An extraction process for separating cobalt and magnesium

By using P507 and Mextral@V10 as a mixed extractant, and combining countercurrent extraction, washing, and back-extraction processes, the problem of high cobalt loss rate in cobalt-magnesium separation was solved, achieving efficient cobalt-magnesium separation and the preparation of battery-grade cobalt sulfate.

CN118127325BActive Publication Date: 2024-11-05湖南金源新材料循环利用有限公司
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410203867.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-02-23
Publication Date
2024-11-05
Estimated Expiration
2044-02-23

AI Technical Summary

Technical Problem

Existing cobalt-magnesium separation methods suffer from high cobalt loss rates and low product purity. Furthermore, fluoride impurities introduced during the extraction process affect the quality of cobalt sulfate products and cause environmental pollution.

Method used

Using P507 and Mextral@V10 as a mixed extractant, combined with countercurrent extraction, countercurrent washing and back-extraction processes, and controlling the O/A ratio and pH value, we can achieve efficient separation of cobalt and magnesium, reduce the loss rate of cobalt and improve product purity.

Benefits of technology

This significantly improved the extraction efficiency of cobalt, reduced the loss rate of cobalt, and achieved efficient separation of cobalt and magnesium, producing battery-grade cobalt sulfate products that meet the raw material requirements of battery materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118127325B_ABST
    Figure CN118127325B_ABST
Patent Text Reader

Abstract

The present invention discloses an extraction process for separating cobalt and magnesium, and belongs to the technical field of hydrometallurgy. The extraction process provided by the present invention comprises the following steps: S1. Using P507 and Mextral@V10 as mixed extractants, extracting the cobalt-magnesium mixed solution to obtain a loaded organic phase and a raffinate phase; S2. Controlling the O / A ratio to be 9-11:1, and performing 15-17 levels of countercurrent washing on the loaded organic phase with a sulfuric acid aqueous solution having a concentration of 0.8-1.2 mol / L to obtain a washing raffinate and a washed loaded organic phase; S3. Back-extracting cobalt from the washed loaded organic phase. The extraction process for separating cobalt and magnesium provided by the present invention can effectively reduce the loss rate of cobalt and increase the content of impurity magnesium in the obtained cobalt product.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of hydrometallurgy, and in particular to an extraction process for separating cobalt and magnesium. Background Art

[0002] When two immiscible and chemically non-reactive phases come into contact, part or most of the dissolved substance (one or several) in one phase is transferred to another phase. This mass transfer (or dissolution) process is called extraction.

[0003] With the rapid development of the new energy vehicle industry and the gradual maturity of the application technology of nickel-cobalt-manganese ternary materials in the field of power batteries, the recycling industry of waste battery positive electrode materials will also usher in a booming development. In wet recycling, magnesium enters the leaching solution together with cobalt during the leaching process. The separation of cobalt and magnesium is currently a major problem in the wet extraction of cobalt from a cobalt-magnesium mixed solution.

[0004] Previously, sodium fluoride and Mg were generally used 2+ The magnesium is removed by generating an insoluble magnesium fluoride precipitate. Although the magnesium removal effect is very good, the quality of the cobalt sulfate product is affected by the introduction of fluoride impurities. At the same time, the introduction of fluoride ions will also cause environmental pollution. Therefore, the fluoridation method for removing magnesium has been gradually eliminated. There are reports in the related art on the use of extraction to separate cobalt and magnesium. At present, acidic extractants are often used for extraction to transfer cobalt into the organic phase while magnesium is retained in the aqueous phase to achieve the separation of cobalt and magnesium. Then, sulfuric acid with different acidities is used to wash magnesium to achieve the separation of cobalt and magnesium. The principle is to use H + Replace Mg in organic phase 2+ , but in actual production, H + Replace Mg 2+ At the same time, it will also replace Co 2+ , resulting in a high cobalt content in the raffinate and a large loss of cobalt metal. In addition, this method does not have the effect of enriching cobalt during extraction, which will inevitably increase the cost of the subsequent cobalt sulfate crystallization process.

[0005] In summary, the existing means of separating cobalt and magnesium by extraction are not mature yet, and may reduce the yield of cobalt, or the resulting cobalt-containing product may not reach high purity. Summary of the invention

[0006] The present invention aims to solve at least one of the technical problems existing in the prior art. To this end, the present invention proposes an extraction process for separating cobalt and magnesium, which can effectively reduce the loss rate of cobalt and increase the content of impurity magnesium in the obtained cobalt product.

[0007] According to an embodiment of the first aspect of the present invention, an extraction process for separating cobalt and magnesium is provided, the extraction process comprising the following steps:

[0008] S1. Using P507 and Mextral@V10 as mixed extractants, the cobalt-magnesium mixed solution was extracted to obtain a loaded organic phase and a raffinate phase;

[0009] S2. Controlling the O / A ratio to 9 to 11:1, performing 15 to 17 levels of countercurrent washing of the loaded organic phase with a 0.8 to 1.2 mol / L aqueous sulfuric acid solution to obtain a washing residue and a washed loaded organic phase;

[0010] S3. Back-extracting cobalt from the washed loaded organic phase.

[0011] The mechanism of the extraction process is as follows:

[0012] Step S1: most of the cobalt and a small amount of nickel and magnesium in the cobalt-magnesium mixed solution are transferred to the loaded organic phase;

[0013] Step S2: substantially all nickel and magnesium, as well as a small amount of cobalt, are transferred from the loaded organic phase to the washing residual solution; the loaded organic phase after washing contains high-purity cobalt;

[0014] Step S3: Cobalt is transferred from the washed loaded organic phase to the back extraction phase. After the back extraction phase is crystallized, a battery-grade cobalt salt can be obtained.

[0015] The extraction process according to the embodiment of the present invention has at least the following beneficial effects:

[0016] (1) The present invention creatively uses P507 and Mextral@V10 as mixed extractants, and the extraction efficiency of cobalt is ≥99.7%, which significantly improves the yield of cobalt. At the same time, the mixed extractant has a weak affinity for magnesium, so most of the magnesium is retained in the raffinate phase, and the separation of cobalt and magnesium is preliminarily achieved.

[0017] (2) The present invention creatively uses P507 and Mextral@V10 as mixed extractants, which significantly improves the distribution coefficient of magnesium and cobalt during the washing process, thereby promoting the washing of magnesium and preventing cobalt from being separated from the loaded organic phase. Ultimately, the separation of cobalt and magnesium is achieved with minimal loss of cobalt.

[0018] (3) Traditional technology focuses more on the control of the extraction process, while ignoring the importance of the washing process. As a result, the nickel and cobalt yields are low, the separation of magnesium and transition metal ions is incomplete, and the impurity content in the cobalt sulfate solution is difficult to meet the raw material requirements of battery materials.

[0019] The present invention achieves the separation of magnesium and cobalt easily and efficiently by controlling the parameters of magnesium washing in step S2, thus solving the problems in the traditional technology.

[0020] According to some embodiments of the present invention, the cobalt-magnesium mixed solution is a product of the cobalt intermediate acid leaching solution after impurities are removed. The cobalt intermediate includes a cobalt ore preliminary enrichment product or a lithium-ion battery positive electrode material. The impurity removal includes at least one of sodium thiosulfate to remove copper and cadmium, sodium hypochlorite to remove iron and aluminum, and P204 extraction to remove impurities.

[0021] According to some embodiments of the present invention, in the cobalt-magnesium mixed solution, the cobalt content is 15-30 g / L; the magnesium content is 3-10 g / L.

[0022] According to some embodiments of the present invention, the content of cobalt in the cobalt-magnesium mixed solution is 15-16 g / L.

[0023] According to some embodiments of the present invention, the content of magnesium in the cobalt-magnesium mixed solution is 3-4 g / L.

[0024] According to some embodiments of the present invention, the nickel content in the cobalt-magnesium mixed solution is ≤5 g / L, for example, it may be about 4.5 g / L.

[0025] According to some embodiments of the present invention, the cobalt-magnesium mixed solution further contains manganese ions and lithium ions. The concentration of manganese ions is ≤0.05 g / L, for example, it can be about 0.03 g / L. The concentration of lithium ions is ≤0.1 g / L, for example, it can be about 0.08 g / L.

[0026] According to some embodiments of the present invention, in step S1, the pH value of the cobalt-magnesium mixed solution is between 3.0 and 4.0, for example, about 3.5.

[0027] According to some embodiments of the present invention, in step S1, the mass ratio of P507 to Mextral@V10 is 2 to 9:1, for example, about 2.2:1, 2.3:1, 2.5:1, 3:1, 4:1, 5:1, 6:1, 7:1 or about 8:1.

[0028] According to some embodiments of the present invention, the saponification rate of the mixed extractant is 40-50%, for example, about 45%.

[0029] According to some embodiments of the present invention, the saponification of the mixed extractant is performed by mixing the mixed extractant with a sodium hydroxide aqueous solution, wherein the mass concentration of the sodium hydroxide aqueous solution is 8 to 12%, for example, about 10%.

[0030] According to some embodiments of the present invention, in step S1, the organic phase used in the extraction includes the mixed extractant and the diluent.

[0031] According to some embodiments of the present invention, the diluent includes at least one of kerosene and light white oil, wherein the kerosene includes sulfonated kerosene, and the model of the sulfonated kerosene is 260#.

[0032] According to some embodiments of the present invention, in step S1, the volume percentage of the mixed extractant in the organic phase is 20-30%.

[0033] According to some embodiments of the present invention, in step S1, the extraction method is countercurrent extraction; the number of stages of the countercurrent extraction is 7 to 9.

[0034] According to some embodiments of the present invention, in step S1, the O / A ratio of the extraction is 1.5 to 2.5:1, for example, specifically about 2:1.

[0035] According to some embodiments of the present invention, in step S1, during the extraction, the extraction efficiency of cobalt is ≥ 99%, for example, about 99.5% or about 99.9%.

[0036] According to some embodiments of the present invention, in step S1, the cobalt content in the raffinate phase is ≤0.15 g / L, for example, ≤0.05 g / L.

[0037] According to some embodiments of the present invention, in step S1, the pH value of the raffinate phase is 4.5-5.0.

[0038] According to some embodiments of the present invention, the extraction process further comprises mixing the raffinate phase with a sulfide salt to react and precipitate nickel.

[0039] According to some embodiments of the present invention, in step S2, the O / A ratio of the washing is about 10:1.

[0040] According to some embodiments of the present invention, in step S2, the concentration of the aqueous sulfuric acid solution is about 1 mol / L.

[0041] According to some embodiments of the present invention, in step S2, the number of stages of the countercurrent washing is 16.

[0042] According to some embodiments of the present invention, in step S2, the pH of the washing residue needs to be controlled in the 13th to 15th stages of the countercurrent washing, and specifically needs to be controlled between 3.6 and 3.8, thereby better improving the elution effect of magnesium and reducing the content of cobalt in the washing residue.

[0043] According to some embodiments of the present invention, in step S2, the washing raffinate and the acid leaching solution are mixed, thereby achieving the purpose of controlling the pH and other conditions of the raffinate; wherein a small amount of cobalt can be further enriched.

[0044] According to some embodiments of the present invention, in step S2, the washing residual liquid is subjected to magnesium precipitation to obtain a mixture containing nickel and magnesium.

[0045] According to some embodiments of the present invention, in step S2, the loss rate of cobalt in the washing residue is ≤5%. The loss rate is the mass percentage of cobalt in the washing residue to cobalt in the loaded organic phase, also known as the cobalt washout rate.

[0046] According to some embodiments of the present invention, in step S2, during the washing, the washing rate of cobalt is ≤2%, for example, ≤1%.

[0047] According to some embodiments of the present invention, in step S3, the aqueous phase used in the back extraction of cobalt is a sulfuric acid aqueous solution, wherein the concentration of the sulfuric acid aqueous solution used is 1.5 to 2.5 mol / L, for example, specifically about 2 mol / L.

[0048] According to some embodiments of the present invention, in step S3, the O / A ratio of the back extraction is 5 to 20:1, for example, about 6:1, about 7:1, 10:1, 15:1 or about 16:1.

[0049] According to some embodiments of the present invention, in step S3, the number of back extraction stages is 4 to 6. For example, it may be 5 stages.

[0050] According to some embodiments of the present invention, in step S3, the mass percentage of magnesium in the aqueous phase obtained by back-extracting cobalt is ≤0.025%.

[0051] According to some embodiments of the present invention, in step S3, the concentration of cobalt in the back-extracted phase obtained by back-extraction is 80-120 g / L. For example, it can be about 100 g / L, 110 g / L or about 115 g / L. It can be seen that the present invention, through the design of the O / A ratio of each step, not only ensures the separation of cobalt and magnesium and reduces the cobalt loss rate, but also enriches cobalt as much as possible, thereby reducing the cost of subsequent crystallization of cobalt-containing products from the back-extracted phase.

[0052] According to some embodiments of the present invention, in step S3, the concentration of magnesium in the back-extracted phase obtained by back-extraction is 0.0064-0.1 g / L, for example, about 0.01 g / L, 0.02 g / L, 0.03 g / L, 0.04 g / L or about 0.05 g / L.

[0053] According to some embodiments of the present invention, the extraction process further comprises crystallizing cobalt sulfate from the back-extracted phase obtained in step S3. The obtained cobalt sulfate meets the purity requirements of battery-grade cobalt sulfate.

[0054] If there is no special explanation, the actual meaning of “about” in the present invention is that the error is allowed to be within the range of ±2%, for example, about 100 is actually 100±2%×100.

[0055] Unless otherwise specified, “between” in the present invention includes the number itself, for example, “between 2 and 3” includes the endpoint values ​​2 and 3.

[0056] Other features and advantages of the present invention will be set forth in the description which follows, and in part will be apparent from the description, or may be learned by practice of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS

[0057] The above and / or additional aspects and advantages of the present invention will become apparent and easily understood from the description of the embodiments in conjunction with the following drawings, in which:

[0058] Figure 1 It is a schematic flow chart of the extraction process adopted in Example 1 of the present invention. DETAILED DESCRIPTION

[0059] The following will be combined with the embodiments to clearly and completely describe the concept of the present invention and the technical effects produced, so as to fully understand the purpose, characteristics and effects of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, other embodiments obtained by those skilled in the art without creative work are all within the scope of protection of the present invention.

[0060] In the description of the present invention, the description with reference to the terms "one embodiment", "some embodiments", "illustrative embodiments", "examples", "specific examples", or "some examples" means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described may be combined in any one or more embodiments or examples in a suitable manner.

[0061] Unless otherwise specified, the main components of the cobalt-magnesium mixed solution used in the specific implementation manner are shown in Table 1:

[0062] Table 1 Main components of cobalt-magnesium mixed solution

[0063] Test items Co Mg Mn Ni Li pH Cobalt-magnesium mixed solution (g / L) 15.34 3.03 0.038 4.28 0.096 3.99

[0064] In Table 1, as well as the concentrations of metal ions in the subsequent solutions, the ICP-OES method was used to test the pH, and the pH was tested using a pH meter.

[0065] The sulfonated kerosene, P507 and Mextral@V10 used were purchased from Luoyang Sannuo Chemical Co., Ltd. and used directly without any pretreatment process.

[0066] Example 1

[0067] This example provides an extraction process for separating cobalt and magnesium. The simple process is shown as follows: Figure 1 As shown, the specific steps are as follows:

[0068] S1. Extracting the cobalt-magnesium mixture with an organic phase to obtain a loaded organic phase and a raffinate phase; wherein,

[0069] The organic phase is a mixture of 260# sulfonated kerosene and mixed extractant in a volume ratio of 3:1;

[0070] In the mixed extractant, the mass ratio of P507 and Mextral@V10 was 7:3;

[0071] Before use, the mixed extractant is mixed with a sodium hydroxide aqueous solution with a mass concentration of 10% for saponification, and the saponification rate is 45%. The saponification rate is determined by testing the acid content in the extractant by titration and calculating the percentage of the acid content decrease during the mixed saponification process.

[0072] During the extraction process, the O / A ratio was controlled at 2:1, and 8-stage countercurrent extraction was performed. The main solute of the raffinate phase was nickel sulfate and contained magnesium ions. The Co concentration was 0.014 g / L, and the Co extraction rate could be maintained above 99.5%.

[0073] Sodium sulfide is added to the raffinate phase to precipitate nickel sulfide, and the filtrate is then used to precipitate magnesium.

[0074] S2. Magnesium washing: add 1 mol / L sulfuric acid aqueous solution to the loaded organic phase obtained in step S1, control the O / A ratio to 10:1, perform 16-stage countercurrent washing, control the pH value of the aqueous phase of magnesium washing from stage 13 to stage 15 to be between 3.6-3.8 (specifically about 3.7 in this example), and then stand and separate to obtain the washed loaded organic phase and the washing residual liquid;

[0075] S3. Cobalt back extraction: add 2 mol / L sulfuric acid aqueous solution to the washed loaded organic phase obtained in step S2, control the phase O / A ratio to 16:1, perform 5-stage countercurrent stripping, and then stand and separate to obtain a back extraction phase (pure cobalt sulfate solution) and an unloaded organic phase.

[0076] The evaporation crystallization back extract phase can obtain battery-grade cobalt sulfate.

[0077] Example 2

[0078] This example provides an extraction process for separating cobalt and magnesium, which is different from Example 1 in that:

[0079] The mass ratio of P507 to Mextral@V10 is 8:1.

[0080] Example 3

[0081] This example provides an extraction process for separating cobalt and magnesium, which is different from Example 1 in that:

[0082] The mass ratio of P507 to Mextral@V10 is 1.8:1.

[0083] Comparative Example 1

[0084] This example provides an extraction process for separating cobalt and magnesium, which is different from Example 1 in that:

[0085] The extractant is pure P507.

[0086] Comparative Example 2

[0087] This example provides an extraction process for separating cobalt and magnesium, which is different from Example 1 in that:

[0088] In step S2, the O / A ratio is controlled to be 8:1.

[0089] Comparative Example 3

[0090] This example provides an extraction process for separating cobalt and magnesium, which is different from Example 1 in that:

[0091] In step S2, the concentration of the sulfuric acid aqueous solution used is 1.5 mol / L.

[0092] Test Case

[0093] This example tests the main components of the raffinate phase, washing raffinate and cobalt sulfate obtained in the examples and comparative examples, and the test methods include ICP-OES and pH meter. The test results are shown in Tables 2 to 5.

[0094] Table 2 Composition of the raffinate phase obtained in step S1

[0095] Test items Co g / L Mg g / L Mn g / L Ni g / L Li g / L Example 1 0.014 2.10 0.005 4.03 0.09 Example 2 0.043 1.80 0.010 3.65 0.087 Example 3 0.102 1.56 0.008 3.25 0.09 Comparative Example 1 3.536 1.52 0.009 3.09 0.009 Comparative Example 2 0.015 2.10 0.005 4.03 0.09 Comparative Example 3 0.014 2.10 0.005 4.03 0.09

[0096] According to the results in Table 2, by controlling the ratio of the two extractants in the mixed extractant, the extraction effects of cobalt and nickel can be significantly affected. Specifically, with the increase of P507 content, the extraction of cobalt first increased and then decreased, while the extraction trend of magnesium was the opposite.

[0097] Table 3 Washout rate of each component in step S2

[0098]

[0099]

[0100] According to the results of Table 3, the composition ratio of the extractant and the specific parameters of magnesium washing will significantly affect the effect of magnesium washing. Among them, it is known that if the ratio with poor magnesium extraction effect during the extraction process is used, it is also easier to wash out magnesium, while the ratio with good cobalt extraction effect is less loss of cobalt. In the magnesium washing step, if the concentration of the sulfuric acid aqueous solution used is adjusted, or the O / A ratio is changed, the effect of magnesium washing will be significantly affected, or the loss rate of cobalt will be increased, or the washing effect of magnesium will be reduced.

[0101] Table 4 Composition of the back extraction phase obtained in step S3

[0102] Test items Co g / L Mg mg / L Mn mg / L Ni mg / L Li mg / L Example 1 118.53 9 2.5 3.3 0.8 Example 2 117.89 30.0 2.3 14.2 1.27 Example 3 111.4 45.4 2.7 40.0 0.83 Comparative Example 1 73.3 95.9 3.3 80.7 4.7 Comparative Example 2 78.7 21 3.1 9.3 0.9 Comparative Example 3 75.8 45 3.6 15.3 0.9

[0103] Table 5 Parameters of cobalt sulfate obtained in step S3

[0104] Test items Co wt% Mg wt% Mn wt% Ni wt% Li wt% Example 1 21 0.0015 0.00045 0.0005 0.0001 Example 2 20.8 0.0056 0.0004 0.0035 0.00022 Example 3 20.1 0.008 0.0005 0.007 0.0002 Comparative Example 1 19.7 0.023 0.0008 0.02 0.001 Comparative Example 2 19.9 0.017 0.0009 0.006 0.0007 Comparative Example 3 19.5 0.026 0.001 0.004 0.0003

[0105] According to the results in Tables 4 to 5, the main content and impurity content of the cobalt sulfate obtained in Examples 1 to 3 of the present invention all meet the performance requirements of battery-grade cobalt sulfate. In Comparative Examples 1 to 3, the main content is reduced or the impurity content is increased due to changes in extraction, washing and other conditions.

[0106] In summary, the extraction process provided by the present invention can achieve the separation of cobalt and magnesium, and the separation of nickel and cobalt by selecting a suitable type of extractant and assisting with improved parameters, and finally produce battery-grade cobalt sulfate material. The extraction process provided by the present invention is expected to have broad application prospects in the field of lithium secondary battery recovery and cobalt mining.

[0107] The embodiments of the present invention are described in detail above in conjunction with the accompanying drawings, but the present invention is not limited to the above embodiments. Various changes can be made within the knowledge of ordinary technicians in the relevant technical field without departing from the purpose of the present invention. In addition, the embodiments of the present invention and the features in the embodiments can be combined with each other without conflict.

Claims

1. An extraction process for separating cobalt and magnesium, characterized in that: The extraction process comprises the following steps: S1. Using P507 and Mextral@V10 as mixed extractants, the cobalt-magnesium mixed solution was extracted to obtain a loaded organic phase and a raffinate phase; S2. Controlling the O / A ratio to 9 to 11:1, performing 15 to 17 levels of countercurrent washing of the loaded organic phase with a 0.8 to 1.2 mol / L aqueous sulfuric acid solution to obtain a washing residue and a washed loaded organic phase; S3. Back-extracting cobalt from the washed loaded organic phase.

2. The extraction process according to claim 1, characterized in that In step S1, the mass ratio of P507 to Mextral@V10 is 2 to 9:

1.

3. The extraction process according to claim 1, characterized in that: In step S1, the organic phase used in the extraction includes the mixed extractant and the diluent; and / or the diluent includes at least one of kerosene and light white oil.

4. The extraction process according to claim 3, characterized in that: In step S1, the volume percentage of the mixed extractant in the organic phase is 20-30%.

5. The extraction process according to claim 1, characterized in that: In step S1, the extraction method is countercurrent extraction; the number of stages of the countercurrent extraction is 7 to 9; and / or the O / A ratio of the extraction is 1.5 to 2.5:

1.

6. The extraction process according to claim 1, characterized in that: In step S1, the pH value of the cobalt-magnesium mixed solution is between 3.0 and 4.

0.

7. The extraction process according to claim 1, characterized in that: In step S3, the O / A ratio of the back extraction is 5 to 20:1; and / or the number of stages of the back extraction is 4 to 6.

8. The extraction process according to any one of claims 1 to 7, characterized in that: The extraction process also includes mixing the raffinate phase with a sulfide salt to react and precipitate nickel.

9. The extraction process according to any one of claims 1 to 7, characterized in that: In step S2, the loss rate of cobalt in the washing residual solution is ≤5%; and / or, in step S3, the mass percentage of magnesium in the aqueous phase obtained by back-extracting cobalt is ≤0.025%.

10. The extraction process according to any one of claims 1 to 7, characterized in that: In step S1, in the extraction, the extraction efficiency of cobalt is ≥99%.