteriorating roasting process parameters, causing changes in the working conditions in the kiln, reducing the service life of refractory materials, and easily causing unstable roasting material indicators.

[0004] Chinese patent CN 111733330 A discloses a method for zinc enrichment and recovery using a rotary kiln, comprising the following steps: pulverized coal and oxygen-enriched air are blown into the kiln tail to carry out a calcination reaction for 80 to 100 minutes; under the action of the kiln head exhaust fan, the flow direction of the flue gas generated by the calcination reaction is consistent with the movement direction of the raw materials entering the kiln, and both move from the kiln tail to the kiln head; the roasted ore is collected, ground and magnetically separated to obtain iron concentrate; the flue gas extracted by the exhaust fan is collected and purified, zinc-containing dust is collected by a dust collection system, and the dust is mixed with the raw materials entering the kiln for granulation to obtain a mixed kiln material, which is sent to a variable diameter rotary kiln, and the calcination process and the zinc-containing dust collection process are cyclically carried out to achieve cyclic enrichment of zinc; when the zinc content in the flue gas reaches more than 10%, the zinc-containing dust in the flue gas is directly collected, and zinc is recovered by an acid leaching process. After entering the rotary kiln, the material first passes through the drying section. In the prior art, the drying section is processed in a uniform temperature range. Due to the different sources of the materials, the composition of the materials varies greatly, which makes it very easy for the material to melt or form rings in the drying section of the reduction device in the prior art. The molten or ringed materials corrode the refractory materials inside the reduction device, causing the reduction device to become thinner or even fall off. At the same time, the technical solution does not accurately constrain the temperature of the drying section in the kiln and the heating rate of each section, resulting in a large amount of melting of the powder in the rotary kiln under the conditions of local high temperature and high reduction atmosphere, and the kiln is seriously agglomerated, resulting in low operating rate. Summary of the invention

[0005] In view of the technical problem that the reduction device in the above-mentioned prior art uses a drying section with a uniform temperature range to treat iron-containing solid waste, causing the material to burst, form rings or melt in the reduction device, the present invention proposes a method for resource utilization of iron-containing solid waste. According to the composition of the iron-containing material to be treated, the temperature and heating rate of the drying section in the reduction device are reasonably adjusted to avoid the material from bursting, forming rings or melting in the reduction device. According to the specific situation of pre-treating the iron-containing solid waste to be treated to obtain composite pellets, the present invention proposes a precise control method for treating iron-containing solid waste using a reduction device. First, the iron-containing solid waste, the reducing agent, and the additive are mixed and pelletized to obtain composite pellets, and then the composite pellets are input into the reduction device, and successively pass through the drying section, preheating section, reduction roasting section, and preliminary cooling section of the reduction device to obtain high-temperature iron slag. According to the particle size, alkalinity and moisture content of the composite pellets, the drying temperature in the drying section of the reduction device and the heating rate in the drying section are controlled. The present invention detects the temperature field in the drying section of the reduction device and calculates the maximum temperature and the maximum heating rate of the drying section in the kiln according to the alkalinity, particle size and moisture of the composite pellets to judge the material reduction environment and make adjustments, so that the material is strictly temperature-controlled according to the specific conditions of the material from the moment it enters the reduction device, thereby avoiding the material in the reduction device from melting in large quantities under the conditions of local high-temperature and high-reducing atmosphere, resulting in kiln stagnation. At the same time, the ingredients are controlled according to the maximum temperature and the maximum heating rate of the drying section to avoid the formation of a large amount of low-melting-point substances, thereby avoiding the material from stagnation in the reduction device.

[0006] According to an embodiment of the present invention, a method for resource utilization of iron-containing solid waste is provided, the method comprising the following steps:

[0007] (1) mixing and pelletizing the iron-containing solid waste, the reducing agent, and the additive to obtain composite pellets;

[0008] (2) The composite pellets are fed into a reduction device and sequentially passed through a drying section, a preheating section, a reduction roasting section, and a preliminary cooling section of the reduction device to obtain high-temperature iron slag;

[0009] The drying temperature and the heating rate in the drying section of the reduction device are controlled according to the particle size, alkalinity and moisture content of the composite pellets.

[0010] In the present invention, the drying temperature in the drying section of the reduction device is controlled according to the particle size, alkalinity and moisture content of the composite pellets:

[0011]

[0012] Among them, T gz is the highest drying temperature in the drying section, ℃; K gzis the maximum temperature coefficient of the drying section, with a value of 0.5-1, ℃·mm; R is the alkalinity of the composite pellets, %; m is the alkalinity index of the composite pellets at the highest drying temperature, with a value of 0.1-0.3; D is the average particle size of the composite pellets, mm; n is the average particle size index of the composite pellets at the highest drying temperature, with a value of 0.4-0.6; W is the moisture content of the composite pellets, %; x is the moisture index of the composite pellets at the highest drying temperature, with a value of 0.4-0.6.

[0013] In the present invention, according to the particle size, alkalinity and moisture content of the composite pellets, the temperature rise rate in the drying section of the reduction device is controlled as follows:

[0014]

[0015] Among them, S gz is the maximum heating rate in the drying section, ℃ / min; K s is the maximum heating rate coefficient of the drying section, which is 0.1-0.3, mm / min; a is the alkalinity index of the composite pellets at the maximum heating rate, which is 0.4-0.6; b is the average particle size index of the composite pellets at the maximum heating rate, which is 0.1-0.4; e is 2.71828.

[0016] In the present invention, the reduction device is a rotary kiln, and the iron-containing solid waste is iron-containing and zinc-containing dust mud.

[0017] Preferably, the method is as follows:

[0018] (1) mixing iron-containing zinc-containing dust, a reducing agent, and an additive, and pelletizing to obtain composite pellets;

[0019] (2) The composite pellets are fed into a rotary kiln, where they pass through a drying section, a preheating section, a reduction roasting section, and a preliminary cooling section in sequence;

[0020] (3) The flue gas discharged from the rotary kiln is optionally subjected to waste heat utilization, and then dust removal is performed to obtain the zinc-containing material, and the gas after dust removal is optionally subjected to flue gas purification before being discharged;

[0021] (4) The slag phase discharged from the rotary kiln is cooled to obtain iron-containing material.

[0022] Preferably, the rotary kiln is a rotary kiln without air inlet into the kiln body; according to the process conditions of the drying section on the rotary kiln, the process of step (1) is adjusted to control the particle size, alkalinity and moisture content of the prepared composite pellets, so that T gz Greater than or equal to the temperature in the drying section of the rotary kiln.

[0023] Preferably, the process of step (1) is adjusted according to the process conditions of the drying section on the rotary kiln to control the particle size, basicity and moisture content of the prepared composite pellets so that Sgz Greater than or equal to the temperature in the drying section of the rotary kiln.

[0024] Preferably, the rotary kiln is a kiln body air inlet rotary kiln; according to the particle size, alkalinity and moisture content of the composite pellets prepared in step (1), the air inlet volume of the rotary kiln is adjusted so that the temperature in the drying section of the rotary kiln is less than or equal to T gz .

[0025] Preferably, according to the particle size, alkalinity and moisture content of the composite pellets prepared in step (1), the air inlet of the rotary kiln is adjusted so that the heating rate in the drying section of the rotary kiln is less than or equal to S gz .

[0026] Preferably, the temperature in the preheating section of the reduction device is 500-1000°C, preferably 600-950°C, more preferably 700-900°C.

[0027] Preferably, the temperature in the reduction roasting section of the reduction device is 800-1500°C, preferably 850-1400°C, and more preferably 900-1300°C.

[0028] In the present invention, the iron-containing solid waste is one or more of blast furnace ash, converter ash, electric furnace ash, copper slag, dust and mud produced by hydrometallurgical zinc extraction, and dust and mud produced by pyrometallurgical zinc extraction.

[0029] In the present invention, the additive is one or more of lime, limestone, slaked lime and dolomite.

[0030] In the present invention, the reducing agent is one or more of lignite, bituminous coal, anthracite, coke powder, semi-coke, biomass, organic pyrolytic carbon, and coal tar.

[0031] Preferably, the particle sizes of zinc-containing dust, additives and reducing agents are -1 mm>50%, preferably -200 mesh>50%, and more preferably -200 mesh>80%.

[0032] In the present invention, the cooling in step (4) is dry cooling or wet cooling, preferably dry cooling.

[0033] Preferably, the iron-containing material obtained in step (4) is used as raw material for a converter, a blast furnace or an electric furnace.

[0034] Preferably, the CaO / SiO2 mass ratio in the composite pellets is >0.5, preferably the CaO / SiO2 mass ratio is >1.5, and more preferably the CaO / SiO2 mass ratio is >2.

[0035] Preferably, the particle size of the composite pellets is 1 mm-30 mm, preferably 3 mm-15 mm, and more preferably 3 mm-8 mm.

[0036] Preferably, the moisture content of the composite pellets is 2%-30%, preferably 5%-15%, and more preferably 8%-12%.

[0037] According to a second embodiment provided by the present invention, a precise control method for treating solid waste using a rotary kiln is provided.

[0038] A precise control method for treating solid waste using a rotary kiln, wherein the rotary kiln is provided with a temperature detection device, and the method comprises the following steps:

[0039] 1) Batching and pelletizing: the zinc dust raw material, the reducing agent and the additive are batched and mixed to obtain a mixed material, and the mixed material is added with water and sent to a pelletizing device to obtain composite pellets.

[0040] 2) Pellet reduction: The composite pellets are sent to the tail of the rotary kiln, and then go through the drying section, preheating section, reduction roasting section, and preliminary cooling section to obtain high-temperature slag.

[0041] 3) Temperature control inside the rotary kiln: The temperature detection device detects the temperature inside the rotary kiln and records the real-time temperature T and real-time heating rate S inside the rotary kiln. The temperature field inside the rotary kiln is controlled by adjusting the formula of the composite pellets or the air inlet state of the rotary kiln.

[0042] 4) Utilization of flue gas waste heat and dust removal: In step 2), the hot exhaust gas discharged from the rotary kiln tail is utilized for waste heat and dust removal, and then after flue gas purification, a part of it is used as a high-temperature slag cooling medium, and the other part is discharged.

[0043] 5) High-temperature slag treatment: The high-temperature slag obtained in step 2) is cooled and recycled.

[0044] In the present invention, according to the condition of the composite pellets, the maximum drying temperature that the composite pellets can withstand in the drying section is calculated as T gz , the calculation formula is:

[0045]

[0046] Among them, T gz is the highest drying temperature in the drying section, ℃; K gz is the maximum temperature coefficient of the drying section, with a value of 0.5-1, ℃·mm; R is the alkalinity of the composite pellets, %; m is the alkalinity index of the composite pellets at the highest drying temperature, with a value of 0.1-0.3; D is the average particle size of the composite pellets, mm; n is the average particle size index of the composite pellets at the highest drying temperature, with a value of 0.4-0.6; W is the moisture content of the composite pellets, %; x is the moisture index of the composite pellets at the highest drying temperature, with a value of 0.4-0.6.

[0047] In the present invention, according to the condition of the composite pellets, the maximum temperature rise rate that the composite pellets can withstand in the drying stage is calculated as S gz , the calculation formula is:

[0048]

[0049] Among them, S gz is the maximum heating rate in the drying section, ℃ / min; K s is the maximum heating rate coefficient of the drying section, which is 0.1-0.3, mm / min; a is the alkalinity index of the composite pellets at the maximum heating rate, which is 0.4-0.6; b is the average particle size index of the composite pellets at the maximum heating rate, which is 0.1-0.4; e is 2.71828.

[0050] In the present invention, the basicity R, the average particle size D, and the moisture W of the composite pellets are detected, and the maximum temperature suitable for drying the composite pellets in the drying section is calculated as T. gz .

[0051] When the real-time temperature in the rotary kiln is T>T gz If a rotary kiln without air inlet is used, the maximum drying temperature T that the composite pellets can withstand in the drying stage can be increased by increasing the pellet basicity R, reducing the average pellet size D or reducing the pellet moisture W. gz , so that T gz Greater than or equal to the real-time temperature T in the rotary kiln.

[0052] When the real-time temperature in the rotary kiln is T>T gz If a rotary kiln with air inlet from the kiln body is used, then by reducing the air inlet △Q t , kiln body air inlet △Q s Or kiln exhaust △Q c Reduce the real-time temperature in the rotary kiln so that the real-time temperature in the rotary kiln is T≤T gz .

[0053] When T≤T gz No matter what structure of rotary kiln is used, no adjustment is required.

[0054] As a preference, when T<T gz When (for example, T gz -T>30℃), in order to increase the processing capacity of the rotary kiln or reduce the use of additives, the use of composite pellet additives can be reduced, the average particle size D of the composite pellets can be increased, or the moisture W of the composite pellets can be increased (to improve the balling performance of the composite pellets).

[0055] When using a rotary kiln with air inlet from the kiln body, when T<T gz When (for example, T gz-T>30℃), and the kiln head air inlet △Q can also be increased t , kiln body air inlet △Q s Or kiln exhaust △Q c , which increases the temperature of the drying section in the rotary kiln, thereby increasing the processing capacity of the rotary kiln.

[0056] In the present invention, the basicity R of the composite pellets, the average particle size D of the pellets, and the moisture W of the pellets are detected, and the maximum temperature rise rate suitable for drying the composite pellets in the drying section is calculated as S. gz .

[0057] When the real-time heating speed in the rotary kiln is S>S gz If a rotary kiln without air inlet is used, the maximum temperature rise rate S that the composite pellets can withstand in the drying stage can be increased by increasing the pellet basicity R, reducing the average pellet size D or reducing the pellet moisture W. gz , so that S gz Greater than or equal to the real-time heating rate S in the rotary kiln.

[0058] When the real-time heating speed in the rotary kiln is S>T gz If a rotary kiln with air inlet from the kiln body is used, then by reducing the air inlet △Q t , kiln body air inlet △Q s Or kiln exhaust △Q c Reduce the real-time heating rate in the rotary kiln so that the real-time heating rate in the rotary kiln S≤S gz .

[0059] When S≤S gz No matter what structure of rotary kiln is used, no adjustment is required.

[0060] As a preference, when S<S gz When (for example S gz -S>10℃), in order to improve the processing efficiency of the rotary kiln or reduce the amount of additives used, the amount of composite pellet additives used can be reduced, the average particle size D of the composite pellets can be increased, or the moisture W of the composite pellets can be increased (to improve the balling performance of the composite pellets).

[0061] When using a rotary kiln with air inlet from the kiln body, when S<S gz When (for example S gz -S>10℃), and the kiln head air inlet △Q can also be increased t , kiln body air inlet △Q s Or kiln exhaust △Q c , improve the heating rate of the drying section in the rotary kiln, thereby improving the processing efficiency of the rotary kiln.

[0062] In order to ensure that the composite pellets do not explode, melt or form rings in the drying section of the reduction device, the real-time temperature T in the rotary kiln is controlled by controlling the identity and physical properties of the composite pellets or by controlling the specific process conditions of the reduction device, so that the maximum drying temperature T that the composite pellets can withstand in the drying section is ≤ gz At the same time, the real-time heating rate S in the rotary kiln is ≤ the maximum heating rate S that the composite pellets can withstand in the drying section. gz .

[0063] In the present invention, in step 4), the hot exhaust gas discharged from the rotary kiln tail is subjected to waste heat power generation and dust removal to collect zinc oxide dust, and then a part of it is used as a dry cooling medium after flue gas purification, and the rest is discharged into the atmosphere.

[0064] In the present invention, the filling rate of the rotary kiln is 5%-30%, preferably 10%-25%, and more preferably 15%-20%.

[0065] In the present invention, in step 5), the high-temperature slag is cooled by dry cooling, and the dry cooling equipment includes one of a cylindrical cooler, a belt cooler, a vertical cooler, and a two-stage cooler, and the cooling medium is one or more of nitrogen, helium, argon, carbon dioxide, hydrogen, carbon monoxide, methane, blast furnace gas, coke oven gas, converter gas, and rotary kiln tail gas. After the high-temperature slag is dry-cooled, a high-metallization slag is obtained, and the temperature of the high-metallization slag after dry cooling is 15-800°C, preferably 20-300°C, and more preferably 25-100°C.

[0066] After cooling, the high metallization slag is screened, and the high metallization slag with a diameter less than 5 mm is used as sintering raw material for ore blending. The high metallization slag with a diameter greater than 5 mm is reduced agglomerate, which is used as converter steelmaking additive.

[0067] In the present invention, in step 5), the high-temperature slag is cooled by water quenching, and low metallization slag is obtained after water cooling. The temperature of the low metallization slag after water quenching is 15-800°C, preferably 20-300°C, and more preferably 25-100°C.

[0068] The low metallization slag obtained after cooling is screened, and the low metallization slag with a diameter less than 5 mm is used as sintering raw material for ore blending. The low metallization slag with a diameter greater than 5 mm is a reduction agglomerate, which is used as an additive for converter steelmaking.

[0069] In the prior art, when using traditional rotary kiln and rotary hearth furnace processes for pyrolysis or combustion reduction of metallurgical solid waste, powder or green balls are put into the kiln, the temperature field in the kiln is improperly controlled, and the relationship between the temperature field in the drying section, preheating section, and reduction section and the performance of the pellet materials entering the kiln is unclear, which can easily cause the pellets to burst in the kiln and increase the powder, resulting in low product quality. When the temperature in the rotary kiln is too high, the ash is likely to melt, and then the temperature is too low, and the molten ash condenses again. Due to the uneven temperature distribution along the kiln body of the rotary kiln, the reduction efficiency is not high, and ringing is likely to occur, affecting normal production.

[0070] In the prior art, a reduction device (such as a rotary kiln) is used to treat iron-containing solid waste. The drying section of the reduction device usually relies on the heat brought by the flue gas from the reduction section at the head of the kiln to the tail of the kiln for drying, and is not adjusted according to the specific conditions of the composition and physical properties of the materials transported to the reduction device. Even if the prior art provides a wide range of adaptability of the drying section of the reduction device, the temperature of the drying section of the reduction device is not adaptively matched according to the characteristics of the input material. However, when the material is transported to the reduction device, the first section it passes through is the drying section; if the temperature of the drying section is too low, the drying effect cannot be achieved, which affects the subsequent preheating and reduction processes, resulting in unqualified material treatment and the preset treatment purpose. If the temperature of the drying section is too high, the material will directly burst, melt, and form circles after entering the reduction device, which will also affect the operation of the material in the reduction device and the effects of the material in other stages in the reduction device; it will also damage the reduction device.

[0071] The inventors of this application have found through research and experiments that the suitable temperature and suitable heating rate of the material in the drying section of the reduction device are directly related to the composition and physical characteristics of the material itself. Since the sources of iron-containing solid waste are very wide, the composition varies greatly, and the ball forming performance also varies greatly, if only considering adding alkali according to the ball forming performance, or balling according to the conventional requirements of the treatment process, it will affect the process of the material in the drying section of the reduction device.

[0072] In order to solve the problems of material bursting, ringing and melting in the drying section of the reduction device, firstly, the maximum temperature and maximum heating rate that the material can withstand in the drying section of the reduction device are calculated according to the specific characteristics of the material (composite pellets). The temperature of the reduction device is measured in real time along the length direction. When the temperature of the drying section of the reduction device is too high or too low, the alkalinity, moisture, particle size of the composite pellets are adjusted, or the air inlet △Q of the kiln head of the drying section of the reduction device is adjusted. t , kiln body air inlet △Q s 、Kiln body exhaust △Q c Adjustments are made to achieve precise control of the kiln temperature so that the temperature field in the drying section of the reduction unit matches the material to be treated.

[0073] Preferably, the reduction device is a rotary kiln, and there are two types of rotary kilns: one is a rotary kiln with air intake in the kiln body, and the other is a rotary kiln without air intake in the kiln body. The kiln head of the rotary kiln is provided with an air inlet, and the kiln body is optionally provided with an air inlet pipe and an exhaust pipe. The left side of the rotary kiln is the kiln tail, and the right side is the kiln head. From the kiln tail to the kiln head, the drying section, preheating section, reduction roasting section, and preliminary cooling section are arranged in sequence. The kiln tail is the feed port end, and the kiln head is the discharge port end. Before the material enters the reduction device, it first passes through a pellet detection device to detect the alkalinity, moisture, and particle size of the pellets. A temperature detection device is provided on the kiln body of the rotary kiln, which can be used to detect the temperature and heating rate of each section of the drying section, preheating section, reduction roasting section, and preliminary cooling section. The method firstly mixes and blends the iron-containing solid waste, reducing agent and additive to obtain a mixed material (the mixing equipment is a powerful mixer or a drum mixer), and then adds water to the mixed material and sends it to a ball-making device to obtain composite pellets. The optimal reduction is achieved by accurately configuring the materials, wherein the filling rate of the rotary kiln is 5%-30%, preferably 10%-25%, and more preferably 15%-20%. By controlling the filling rate of the rotary kiln, the surface area of ​​the material in the rotary kiln exposed to the space can be reduced, and the amount of CO on the surface of the rotary kiln material is greatly increased, which is conducive to enhancing the reducing atmosphere in the kiln and reducing the reoxidation rate. Secondly, the composite pellets are tested by a pellet detection device to obtain various coefficients of the pellets, and the tested composite pellets are sent to the tail of the rotary kiln, and then reduced and cooled through the drying section, preheating section, reduction roasting section, and preliminary cooling section to obtain high-temperature slag. Again, the temperature detection device detects the temperature in the drying section of the rotary kiln, and records the real-time temperature T and real-time heating rate S of the drying section of the rotary kiln, determines whether the real-time temperature and real-time heating rate of the drying section of the kiln are lower than the maximum temperature and maximum heating rate that the material can withstand, and adjusts the various parameters of the composite pellets or the air intake of the drying section of the rotary kiln according to the maximum temperature and maximum heating rate to control the temperature field of the drying section of the rotary kiln. Then, the hot exhaust gas discharged from the tail of the rotary kiln is used for waste heat utilization, dust removal and recovery of secondary zinc oxide. The exhaust gas after dust removal is purified by flue gas, and a part is used as a high-temperature slag cooling medium, and the other part is discharged. Finally, the high-temperature slag obtained after reduction cooling is dry-cooled or water-quenched, and recycled. The method detects and records various coefficients of composite pellets in a rotary kiln, calculates the maximum temperature and the maximum heating rate of the drying section according to the various coefficients of the pellets, and compares them with the real-time temperature and the real-time heating rate in the rotary kiln, adjusts the alkalinity, moisture, and particle size of the pellets or the air volume of the kiln head air inlet, kiln body air inlet, and kiln body exhaust of the rotary kiln, thereby controlling the temperature field of the drying section in the rotary kiln and preventing the material from melting in large quantities under the high-temperature and high-reducing atmosphere conditions in the drying section, resulting in kiln calcination.

[0074] In the present invention, the maximum temperature of the drying section is T gz , the calculation formula is:

[0075]

[0076] The inventor concluded through research and experiments that the maximum temperature that the material can withstand in the drying section is directly related to the alkalinity of the material, the particle size of the material, and the moisture content of the material. Through parallel tests and cross-tests, it was concluded that the maximum temperature of the above drying section is T gz The formula has universal adaptability through the adjustment of the maximum temperature coefficient of the drying section.

[0077] In the present invention, the maximum temperature rise rate of the drying section is S gz , the calculation formula is:

[0078]

[0079] The inventor concluded through research and experiments that the maximum temperature rise rate that the material can withstand in the drying section is also directly related to the alkalinity of the material, the particle size of the material, and the moisture content of the material. Through parallel tests and cross-tests, it was concluded that the maximum temperature rise rate of the above drying section is S gz The formula is universally adaptable by adjusting the maximum temperature rise rate coefficient of the drying section.

[0080] In the present invention, the basicity of the composite pellet refers to the calcium-silicon ratio of the composite pellet, specifically the ratio of the weight of calcium oxide to the weight of silicon oxide in the composite pellet (mass ratio); the basicity can be obtained by material composition analysis. The particle size of the composite pellet is just the average outer diameter of the pellet in the whole material, which is obtained by direct measurement. The moisture content of the composite pellet is the weight percentage of the moisture in the composite pellet to the whole composite pellet, and the moisture content is obtained by drying method.

[0081] In the present invention, the inventors fitted the formula through experiments, the unit of alkalinity is %, the unit of particle size is mm, the unit of moisture content is %, and each coefficient has no unit. Each performance index is converted into a corresponding unit, and through formula fitting, the unit of the maximum drying temperature is ℃, and the unit of the maximum heating rate is ℃ / min. That is to say, in the present invention, each parameter in the formula is converted into an agreed unit, and the maximum drying temperature and the maximum heating rate can be directly calculated through the fitting formula.

[0082] In the present invention, the temperature in the drying section of the reduction device is also detected (by thermocouple). In the process of treating iron-containing solid waste, the basicity R of the composite pellets, the average particle size D of the composite pellets, and the moisture content W of the composite pellets are first measured by the pellet detection device, and the maximum temperature that the composite pellets can withstand after entering the drying section for drying is calculated as T. gz , according to the maximum temperature T that the drying section can withstand gzCompared with T. Among them, the rotary kiln can be a rotary kiln without air entering the kiln body or a rotary kiln with air entering the kiln body. When T>T gz When using a rotary kiln without air inlet to the kiln body, the alkalinity of the composite pellets will be increased, the average particle size of the composite pellets will be reduced, or the moisture content of the composite pellets will be reduced. s Or kiln exhaust △Q c ; or at the same time increase the basicity of the composite pellets, reduce the average particle size of the composite pellets or reduce the moisture content of the composite pellets. When T≤T gz As a preference, when T is much smaller than T gz When the kiln body is not air-inletted, the alkalinity of the composite pellets is reduced, the average particle size of the composite pellets is increased, or the moisture content of the composite pellets is increased. When the kiln body is air-inletted, the kiln head air inlet △Q is increased. t , kiln body air inlet △Q s Or kiln exhaust △Q c ; or reduce the basicity of the composite pellets, increase the average particle size of the composite pellets, or increase the moisture content of the composite pellets at the same time. By controlling the maximum temperature of the drying section and adjusting the temperature field in the rotary kiln, the kiln calcination phenomenon in the rotary kiln can be effectively prevented. At the same time, according to the maximum temperature that the composite pellets can withstand, the process conditions of the reduction device are adjusted in real time to ensure the treatment efficiency of the reduction device and the quality of the pellet treatment, thereby ensuring the removal of zinc in the iron-containing solid waste and the quality of the high-temperature iron slag.

[0083] In the present invention, the real-time temperature rise rate S in the drying section of the reduction device can be calculated by detecting the temperature change in the drying section of the reduction device per unit time. In the process of treating iron-containing solid waste, the alkalinity R of the composite pellets, the average particle size D of the composite pellets, and the moisture content W of the composite pellets are first detected by the pellet detection device, and the calculated maximum temperature T gz Calculate that the maximum temperature rise rate that the composite pellets can withstand after entering the drying section is S gz . According to the maximum temperature rise rate S that the drying section can withstand gz Compare with the heating speed S. Among them, the rotary kiln can be a rotary kiln without air inlet or a rotary kiln with air inlet. When S>S gz The use of a rotary kiln with air inlet to the kiln body can increase the alkalinity of the composite pellets, reduce the average particle size of the composite pellets, or reduce the moisture content of the composite pellets. The use of a rotary kiln without air inlet to the kiln body can reduce the kiln head air inlet △Qt, kiln body air inlet △Q s Or kiln exhaust △Q c ; or at the same time increase the basicity of the composite pellets, reduce the average particle size of the composite pellets or reduce the moisture content of the composite pellets. gz , no adjustment is required. As a preference, when S is much smaller than S gzThe use of a rotary kiln with air inlet in the kiln body will reduce the alkalinity of the composite pellets, increase the average particle size of the composite pellets, or increase the moisture content of the composite pellets. The use of a rotary kiln without air inlet in the kiln body will increase the air inlet at the kiln head △Q t , kiln body air inlet △Q s Or kiln exhaust △Q c ; or reduce the basicity of the composite pellets, increase the average particle size of the composite pellets, or increase the moisture content of the composite pellets at the same time. By controlling the maximum heating rate of the drying section and adjusting the temperature field in the rotary kiln, the kiln calcination phenomenon in the rotary kiln can be effectively prevented. At the same time, according to the maximum heating rate that the composite pellets can withstand, the process conditions of the reduction device are adjusted in real time to ensure the treatment efficiency of the reduction device and the quality of the pellet treatment, thereby ensuring the removal of zinc in the iron-containing solid waste and the quality of the high-temperature iron slag.

[0084] In the present invention, by clarifying the relationship between the temperature field in the drying section of the reduction device and the performance of the pellet material entering the kiln, the temperature in the drying section of the reduction device is controlled, which can reduce the composite pellets from bursting in the kiln, avoid pellet bursting and powder ringing, and improve product quality. The temperature field distribution in the kiln is regulated according to the performance of the pellets, and efficient reduction and dezincification of iron-containing solid waste is achieved, and the quality of the material after reduction treatment is also guaranteed.

[0085] In the present invention, the iron-containing solid waste can be all iron-containing and zinc-containing solid wastes generated in industrial production. For example, zinc-containing dust includes one or more of blast furnace ash, converter ash, electric furnace ash, copper slag, dust mud generated by wet zinc extraction and dust mud generated by pyrometallurgical zinc extraction. Additives include one or more of lime, limestone, slaked lime and dolomite. Reducing agents include one or more of lignite, bituminous coal, anthracite, coke powder, blue carbon, biomass, organic pyrolytic carbon and coal tar.

[0086] Preferably, in order to ensure the ball-forming performance of the composite pellets, the present invention further includes pretreatment of the raw materials, and the pretreatment is to make the particle size of the zinc-containing dust, additives, and reducing agents entering the mixing device all be -1mm>50%, preferably -200 mesh>50%, and more preferably -200 mesh>80%. By controlling the particle size of the zinc-containing dust, additives, and reducing agents, the stability of the materials in the mixing and pelletizing process can be improved, the ball-forming performance of the composite pellets can be ensured, and the efficiency of pellet reduction can be improved.

[0087] In the present invention, it is verified by experiments that the CaO / SiO2 mass ratio of the mixed material after batching containing zinc dust, additives and reducing agents is greater than 0.5, preferably the CaO / SiO2 mass ratio is greater than 1.5, and more preferably the CaO / SiO2 mass ratio is greater than 2. The fixed carbon content of the mixed material after batching is 5%-30%, preferably 8%-25%, and more preferably 10%-20%.

[0088] In the present invention, the pelletizing equipment can be selected from conventional pelletizing machines in the prior art, such as a cylinder pelletizing machine, a disc pelletizing machine, or a strong disturbance pelletizing machine.

[0089] According to the common treatment in the actual production process, the composite pellets prepared by the inventor have a particle size of 1mm-30mm, preferably 3mm-15mm, and more preferably 3mm-8mm. The moisture content of the composite pellets is 2%-30%, preferably 5%-15%, and more preferably 8%-12%. By controlling the particle size, the air permeability of the pellets is improved, the reduction efficiency is improved, the quality index is improved, the size of the formed pellets is adjusted in time, and the height of the pellets and the rotary kiln are matched. The pellets are gradually heated and dried during the reduction process, thereby improving the reduction efficiency.

[0090] In the present invention, the hot exhaust gas discharged from the tail of the rotary kiln can be used for waste heat power generation, and the exhaust gas after waste heat utilization is dedusted to collect zinc oxide dust, and then a part of it is used as a dry cooling medium after flue gas purification, and the remaining part is discharged into the atmosphere. Among them, the rotary kiln is reduced and cooled to obtain high-temperature slag, and the high-temperature slag can be cooled by dry cooling or water quenching to obtain slag with different metallization rates. The dry cooling equipment includes one of a cylindrical cooler, a belt cooler, a vertical cooler, and a two-stage cooler, and the cooling medium is one or more of nitrogen, helium, argon, carbon dioxide, hydrogen, carbon monoxide, methane, blast furnace gas, coke oven gas, converter gas, and rotary kiln tail gas. After dry cooling, the high-temperature slag obtains high-metallization slag, and the temperature of the high-metallization slag after dry cooling is 15-800°C, preferably 20-300°C, and more preferably 25-100°C. Among them, after cooling, the high metallization slag is screened, and the material less than 5mm contains reduced zinc-containing dust and unreacted coke powder, which is used as sintering raw material for ore matching and consumption, and the material greater than 5mm is a reduction agglomerate, which contains a high iron content and a high metallization rate, and is used as a converter steelmaking additive. The high-temperature slag cooled by water quenching is water-cooled to obtain low metallization slag, and the temperature of the low metallization slag after water quenching is 15-800℃, preferably 20-300℃, and more preferably 25-100℃. Among them, after cooling, the low metallization slag is screened, and the material less than 5mm contains reduced zinc-containing dust and unreacted coke powder, which is used as sintering raw material for ore matching and consumption, and the material greater than 5mm is a reduction agglomerate, which contains a high iron content and a high metallization rate, and is used as a converter steelmaking additive. Efficiency is improved by dry cooling and water quenching cooling.

[0091] Compared with the prior art, the present invention has the following beneficial technical effects:

[0092] 1. The present invention controls the maximum temperature and the maximum heating rate of the drying section of the reduction device according to the different sources of raw materials, the composition of the composite pellets and the specific properties of the materials, which can effectively avoid the pellets from bursting after entering the kiln; at the same time, the temperature field distribution in the kiln is regulated according to the performance of the pellets to achieve efficient reduction and dezincification of zinc-containing dust and mud pellets.

[0093] 2. The present invention detects various coefficients of the composite pellets, calculates the maximum temperature and maximum heating rate of the drying section in the rotary kiln according to the alkalinity, particle size and moisture of the composite pellets, and adjusts the alkalinity, particle size and moisture of the composite pellets according to the actual detected temperature, thereby balancing the temperature field in the drying section of the reduction device, thereby being able to more accurately control the pellet temperature in each process section, and also making the temperature control of the present application more precise, so as to guide production practice.

[0094] 3. The present invention optimizes the ingredients of the composite pellets and feeds them into the reduction device for reduction. At the same time, the temperature and heating rate in the reduction device are monitored to avoid a large amount of melting of the material under the high temperature and high reducing atmosphere in the reduction device, to prevent the material from bursting and ringing in the reduction device, and to improve the quality of the reduced product of the reduction device. BRIEF DESCRIPTION OF THE DRAWINGS

[0095] Figure 1 This is a flow chart of the precise control method for treating solid waste using a rotary kiln according to the present invention;

[0096] Figure 2 This is a flow chart of adjusting the maximum temperature of the drying section when the rotary kiln without air entering the kiln body is used in the present invention;

[0097] Figure 3 It is a flow chart of adjusting the maximum temperature of the drying section when the rotary kiln with air entering the kiln body is adopted in the present invention;

[0098] Figure 4 This is a flow chart of adjusting the maximum heating speed of the drying section when the rotary kiln without air entering the kiln body is used in the present invention;

[0099] Figure 5 The present invention is a flow chart for adjusting the maximum heating speed of the drying section when the rotary kiln with air entering the kiln body is adopted. DETAILED DESCRIPTION

[0100] The technical solution of the present invention is illustrated below by way of example, and the scope of protection requested by the present invention includes but is not limited to the following embodiments.

[0101] Example 1

[0102] A method for resource utilization of iron-containing solid waste, the method comprising the following steps:

[0103] (1) mixing and pelletizing iron-containing solid waste, limestone and lignite to obtain composite pellets;

[0104] (2) The composite pellets are fed into a reduction device and sequentially passed through a drying section, a preheating section, a reduction roasting section, and a preliminary cooling section of the reduction device to obtain high-temperature iron slag;

[0105] The drying temperature and the heating rate in the drying section of the reduction device are controlled according to the particle size, alkalinity and moisture content of the composite pellets.

[0106] Example 2

[0107] Example 1 was repeated, except that the drying temperature in the drying section of the reduction device was controlled according to the particle size, alkalinity and moisture content of the composite pellets as follows:

[0108]

[0109] Among them, T gz is the highest drying temperature in the drying section, ℃; K gz is the maximum temperature coefficient of the drying section, with a value of 0.5-1, ℃·mm; R is the alkalinity of the composite pellets, %; m is the alkalinity index of the composite pellets at the highest drying temperature, with a value of 0.1-0.3; D is the average particle size of the composite pellets, mm; n is the average particle size index of the composite pellets at the highest drying temperature, with a value of 0.4-0.6; W is the moisture content of the composite pellets, %; x is the moisture index of the composite pellets at the highest drying temperature, with a value of 0.4-0.6.

[0110] Example 3

[0111] Example 2 was repeated, except that the temperature rise rate in the drying section of the reduction device was controlled according to the particle size, alkalinity and moisture content of the composite pellets as follows:

[0112]

[0113] Among them, S gz is the maximum heating rate in the drying section, ℃ / min; K s is the maximum heating rate coefficient of the drying section, which is 0.1-0.3, mm / min; a is the alkalinity index of the composite pellets at the maximum heating rate, which is 0.4-0.6; b is the average particle size index of the composite pellets at the maximum heating rate, which is 0.1-0.4; e is 2.71828.

[0114] Example 4

[0115] A method for resource utilization of iron-containing solid waste by using a rotary kiln, wherein the iron-containing solid waste is iron-containing and zinc-containing dust mud; the method specifically comprises:

[0116] (1) mixing iron-containing zinc-containing dust, limestone and lignite, and pelletizing to obtain composite pellets;

[0117] (2) The composite pellets are fed into a rotary kiln, where they pass through a drying section, a preheating section, a reduction roasting section, and a preliminary cooling section in sequence;

[0118] (3) The flue gas discharged from the rotary kiln is optionally subjected to waste heat utilization, and then dust removal is performed to obtain the zinc-containing material, and the gas after dust removal is optionally subjected to flue gas purification before being discharged;

[0119] (4) The slag phase discharged from the rotary kiln is cooled to obtain iron-containing material.

[0120] Example 5

[0121] Example 4 was repeated, except that the drying temperature in the drying section of the reduction device was controlled according to the particle size, alkalinity and moisture content of the composite pellets as follows:

[0122]

[0123] Among them, T gz is the highest drying temperature in the drying section, ℃; K gz is the maximum temperature coefficient of the drying section, with a value of 0.5-1, ℃·mm; R is the alkalinity of the composite pellets, %; m is the alkalinity index of the composite pellets at the highest drying temperature, with a value of 0.1-0.3; D is the average particle size of the composite pellets, mm; n is the average particle size index of the composite pellets at the highest drying temperature, with a value of 0.4-0.6; W is the moisture content of the composite pellets, %; x is the moisture index of the composite pellets at the highest drying temperature, with a value of 0.4-0.6.

[0124] Example 6

[0125] Example 5 was repeated, except that the temperature rise rate in the drying section of the reduction device was controlled according to the particle size, alkalinity and moisture content of the composite pellets as follows:

[0126]

[0127] Among them, S gz is the maximum heating rate in the drying section, ℃ / min; K s is the maximum heating rate coefficient of the drying section, which is 0.1-0.3, mm / min; a is the alkalinity index of the composite pellets at the maximum heating rate, which is 0.4-0.6; b is the average particle size index of the composite pellets at the maximum heating rate, which is 0.1-0.4; e is 2.71828.

[0128] Example 7

[0129] Example 6 was repeated, except that the rotary kiln was a rotary kiln without air inlet; the process of step (1) was adjusted according to the process conditions of the drying section on the rotary kiln to control the particle size, alkalinity and moisture content of the prepared composite pellets, so that T gz Greater than or equal to the temperature in the drying section of the rotary kiln;

[0130] According to the process conditions of the drying section on the rotary kiln, the process of step (1) is adjusted to control the particle size, basicity and moisture content of the prepared composite pellets so that S gz Greater than or equal to the temperature in the drying section of the rotary kiln.

[0131] Example 8

[0132] Example 6 was repeated, except that the rotary kiln was a kiln body air inlet rotary kiln; according to the particle size, alkalinity and moisture content of the composite pellets prepared in step (1), the air inlet volume of the rotary kiln was adjusted so that the temperature in the drying section of the rotary kiln was less than or equal to T gz ;

[0133] According to the particle size, alkalinity and moisture content of the composite pellets prepared in step (1), the air inlet of the rotary kiln is adjusted so that the heating rate in the drying section of the rotary kiln is less than or equal to S gz .

[0134] Example 9

[0135] Example 8 was repeated except that the iron-containing solid waste was blast furnace ash.

[0136] Example 10

[0137] Example 8 was repeated, except that the iron-containing solid waste was converter ash.

[0138] Embodiment 11

[0139] Example 8 was repeated, except that the iron-containing solid waste was electric furnace ash.

[0140] Example 12

[0141] Example 8 was repeated except that the iron-containing solid waste was dust and mud produced by wet zinc extraction.

[0142] Example 13

[0143] Example 8 was repeated except that the additive was dolomite.

[0144] Embodiment 14

[0145] Example 8 was repeated except that the reducing agent was coke powder.

[0146] Embodiment 15

[0147] Example 8 was repeated except that the reducing agent was biomass.

[0148] Application Example A

[0149] According to the data measured by the pellet detection device and the maximum temperature of the drying section, T gz , the calculation formula is:

[0150]

[0151] Among them, T gz is the highest drying temperature in the drying section, ℃; K gz is the highest temperature coefficient of the drying section, ℃·mm; R is the alkalinity of the composite pellets, %; m is the alkalinity index of the composite pellets at the highest drying temperature; D is the average particle size of the composite pellets, mm; n is the average particle size index of the composite pellets at the highest drying temperature; W is the moisture content of the composite pellets, %; x is the moisture index of the composite pellets at the highest drying temperature. The calculated data are:

[0152] Table 1

[0153]

[0154]

[0155] Through experiments, it was found that the moisture content and particle size of the pellets have a great influence on the maximum temperature that the composite pellets can withstand in the drying section of the reduction device. If the material is reduced according to experience and conventional procedures, the composite pellets are likely to burst and melt in the drying section of the reduction device.

[0156] According to the data measured by the pellet detection device combined with the highest drying temperature T in the drying section gz , calculate the maximum temperature rise rate of the drying section as:

[0157]

[0158] Among them, S gz is the maximum heating rate in the drying section, ℃ / min; K s is the maximum temperature rise rate coefficient of the drying section, mm / min; a is the composite pellet basicity index of the maximum temperature rise rate; b is the composite pellet average particle size index of the maximum temperature rise rate; e is 2.71828. The calculated data are:

[0159] Table 2

[0160]

[0161]

[0162] Through experimental verification, it is found that the moisture content and particle size of the pellets have a great influence on the heating rate, especially the moisture content. If the material is reduced according to experience and conventional procedures, the temperature rises too fast in the drying section of the reduction device. Since the pellets have not yet solidified, the composite pellets are very likely to burst and melt in the drying section of the reduction device, and the material is easy to form a ring in the reduction device.

[0163] Application Example B

[0164] The technical scheme described in Example 8 is adopted, and the same batch of iron-containing solid waste, limestone and lignite are used, wherein each raw material is ground to -200 mesh>50%. The composite pellets are obtained by balling, and the same rotary kiln with air inlet is used, and the filling rate of the rotary kiln is 20%; the temperature of the preheating section is controlled to 900°C, the temperature of the reduction section is controlled to 1100°C, and the residence time of the material in the reduction section is 40min; vertical cooling is uniformly adopted to cool to 80°C. Different drying section temperatures and drying section heating rates are controlled, and the proportion of materials smaller than 5mm in the materials discharged from the rotary kiln is detected; the recorded data are as follows:

[0165]

[0166]

[0167] Through experiments, it was found that by treating the same batch of iron-containing solid waste, adjusting the alkalinity, particle size and moisture content of the prepared composite pellets, and controlling the temperature of the drying section of the reduction device to be less than or equal to the maximum drying temperature that the composite pellets can withstand, and controlling the heating rate in the drying section of the reduction device to be less than or equal to the maximum heating rate that the composite pellets can withstand, the bursting of the composite pellets in the reduction device can be reduced, and the proportion of materials less than 5 mm in the total discharged materials can be reduced, thereby reducing the phenomenon of material ringing and melting in the rotary kiln.

Claims

1. A method for resource utilization of iron-containing solid waste, the method comprising the following steps: (1) mixing and pelletizing the iron-containing solid waste, the reducing agent, and the additive to obtain composite pellets; (2) The composite pellets are fed into a reduction device and sequentially passed through a drying section, a preheating section, a reduction roasting section, and a preliminary cooling section of the reduction device to obtain high-temperature iron slag; The invention is characterized in that: the drying temperature and the heating rate in the drying section of the reduction device are controlled according to the particle size, alkalinity and moisture content of the composite pellets; the drying temperature in the drying section of the reduction device is controlled specifically as follows: Among them, T gz is the highest drying temperature in the drying section, ℃; K gz is the maximum temperature coefficient of the drying section, with a value of 0.5-1, ℃·mm; R is the alkalinity of the composite pellets, %; m is the alkalinity index of the composite pellets at the highest drying temperature, with a value of 0.1-0.3; D is the average particle size of the composite pellets, mm; n is the average particle size index of the composite pellets at the highest drying temperature, with a value of 0.4-0.6; W is the moisture content of the composite pellets, %; x is the moisture index of the composite pellets at the highest drying temperature, with a value of 0.4-0.6; The specific temperature rise rate in the drying section of the reduction device is controlled as follows: Among them, S gz is the maximum heating rate in the drying section, ℃ / min; K s is the maximum heating rate coefficient of the drying section, which is 0.1-0.3, mm / min; a is the alkalinity index of the composite pellets at the maximum heating rate, which is 0.4-0.6; b is the average particle size index of the composite pellets at the maximum heating rate, which is 0.1-0.4; e is 2.71828.

2. The method according to claim 1, characterized in that: The reduction device is a rotary kiln, and the iron-containing solid waste is iron-containing and zinc-containing dust mud; the method is specifically: (1) mixing iron-containing zinc-containing dust, a reducing agent, and an additive, and pelletizing to obtain composite pellets; (2) The composite pellets are fed into a rotary kiln, where they pass through a drying section, a preheating section, a reduction roasting section, and a preliminary cooling section in sequence; (3) The flue gas discharged from the rotary kiln is optionally subjected to waste heat utilization, and then dust removal is performed to obtain the zinc-containing material, and the gas after dust removal is optionally subjected to flue gas purification before being discharged; (4) The slag phase discharged from the rotary kiln is cooled to obtain iron-containing material.

3. The method according to claim 2, characterized in that: The rotary kiln is a rotary kiln without air inlet into the kiln body; according to the process conditions of the drying section on the rotary kiln, the process of step (1) is adjusted to control the particle size, alkalinity and moisture content of the prepared composite pellets, so that T gz Greater than or equal to the temperature in the drying section of the rotary kiln; According to the process conditions of the drying section on the rotary kiln, the process of step (1) is adjusted to control the particle size, basicity and moisture content of the prepared composite pellets so that S gz Greater than or equal to the temperature in the drying section of the rotary kiln.

4. The method according to claim 2, characterized in that: The rotary kiln is a kiln body air inlet rotary kiln; according to the particle size, alkalinity and moisture content of the composite pellets prepared in step (1), the air inlet volume of the rotary kiln is adjusted so that the temperature in the drying section of the rotary kiln is less than or equal to T gz ; According to the particle size, alkalinity and moisture content of the composite pellets prepared in step (1), the air inlet of the rotary kiln is adjusted so that the heating rate in the drying section of the rotary kiln is less than or equal to S gz .

5. The method according to any one of claims 1 to 4, characterized in that: The temperature in the preheating section of the reduction device is 500-1000°C; the temperature in the reduction roasting section of the reduction device is 800-1500°C.

6. The method according to claim 5, characterized in that: The temperature in the preheating section of the reduction device is 600-950°C; the temperature in the reduction roasting section of the reduction device is 850-1400°C.

7. The method according to claim 6, characterized in that: The temperature in the preheating section of the reduction device is 700-900°C; the temperature in the reduction roasting section of the reduction device is 900-1300°C.

8. The method according to any one of claims 1-4, 6-7, characterized in that: The iron-containing solid waste is one or more of blast furnace ash, converter ash, electric furnace ash, copper slag, dust and mud produced by wet zinc extraction, and dust and mud produced by pyrometallurgical zinc extraction; the additive is one or more of lime, limestone, slaked lime, and dolomite; the reducing agent is one or more of lignite, bituminous coal, anthracite, coke powder, lignite, biomass, organic pyrolytic carbon, and coal tar.

9. The method according to claim 5, characterized in that: The iron-containing solid waste is one or more of blast furnace ash, converter ash, electric furnace ash, copper slag, dust and mud produced by wet zinc extraction, and dust and mud produced by pyrometallurgical zinc extraction; the additive is one or more of lime, limestone, slaked lime, and dolomite; the reducing agent is one or more of lignite, bituminous coal, anthracite, coke powder, lignite, biomass, organic pyrolytic carbon, and coal tar.

10. The method according to claim 8, characterized in that: The particle size of zinc dust, additives and reducing agents is -1mm>50%.

11. The method according to claim 9, characterized in that: The particle size of zinc dust, additives and reducing agents is -1mm>50%.

12. The method according to claim 10 or 11, characterized in that: The particle size of zinc dust, additives and reducing agents is -200 mesh>50%.

13. The method according to claim 12, characterized in that: The particle size of zinc dust, additives and reducing agents is -200 mesh>80%.

14. The method according to claim 2, characterized in that: The cooling in step (4) is dry cooling or wet cooling; and / or The iron-containing material obtained in step (4) is used as raw material for a converter, a blast furnace or an electric furnace.

15. The method according to claim 14, characterized in that: The cooling in step (4) is dry cooling.

16. The method according to any one of claims 1-4, 6-7, 9-11, 13-15, characterized in that: The CaO / SiO2 mass ratio in the composite pellets is >0.5; The particle size of composite pellets is 1mm-30mm; The moisture content of the composite pellets is 2%-30%.

17. The method according to claim 5, characterized in that: The CaO / SiO2 mass ratio in the composite pellets is >0.5; The particle size of composite pellets is 1mm-30mm; The moisture content of the composite pellets is 2%-30%.

18. The method according to claim 16, characterized in that: The CaO / SiO2 mass ratio in the composite pellets is >1.5; The particle size of composite pellets is 3mm-15mm; The moisture content of the composite pellets is 5%-15%.

19. The method according to claim 17, characterized in that: The CaO / SiO2 mass ratio in the composite pellets is >1.5; The particle size of composite pellets is 3mm-15mm; The moisture content of the composite pellets is 5%-15%.

20. The method according to claim 18 or 19, characterized in that: The CaO / SiO2 mass ratio in the composite pellets is >2; The particle size of composite pellets is 3mm-8mm; The moisture content of the composite pellets is 8%-12%.