A method for preparing graphene oxide from waste organic matter

By using the combination of waste organic matter and conductive ink, high-quality graphene is prepared by flash evaporation and purified in smoked nitric acid, the existing graphene oxide process is solved, and high energy consumption is achieved, and high efficiency and low Costly high-purity graphene oxide preparation promotes the green resource utilization of organic waste.

CN118145632BActive Publication Date: 2024-11-26FOSHAN MINGCHENG MANAGEMENT CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410391758.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-04-02
Publication Date
2024-11-26
Estimated Expiration
2044-04-02

AI Technical Summary

Technical Problem

The existing graphene oxide preparation process is cumbersome, energy consumption is high, toxic and harmful liquids are produced, and the product performance is poor, which hinders the large-scale application of graphene and its derivatives.

Method used

Use waste organic matter as raw materials, crushing, drying, and adding conductive ink to make filler, and high-quality graphene is prepared by flash evaporation with low voltage and high current, and oxidizing it in smoked nitric acid to obtain high-purity graphene oxide .

Benefits of technology

It realizes efficient and high value-added treatment of organic waste with simple operation, low cost, green and environmental protection, and prepares graphene oxide materials with high purity and high recovery, simplifies the process and reduces costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118145632B_ABST
    Figure CN118145632B_ABST
Patent Text Reader

Abstract

The present invention provides a method for preparing graphene oxide from waste organic matter, comprising the following steps: collecting and pre-treating waste organic matter, crushing and drying the waste organic matter; preparing filler, adding conductive powder to the treated waste organic matter to prepare filler (3); preparing high-quality graphene, filling the filler in a quartz tube (1), compacting it with an electrode rod (2) matching the quartz tube diameter and applying a specific voltage for flash evaporation to obtain a graphene product; preparing high-quality and high-purity graphene oxide, adding the obtained graphene product to fuming nitric acid for oxidation to obtain graphene oxide. The method has the characteristics of simple operation, low cost, green environmental protection, etc., and is of great significance for the efficient and high value-added treatment of organic waste.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of graphene oxide preparation, and in particular to a method for preparing graphene oxide from waste organic matter. Background Art

[0002] Graphene and its derivatives have become a rising star in the field of materials due to their excellent electrical, mechanical, optical, catalytic, and magnetic properties in the fields of medicine, food, chemical, electrical appliances, environment, biology, and energy. Their preparation and application technologies have made great progress in a short period of time since their introduction. The existing raw materials for graphene oxide are mainly graphite ore. After mining and mineral processing, they are often oxidized by harsh conditions such as Hummer to obtain well-dispersed graphite oxide, and then dispersible graphene oxide dispersion is obtained through ultrasonic stripping steps. The entire process is not only cumbersome, energy-intensive, and produces a large amount of toxic and harmful liquids, but also the product performance is greatly reduced due to chemical defects. Its high cost and insufficient performance have hindered the large-scale application of graphene and its derivatives. Therefore, finding cheap raw materials and preparing high-quality graphene oxide have become the key to solving the above problems. Summary of the invention

[0003] The purpose of the present invention is to provide a method for preparing graphene oxide from waste organic matter, which has the characteristics of simple operation, low cost, green and environmental protection, and is of great significance for the efficient and high value-added treatment of organic waste.

[0004] The embodiment of the present invention is achieved as follows:

[0005] The present invention provides a method for preparing graphene oxide from waste organic matter, comprising the steps of:

[0006] a. Collection and pre-treatment of waste organic matter, crushing and drying of waste organic matter;

[0007] b. Preparation of filler: adding conductive powder to the treated waste organic matter to prepare filler;

[0008] c. Preparation of high-quality graphene: fill the filler into a quartz tube, compact it with an electrode rod that matches the diameter of the quartz tube, and apply a specific voltage for flash evaporation to obtain a graphene product;

[0009] d. Preparation of high-quality and high-purity graphene oxide, adding the prepared graphene product into fuming nitric acid for oxidation to obtain graphene oxide.

[0010] Furthermore, the waste organic matter includes artificial high molecular organic matter products or natural high molecular organic matter.

[0011] Furthermore, the artificial macromolecular organic products include plastic bags, syringe tubes, electrical appliance housings, beverage bottles, and tires; the natural macromolecular organic products include fruit peels, dead branches, dried flowers and plants, and animal specimens.

[0012] Furthermore, in step a, the waste organic matter needs to be broken into small pieces or powder, and then dehydrated in a vacuum drying oven.

[0013] Furthermore, in step a, after the waste organic matter with grease is crushed, the waste organic matter fragments are poured into 100mL of 1mol / L NaOH solution and stirred at 80°C for 2h to remove the grease attached to the surface of the waste organic matter fragments, and then the waste organic matter fragments are thoroughly washed with deionized water with the assistance of a suction filtration device, and vacuum dried at 80°C to constant weight.

[0014] Furthermore, in step b, the conductive powder is graphite powder, and graphite powder is added to the treated waste organic matter, mixed evenly, and the conductivity is enhanced to prepare a filler.

[0015] Furthermore, in step c, the electrode rod is a copper screw.

[0016] Furthermore, the specific voltage is 70-130V, the resistance of the filler is 1.4-4Ω, the flash temperature is 2850-3100K, and the time for applying the specific voltage, i.e., the pulse time, is 10-150ms.

[0017] Furthermore, the time for applying the specific voltage, i.e., the pulse time, is 100 ms.

[0018] Furthermore, in step d, the prepared graphene product is added to fuming nitric acid and refluxed at 80° C. for 1 hour. While the graphene is oxidized to graphene oxide, amorphous carbon and low-chain alkanes can be oxidized to CO2 to achieve the purpose of purification. The graphene oxide powder can then be obtained by filtering, washing and drying.

[0019] The beneficial effects of the method for preparing graphene oxide from waste organic matter provided by the present invention are:

[0020] The present invention dries and crushes the waste organic matter, and then mixes an appropriate amount of conductive powder into the waste organic matter fragments to increase the conductivity; then, the mixture of the waste organic matter and the conductive powder is made into a filler, and the filler is pressed between the positive and negative electrodes of the quartz tube. At this time, due to the large resistance of the waste, when the voltage is applied until a path is formed, the excessive power will generate a high temperature of more than 3000K, causing the waste organic matter to instantly vaporize to form single atoms such as C, H, O, S, and N; at the same time, the excessive energy will be radiated in the form of strong light, causing the temperature in the reaction pool to cool rapidly. However, in this process, highly active single atoms will seek the form with the lowest energy and the most stable structure to bond; among them, a small amount of S, N, and O will form oxide gas molecules and volatilize, while the most abundant C atoms and a small amount of H atoms will form hexagonal graphene with a purity of 99%, and the recovery rate can reach more than 90%; then, the graphene product is poured into fuming nitric acid and refluxed for 1 hour, the graphene can be oxidized into graphene oxide, and the residual, a small amount of amorphous carbon and low-chain alkanes are oxidized into CO2 and removed, so as to achieve the purpose of product purification. The present invention has the characteristics of simple operation, low cost, green environmental protection, etc., and has practical significance for the efficient and high value-added treatment of organic waste. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings required for use in the embodiments are briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present invention and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without creative work.

[0022] Figure 1 It is a schematic diagram of the structure in which the filler is filled in the quartz tube;

[0023] Figure 2 XRD spectra of the sample self-assembled on the hybrid cellulose membrane and the commercial GO membrane;

[0024] Figure 3 is the Raman spectrum of graphene oxide product;

[0025] Figure 4 TEM image of graphene oxide product;

[0026] Figure 5 AFM characterization image of graphene oxide product;

[0027] In the figure: 1. quartz tube; 2. electrode rod; 3. filler. DETAILED DESCRIPTION

[0028] In order to further understand the present invention, preferred embodiments of the present invention are described below in conjunction with examples. However, it should be understood that these descriptions are only to further illustrate the features and advantages of the present invention, rather than to limit the claims of the present invention.

[0029] The present invention provides a method for preparing high-quality and high-purity graphene oxide using organic waste, comprising the following steps:

[0030] a. Collection and pre-treatment of organic waste

[0031] After the waste organic matter is collected, it is broken into small pieces or powder to expose the surface as much as possible, and then dehydrated in a vacuum drying oven.

[0032] b. Preparation of fillers

[0033] The dried waste organic matter fragments have a large resistance and are not easy to conduct electricity at low voltage. Therefore, a certain amount of graphite powder is mixed in as conductive powder to make filler 3 to reduce process requirements.

[0034] c. Preparation of high-quality graphene

[0035] Waste organic matter fragments mixed with graphite powder are filled into a quartz tube 1, and are compacted with an electrode rod 2 matching the diameter of the quartz tube 1 and a specific voltage is applied for 100ms. After flashing inside the quartz tube 1, high-quality graphene materials with a purity of 99% and a recovery rate of 90% are obtained.

[0036] d. Preparation of high-quality, high-purity graphene oxide

[0037] The above graphene product is added into fuming nitric acid and refluxed at 80°C for 1 hour. While the graphene is oxidized into graphene oxide, amorphous carbon and low-chain alkanes can be oxidized into CO2 to achieve the purpose of purification. The graphene oxide powder can then be obtained by filtering, washing and drying.

[0038] Specifically, the operator collected a variety of plastic beverage bottles without distinguishing the specific composition of the waste organic matter, and cut and mixed them with scissors. Then, the waste organic matter fragments were poured into 100mL 1mol / L NaOH solution, stirred at 80℃ for 2h to remove the grease attached to the surface of the waste organic matter fragments, and then, with the assistance of the suction filtration device, the garbage fragments were thoroughly washed with deionized water, and vacuum dried at 80℃ to constant weight for subsequent experiments.

[0039] Pure plastic and other waste organic fragments have poor conductivity. After mixing a certain amount of graphite powder as conductive powder, filler 3 is made. The filler 3 is filled in the Figure 1The cylindrical quartz tube 1 with a diameter of 1 cm and a height of 4 cm is shown, and the plastic fragments are compacted with a copper screw as an electrode. Subsequently, the operator optimizes the conditions by controlling the specific voltage to be 70-130V, the resistance of the filler to be 1.4-4Ω, the flash temperature to be 2850-3100K, the time for applying the specific voltage, i.e., the pulse time to be 10-150ms, etc., to obtain high-quality graphene products. The conductive powder can also be other highly conductive powders, preferably graphite powder. The copper screw is the electrode rod 2. Preferably, the time for applying the specific voltage, i.e., the pulse time, is 100ms.

[0040] Subsequently, the operator used fuming nitric acid to oxidize and purify the above graphene product to prepare high-quality, high-purity graphene oxide, and after vacuum filtration to a mixed cellulose microporous filter membrane, its XRD spectrum was compared with that of commercial GO. Figure 2 As shown in the figure, both of them have sharp peaks near 12° and broad peaks near 21°. Among them, 12° is the characteristic peak of the interlayer spacing of the GO membrane, indicating that the interlayer spacing distribution of the two-dimensional membrane is narrow at this time, concentrated at The peak at 21° is the characteristic peak of the mixed cellulose membrane. The results show that the product obtained by the inventors has similar dispersibility and self-assembly ability as commercial GO.

[0041] In addition, if Figure 3 As shown, the inventors found from the Raman spectrum that the product had two characteristic peaks of GO material, D band and G band, at 1365cm-1 and 1602cm-1 respectively. The D peak is a disordered band caused by the first-order zone boundary phonons at the edge of the graphene oxide nanosheet, while the G peak corresponds to the in-phase vibration in the defect-free graphene lattice, representing the integrity of the graphene lattice. This result proves that the product is graphene oxide, but the shorter D peak indicates that its oxidation degree is not high.

[0042] Subsequently, the operator characterized the morphology of the product. Figure 4 In the figure, it can be seen that the product has an obvious two-dimensional ultra-thin morphology, which is consistent with the existing literature. Figure 5 The thickness of the single-layer material was characterized and it was shown that the thickness of the nanosheet was about 350pm, or 0.35nm, which is close to that of graphene material, further verifying that the material is a single-atom-layer two-dimensional material. At the same time, the 0.35nm nanosheet thickness is much lower than the 0.8-1.2nm reported in the literature, indicating that the degree of oxidation of the material is not high, and the oxygen-containing functional groups do not make a significant contribution to the height of the nanosheet, which is further confirmed by the Raman spectrum.

[0043] The present invention provides a low-cost, environmentally friendly and efficient method for preparing high-quality graphene oxide materials to solve the problems existing in the prior art: first, high-carbon organic waste generated in human life, including but not limited to artificial polymer products such as plastic bags, syringe tubes, electrical housings, beverage bottles, tires, and natural polymers such as fruit peels, dead branches, dried flowers and plants, and animal specimens, is used as a zero-cost carbon source to replace graphite ore, greatly reducing the cost of graphene manufacturing; secondly, a low-voltage, high-current flash evaporation method is used to convert organic waste into high-quality graphene materials with a purity of 99% and a recovery rate of more than 90% within 100ms, and then the fuming nitric acid is refluxed to further purify and prepare high-quality, high-purity graphene oxide materials. This method not only simplifies the preparation process of graphene oxide and reduces the cost, but also solves the problem of substandard quality of graphene oxide in the prior art, opening up a new way for the green and resource utilization of organic waste.

[0044] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A method for preparing graphene oxide from waste organic matter, characterized in that: Includes steps: a. Collection and pre-treatment of waste organic matter Crushing and drying of waste organic matter; b. Preparation of fillers Adding conductive powder to the treated waste organic matter to prepare a filler (3); c. Preparation of high-quality graphene Filling a filler into a quartz tube (1), compacting it with an electrode rod (2) matching the diameter of the quartz tube, and applying a voltage to perform flash evaporation to obtain a graphene product; d. Preparation of high-quality, high-purity graphene oxide The prepared graphene product is added into fuming nitric acid for oxidation to obtain graphene oxide; In step a, the waste organic matter needs to be crushed into small pieces or powder, and then dehydrated in a vacuum drying oven; In step a, after crushing the waste organic matter with grease, pour the waste organic matter fragments into 100 mL of 1 mol / L NaOH solution, stir at 80° C. for 2 h to remove grease attached to the surface of the waste organic matter fragments, and then thoroughly wash the waste organic matter fragments with deionized water with the aid of a suction filtration device, and vacuum dry at 80° C. to constant weight; In step b, the conductive powder is graphite powder, and graphite powder is added to the treated waste organic matter, mixed evenly, and the conductivity is enhanced to prepare filler (3); In step d, the prepared graphene product is specifically added to fuming nitric acid and refluxed at 80° C. for 1 hour. While the graphene is oxidized to graphene oxide, amorphous carbon and low-chain alkanes can be oxidized to CO2 to achieve the purpose of purification. The graphene oxide powder can then be obtained by filtering, washing and drying.

2. The method for preparing graphene oxide from waste organic matter according to claim 1, characterized in that: The waste organic matter includes artificial high molecular organic matter products or natural high molecular organic matter.

3. The method for preparing graphene oxide from waste organic matter according to claim 2, characterized in that: The artificial high molecular organic products include plastic bags, syringe tubes, electrical appliance housings, beverage bottles, and tires; the natural high molecular organic products include fruit peels, dead branches, dried flowers and plants, and animal specimens.

4. The method for preparing graphene oxide from waste organic matter according to claim 1, characterized in that: In step c, the electrode rod (2) is a copper screw.

5. The method for preparing graphene oxide from waste organic matter according to claim 1, characterized in that: The voltage is 70-130V, the resistance of the filler (3) is 1.4-4Ω, the flash temperature is 2850-3100K, and the time for applying the voltage, i.e. the pulse time, is 10-150ms.

6. The method for preparing graphene oxide from waste organic matter according to claim 5, characterized in that: The time for applying the voltage, ie, the pulse time, is 100 ms.